Method for co-processing sulfur-containing tailings and sulfur-containing waste rocks
Dry multi-stage screening and photoelectric separation technology are used to sort sulfur-containing tailings and sulfur-containing waste rock into low-sulfur gravel and fine gravel, and spiral chute and suspended cone gravity separation technologies are used to separate sulfur fines. Mine, solves the pollution and reuse problems of sulfur-containing tailings and waste rock, and achieves efficient resource utilization and low-cost sulfur concentrate production.
Patent Information
- Application Number
- CN202411144657.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-11
AI Technical Summary
Sulfur-containing tailings and sulfur-containing waste rock cause pollution problems during the storage process, and the sulfur content during their reuse does not meet standards, resulting in limited application and complicated initial investment and management.
Dry multi-stage screening, crushing and photoelectric separation technology are used to efficiently separate low-sulfur gravel and fine gravel from sulfur-containing waste rock, and through spiral chute separation, suspended cone gravity separation and sulfur flotation technology to achieve efficient separation of coarse-grained sulfur concentrate, fine-grained sulfur concentrate and low-sulfur fine sand and medium sand, and reduce the heavy metal content in water.
Efficient resource utilization of sulfur-containing tailings and sulfur-containing waste rocks has been achieved. The sulfur content of the sand and gravel produced for construction meets the standards. The sulfur concentrate can be used to make sulfuric acid and iron smelting, reducing the sulfur content of the flotation products and improving the efficiency of the flotation products. Process efficiency and economic benefits.
Smart Images

Figure CN118751391A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste treatment, and in particular to a method for co-processing sulfur-containing tailings and sulfur-containing waste rocks. Background Art
[0002] Mining companies will produce a huge amount of sulfur-containing tailings during production. During the storage process, the sulfide ore will gradually oxidize, leading to pollution problems such as acidification of the tailings pond water and dissolution of heavy metal elements. At the same time, a large amount of sulfur-containing waste rock is generally stored around the sulfur-containing tailings, mainly the stripped surrounding rock produced by sulfide mining, and large pieces of sulfur-containing ore (pieces larger than 100mm) discarded during pre-selection. The storage of sulfur-containing waste rock not only occupies a large amount of land, but long-term storage will also cause migration pollution problems similar to the above-mentioned sulfur-containing tailings.
[0003] The use of sulfur-containing tailings and sulfur-containing waste rock to prepare sand and gravel aggregates for construction is currently a relatively feasible method for the treatment of mining solid waste. However, the sulfur content of construction materials prepared from sulfur-containing tailings and sulfur-containing waste rock often does not meet the standard, resulting in limited application. In addition, the particle size of sulfur-containing tailings is fine, while sulfur-containing waste rock is mostly large-block ore. Therefore, it is often necessary to establish separate production lines during the reuse process, resulting in large initial investment and complex management of the reuse project.
[0004] Based on the above problems, the present invention aims to develop an efficient and easy-to-implement collaborative processing method to solve the resource utilization and pollution problems of sulfur-containing tailings and sulfur-containing waste rocks. Summary of the invention
[0005] The main technical problem solved by the present invention is to provide a method for the coordinated treatment of sulfur-containing tailings and sulfur-containing waste rock, which can achieve effective utilization of sulfur-containing tailings and sulfur-containing waste rock resources.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for co-processing sulfur-containing tailings and sulfur-containing waste rock, comprising the steps of:
[0007] S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =50~80mm, the coarsely crushed product enters the screening I operation;
[0008] The screening size of the screening operation I is 30-55 mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the product of the secondary crushing operation is P 100 =15-30mm, the product of the medium crushing operation is returned to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II;
[0009] The screening size of the screening II operation is 10-15 mm. The screened product obtained by the screening II operation enters the photoelectric sorting I operation. The ore blocks with a spot coefficient greater than 0.5% in the photoelectric sorting I operation are high-sulfur products. The photoelectric sorting I operation obtains the first high-sulfur product and the first low-sulfur product respectively. The first low-sulfur product is crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 = 5-8 mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening operation II, and then enters the screening operation III;
[0010] The screening size of the screening III operation is 3-5 mm. The screened product obtained from the screening III operation enters the photoelectric sorting II operation. The ore blocks with a spot coefficient greater than 0.5% selected by the photoelectric sorting II operation are high-sulfur products. The photoelectric sorting II operation obtains the second high-sulfur product and the second low-sulfur product respectively. The obtained second low-sulfur product is fine gravel. The obtained second high-sulfur product is returned to the fine crushing operation and enters the screening III operation after fine crushing; the under-size product obtained from the screening III operation enters the screening IV operation;
[0011] The screening size of the screening IV operation is 0.5-2mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The specific gravity of the heavy medium liquid is controlled at 2.5-2.8. The heavy medium sorting obtains the third high sulfur product and the third low sulfur product respectively. The third low sulfur product is coarse sand; the third high sulfur product is subjected to rod milling operation to obtain a rod mill product with a particle size of P 80 =0.2~0.5mm;
[0012] S2: The undersize product obtained from the screening IV operation, the rod mill product and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation;
[0013] The grading particle size of hydraulic classification I is 0.15-0.30mm. The sand settling products of hydraulic classification I enter the spiral chute for sorting. The spiral chute uses a cubic parabola cross section. Type chute, pitch and diameter ratio is 0.5-0.7, feed concentration is 30-40%, and the first heavy mineral product, the first intermediate product and the first light mineral product are obtained respectively. The first intermediate product enters the suspended vibration cone gravity separation operation. The suspended vibration cone concentrator is selected Type, feed ore concentration 20-25%, disk rotation period 200-240 seconds, vibration frequency 5.5-6.5Hz, respectively obtain the second heavy mineral product, the second intermediate product and the second light mineral product, the first heavy mineral product and the second heavy mineral product are combined to obtain coarse sulfur concentrate, the first light mineral product and the second light mineral product are combined to obtain medium sand;
[0014] The overflow product of hydraulic classification I operation enters hydraulic classification II operation, and the classification particle size of hydraulic classification II operation is 0.045~0.10mm. The sedimentation product of hydraulic classification II operation is combined with the second intermediate product and enters the ball milling operation. The particle size of the product of ball milling operation is P 80 = 0.045-0.063 mm, the ball milled product is returned to the hydraulic classification II operation for re-classification;
[0015] The overflow product of the hydraulic classification II operation enters the sulfur flotation operation. The concentrate product obtained from the sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of the sulfur flotation operation is fine sand.
[0016] As an embodiment of the present invention, the sulfur grade of the sulfur-containing tailings is 0.60-3.00%.
[0017] As an embodiment of the present invention, the sulfur grade of the sulfur-containing waste rock is 0.70-3.50%.
[0018] As an implementation scheme of the present invention, the mass ratio of the sulfur-containing waste rock to the sulfur-containing tailings is (1-4): (1-3).
[0019] As an implementation scheme of the present invention, the sulfur content of the crushed stone, fine gravel, coarse sand, medium sand and fine sand is ≤0.50%.
[0020] As an embodiment of the present invention, the sulfur content of the coarse-grained sulfur concentrate is greater than 29.0%.
[0021] As an embodiment of the present invention, the sulfur content of the fine-grained sulfur concentrate is greater than 28.0%.
[0022] As an embodiment of the present invention, the sulfur flotation operation adopts a beneficiation process of 1 roughing, 1-2 scavenging, and 1-2 cleaning, and the collector used is butyrate and / or kerosene.
[0023] Preferably, a frother is added during the sulfur flotation operation, and the frother is No. 2 oil.
[0024] As an embodiment of the present invention, an adjusting agent is further added during the sulfur flotation operation, and the adjusting agent is copper sulfate or a mixture of sulfuric acid and copper sulfate.
[0025] The method for co-processing sulfur-containing tailings and sulfur-containing waste rock provided by the present invention realizes the production of low-sulfur crushed stone and fine gravel for sulfur-containing waste rock through dry multi-stage screening, crushing and two-stage photoelectric sorting operations, and realizes the efficient separation of fine-grained sulfur concentrate, coarse-grained sulfur concentrate and low-sulfur fine sand and medium sand products through spiral chute sorting, suspended vibration cone gravity separation and sulfur flotation operations. The method of the present invention also utilizes the mineral new surface generated in the process of crushing and grinding sulfur-containing waste rock to effectively adsorb heavy metal ions in sulfur-containing tailing acidic wastewater, such as heavy metal ions such as lead and chromium, effectively reducing the heavy metal content of the water body; and the adsorbed heavy metal ions further activate the surface of sulfide ore minerals, improve the sorting effect of subsequent sulfur flotation operations, and reduce the sulfur content of the fine sand products obtained by flotation.
[0026] The sulfur-containing tailings and sulfur-containing waste rock treated by the method of the present invention are products of the same ore body. When the two are treated in coordination, the sulfur-containing waste rock is first treated in accordance with the technical ideas of "green energy saving, more crushing and less grinding", "multi-stage screening, step-by-step crushing, and early output when possible", and the dry crushing, screening and photoelectric sorting technologies are used to achieve efficient sorting of low-sulfur crushed stone products and low-sulfur fine gravel products; for intermediate particle size products (0.5-5 mm) that are difficult to be efficiently processed by photoelectric sorting technology, the present invention adopts heavy medium sorting technology for sorting, thereby achieving effective sorting of low-sulfur coarse sand products; "Hydraulic classification - graded sand settling into spiral chute - suspended vibration cone gravity separation" can effectively separate the coarse sulfur concentrate and low-sulfur medium sand products with monomer dissociation, and reduce the processing volume of ball milling and sulfur flotation operations. The spiral chute is used for coarse sand settling, and low-sulfur medium sand products can be directly obtained. The intermediate products obtained from the spiral chute are then selected by suspended vibration cone gravity separation, which has a large processing volume and saves site area, greatly improving the sorting efficiency and processing capacity of the process; the sulfur flotation operation uses the difference in the floatability of minerals to achieve efficient separation of fine-grained sulfur concentrate and low-sulfur fine sand products. Among them, the heavy medium separation uses ferrosilicon powder as the separation medium, and uses the principle that the mineral particles with high sulfur content have a higher specific gravity to achieve the separation of high-sulfur and low-sulfur products; the spiral chute and suspended vibration cone gravity separation use the density difference of minerals to achieve the separation of sulfide ores.
[0027] The method of the present invention can effectively realize the resource utilization of sulfur-containing tailings and sulfur-containing waste rock by rationally designing the process steps and controlling the process parameters of each step. The method of the present invention obtains a variety of products, including low-sulfur crushed stone, fine gravel, coarse sand, medium sand, and fine sand products, as well as coarse-grained sulfur concentrate and fine-grained sulfur concentrate with high sulfur content. The sulfur content of the obtained crushed stone, fine gravel, coarse sand, medium sand, and fine sand products meets the requirements of building sand and gravel (SO3≤0.5wt%), and can be used to prepare building materials that meet the requirements; the sulfur grade of coarse-grained sulfur concentrate and fine-grained sulfur concentrate meets the requirements of sulfur concentrate products, and can be used for sulfuric acid production, iron smelting, etc. The tail water generated in the production process has a low content of heavy metal ions and can be recycled. The method of the present invention provides a new way for the efficient utilization of sulfur-containing tailings and sulfur-containing waste rock, and has significant economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of the treatment process used in Examples 1-5 of the present invention. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in detail below through specific embodiments. The following embodiments are intended to further illustrate the content of the present invention in detail, but are not intended to limit the scope of protection of the claims of the present invention.
[0030] In the following examples, the pharmaceutical agents used are all commercially available products. Unless otherwise specified, the content percentages in each example are all mass percentages.
[0031] Example 1
[0032] This embodiment provides a method for the coordinated treatment of sulfur-containing tailings and sulfur-containing waste rock. The sulfur-containing tailings and the sulfur-containing waste rock are both from a mining enterprise in Shaxi Town, Qujiang District, Shaoguan City, Guangdong Province. The sulfur grades (sulfur grade, i.e., the mass percentage content of sulfur) of the sulfur-containing tailings and the sulfur-containing waste rock are 1.96% and 1.32%, respectively. The mass ratio of the sulfur-containing tailings to the sulfur-containing waste rock is 1:1. The process flow of the treatment method is shown in FIG. Figure 1 As shown, the specific steps are as follows:
[0033] S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =80mm, the coarsely crushed product enters the screening I operation;
[0034] The screening size of the screening operation I is 55mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the product of the secondary crushing operation is P 80 =30mm, the product of the medium crushing operation returns to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II;
[0035] The screening size of the screening II operation is 15mm. The screened product obtained by the screening II operation enters the photoelectric sorting I operation. The ore blocks with a spot coefficient greater than 0.5% in the photoelectric sorting I operation are high-sulfur products. The photoelectric sorting I operation selects the high-sulfur ore particles to obtain the first high-sulfur product. The ones not selected by the photoelectric sorting I operation are the first low-sulfur product, i.e., crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 =8mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening operation II, and then enters the screening operation III;
[0036] The screening size of the screening III operation is 5mm. The over-screen product obtained by the screening III operation enters the photoelectric sorting II operation. The ore blocks with a spot coefficient greater than 0.5% selected by the photoelectric sorting II operation are high-sulfur products. The photoelectric sorting II operation selects the high-sulfur ore particles to obtain the second high-sulfur product. The products not selected by the photoelectric sorting II operation are the second low-sulfur product, i.e., fine gravel. The obtained second high-sulfur product is returned to the above-mentioned fine crushing operation and enters the screening III operation after fine crushing; the under-screen product obtained by the screening III operation enters the screening IV operation;
[0037] The screening size of the screening IV operation is 2mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The heavy medium sorting uses ferrosilicon powder as the sorting medium. The specific gravity of the heavy medium liquid is controlled at 2.8. The high-density product obtained by the heavy medium sorting is the third high-sulfur product, and the low-density product obtained by the heavy medium sorting is the third low-sulfur product, i.e., coarse sand; the third high-sulfur product is subjected to rod milling operation to obtain a rod mill product with a particle size of P 80 =0.5mm;
[0038] S2: The undersize products obtained from the screening IV operation, the rod mill products and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation;
[0039] The grading particle size of hydraulic classification I is 0.30mm. The sand settling products of hydraulic classification I enter the spiral chute for sorting. The spiral chute uses a cubic parabola cross section. Type chute, pitch and diameter ratio is 0.7, feed concentration is 40%, first heavy mineral product, first intermediate product and first light mineral product are obtained respectively, first intermediate product enters suspended vibration cone gravity separation operation, suspended vibration cone concentrator is selected Type, feed ore concentration 25%, disk rotation period 240 seconds, vibration frequency 5.5Hz, respectively obtain the second heavy mineral product, the second intermediate product and the second light mineral product, the first heavy mineral product and the second heavy mineral product are combined to obtain coarse sulfur concentrate, the first light mineral product and the second light mineral product are combined to obtain medium sand;
[0040] The overflow product of hydraulic classification I operation enters hydraulic classification II operation. The classification particle size of hydraulic classification II operation is 0.10mm. The sand settling product of hydraulic classification II operation is combined with the second intermediate product and then ball milled. The particle size of the product of ball milling operation is P 80 =0.063mm, the ball-milled product is returned to the hydraulic classification II operation for re-classification;
[0041] The overflow product of hydraulic classification II operation enters the sulfur flotation operation, and the sulfur flotation operation carries out one roughing selection, one scavenging selection and one fine selection. The collector used is butyrate with a dosage of 36g / t (based on the mass of flotation feed), the adjusting agent is sulfuric acid and copper sulfate with a dosage of 200g / t (based on the mass of flotation feed) and 50g / t (based on the mass of flotation feed) respectively, and the frother is No. 2 oil with a dosage of 12g / t (based on the mass of flotation feed). The concentrate product of sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of sulfur flotation operation is fine sand.
[0042] The flotation indexes obtained in this example are shown in Table 1 below.
[0043] Table 1
[0044]
[0045]
[0046] The sulfur content of crushed stone, fine gravel, coarse sand, medium sand and fine sand products in Table 1 all meet the requirements for construction sand and gravel; the sulfur grade of coarse-grained sulfur concentrate and fine-grained sulfur concentrate all meet the requirements of sulfur concentrate products, and the overall sulfur recovery rate is 91.05%. The heavy metal ion content in the tail water (the sum of the sedimentation water and filtered water of each product) generated during the production process is as follows: Cu content = 0.18 mg / L, Pb content = 0.33 mg / L, Zn content = 0.19 mg / L, COD content = 12.49 mg / L, which can be recycled.
[0047] Example 2
[0048] This embodiment provides a method for the coordinated treatment of sulfur-containing tailings and sulfur-containing waste rock. The sulfur-containing tailings and the sulfur-containing waste rock are both from a mining enterprise in Hongling Town, Wengyuan County, Shaoguan City, Guangdong Province. The sulfur grades of the sulfur-containing tailings and the sulfur-containing waste rock are 1.34% and 1.88%, respectively. The mass ratio of the sulfur-containing tailings to the sulfur-containing waste rock is 1:4. The process flow of the treatment method is shown in FIG. Figure 1 As shown, the specific steps are as follows:
[0049] S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =50mm, the coarsely crushed product enters the screening I operation;
[0050] The screening size of the screening operation I is 30mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the product of the secondary crushing operation is P 80 =15mm, the product of the medium crushing operation returns to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II;
[0051] The screening size of the screening II operation is 10mm. The screened product obtained by the screening II operation enters the photoelectric sorting I operation. The ore blocks with a spot coefficient greater than 0.5% in the photoelectric sorting I operation are high-sulfur products. The photoelectric sorting I operation selects the high-sulfur ore particles to obtain the first high-sulfur product. The ore particles not selected by the photoelectric sorting I operation are the first low-sulfur product, i.e., crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 =5mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening operation II, and then enters the screening operation III;
[0052] The screening size of the screening III operation is 3mm. The over-screen product obtained by the screening III operation enters the photoelectric sorting II operation. The ore blocks with a spot coefficient greater than 0.5% selected by the photoelectric sorting II operation are high-sulfur products. The photoelectric sorting II operation selects the high-sulfur ore particles to obtain the second high-sulfur product. The products not selected by the photoelectric sorting II operation are the second low-sulfur product, i.e., fine gravel. The obtained second high-sulfur product is returned to the above-mentioned fine crushing operation and enters the screening III operation after fine crushing; the under-screen product obtained by the screening III operation enters the screening IV operation;
[0053] The screening size of the screening IV operation is 0.5mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The heavy medium sorting uses ferrosilicon powder as the sorting medium. The specific gravity of the heavy medium liquid is controlled at 2.5. The high-density product obtained by the heavy medium sorting is the third high-sulfur product, and the low-density product obtained by the heavy medium sorting is the third low-sulfur product, i.e., coarse sand; the third high-sulfur product is subjected to rod milling operation, and the particle size is P80=0.2mm;
[0054] S2: The undersize products obtained from the screening IV operation, the rod mill products and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation;
[0055] The grading particle size of hydraulic classification I is 0.15mm. The sand settling products of hydraulic classification I enter the spiral chute for sorting. The spiral chute uses a cubic parabola cross section. Type chute, pitch and diameter ratio is 0.5, feed concentration is 30%, first heavy mineral product, first intermediate product and first light mineral product are obtained respectively, first intermediate product enters suspended vibration cone gravity separation operation, suspended vibration cone concentrator is selected Type, feed ore concentration 20%, disk rotation period 200 seconds, vibration frequency 6.5Hz, respectively obtain the second heavy mineral product, the second intermediate product and the second light mineral product, the first heavy mineral product and the second heavy mineral product are combined to obtain coarse sulfur concentrate, the first light mineral product and the second light mineral product are combined to obtain medium sand;
[0056] The overflow product of hydraulic classification I operation enters hydraulic classification II operation. The classification particle size of hydraulic classification II operation is 0.045mm. The sedimentation product of hydraulic classification II operation is combined with the second intermediate product and then ball milled. The particle size of the product of ball milling operation is P 80 =0.045mm, the ball-milled product is returned to the hydraulic classification II operation for re-classification;
[0057] The overflow product of hydraulic classification II operation enters the sulfur flotation operation. The sulfur flotation operation conducts one roughing selection, one scavenging selection and one fine selection. The collectors used are butyrate and kerosene, with the dosages of 21g / t (based on the mass of flotation feed) and 9g / t (based on the mass of flotation feed) respectively. The adjusting agent is copper sulfate with the dosage of 80g / t (based on the mass of flotation feed). The frother is No. 2 oil with the dosage of 20g / t (based on the mass of flotation feed). The concentrate product of sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of sulfur flotation operation is fine sand.
[0058] The flotation indexes obtained in this example are shown in Table 2 below.
[0059] Table 2
[0060]
[0061] The sulfur content of crushed stone, fine gravel, coarse sand, medium sand and fine sand products in Table 2 all meet the requirements for construction sand and gravel; the sulfur grade of coarse-grained sulfur concentrate and fine-grained sulfur concentrate all meet the requirements of sulfur concentrate products, and the overall sulfur recovery rate is 92.31%. The heavy metal ion content in the tail water (the sum of the sedimentation water and filtered water of each product) generated during the production process is as follows: Cu content = 0.20 mg / L, Pb content = 0.50 mg / L, Zn content = 0.31 mg / L, COD content = 15.31 mg / L, which can be recycled.
[0062] Example 3
[0063] This embodiment provides a method for the coordinated treatment of sulfur-containing tailings and sulfur-containing waste rock. The sulfur-containing tailings and the sulfur-containing waste rock are both from a mining enterprise in Shirenzhang, Shixing County, Shaoguan City, Guangdong Province. The sulfur grades of the sulfur-containing tailings and the sulfur-containing waste rock are 0.83% and 0.91%, respectively. The mass ratio of the sulfur-containing tailings to the sulfur-containing waste rock is 2:3. The process flow of the treatment method is shown in FIG. Figure 1 As shown, the specific steps are as follows:
[0064] S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =65mm, the coarsely crushed product enters the screening I operation;
[0065] The screening size of the screening operation I is 50mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the secondary crushing product is P 80 =25mm, the product of the medium crushing operation returns to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II;
[0066] The screening size of the screening II operation is 12mm. The screened product obtained by the screening II operation enters the photoelectric sorting I operation. The ore blocks with a spot coefficient greater than 0.5% in the photoelectric sorting I operation are high-sulfur products. The photoelectric sorting I operation selects the high-sulfur ore particles to obtain the first high-sulfur product. The ore particles not selected by the photoelectric sorting I operation are the first low-sulfur product, i.e., crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 =6mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening II operation, and then enters the screening III operation;
[0067] The screening size of the screening III operation is 3.5mm. The screened product obtained by the screening III operation enters the photoelectric sorting II operation. The ore blocks with a spot coefficient greater than 0.5% selected by the photoelectric sorting II operation are high-sulfur products. The photoelectric sorting II operation selects the high-sulfur ore particles to obtain the second high-sulfur product. The products not selected by the photoelectric sorting II operation are the second low-sulfur product, i.e., fine gravel. The obtained second high-sulfur product is returned to the above-mentioned fine crushing operation and enters the screening III operation after fine crushing; the undersize product obtained by the screening III operation enters the screening IV operation;
[0068] The screening size of the screening IV operation is 1.2mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The heavy medium sorting uses ferrosilicon powder as the sorting medium. The specific gravity of the heavy medium liquid is controlled at 2.6. The high-density product obtained by the heavy medium sorting is the third high-sulfur product, and the low-density product obtained by the heavy medium sorting is the third low-sulfur product, i.e., coarse sand; the third high-sulfur product is subjected to rod milling operation to obtain a rod mill product with a particle size of P 80 =0.38mm;
[0069] S2: The undersize products obtained from the screening IV operation, the rod mill products and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation;
[0070] The grading particle size of hydraulic classification I is 0.25mm. The sand settling products of hydraulic classification I enter the spiral chute for sorting. The spiral chute uses a cubic parabola cross section. Type chute, pitch and diameter ratio is 0.55, feed concentration is 35%, first heavy mineral product, first intermediate product and first light mineral product are obtained respectively, first intermediate product enters suspended vibration cone gravity separation operation, suspended vibration cone concentrator is selected Type, feed ore concentration 22%, disk rotation period 210 seconds, vibration frequency 6.0Hz, respectively obtain the second heavy mineral product, the second intermediate product and the second light mineral product, the first heavy mineral product and the second heavy mineral product are combined to obtain coarse sulfur concentrate, the first light mineral product and the second light mineral product are combined to obtain medium sand;
[0071] The overflow product of hydraulic classification I operation enters hydraulic classification II operation. The classification particle size of hydraulic classification II operation is 0.074mm. The sedimentation product of hydraulic classification II operation is combined with the second intermediate product and then ball milled. The particle size of the product of ball milling operation is P 80 =0.050mm, the ball-milled product is returned to the hydraulic classification II operation for re-classification;
[0072] The overflow product of hydraulic classification II operation enters the sulfur flotation operation. The sulfur flotation operation conducts one roughing selection, one scavenging selection and two cleaning selections. The collector used is butyrate with a dosage of 15g / t (based on the mass of flotation feed), and the frother is No. 2 oil with a dosage of 10g / t (based on the mass of flotation feed). The concentrate product of the sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of the sulfur flotation operation is fine sand.
[0073] The flotation indexes obtained in this example are shown in Table 3 below.
[0074] Table 3
[0075]
[0076] The sulfur content of crushed stone, fine gravel, coarse sand, medium sand and fine sand products in Table 3 all meet the requirements for construction sand and gravel; the sulfur grade of coarse-grained sulfur concentrate and fine-grained sulfur concentrate all meet the requirements of sulfur concentrate products, and the overall sulfur recovery rate is 87.34%. The heavy metal ion content in the tail water (the sum of the sedimentation water and filtered water of each product) generated during the production process is as follows: Cu content = 0.17 mg / L, Pb content = 0.38 mg / L, Zn content = 0.09 mg / L, COD content = 10.71 mg / L, which can be recycled.
[0077] Example 4
[0078] This embodiment provides a method for the coordinated treatment of sulfur-containing tailings and sulfur-containing waste rock. The sulfur-containing tailings and the sulfur-containing waste rock are both from mining enterprises in Dayu County, Ganzhou City, Jiangxi Province. The sulfur grades of the sulfur-containing tailings and the sulfur-containing waste rock are 2.79% and 3.38%, respectively. The mass ratio of the sulfur-containing tailings to the sulfur-containing waste rock is 3:2. The process flow of the treatment method is shown in Figure 1 As shown, the specific steps are as follows:
[0079] S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =65mm, the coarsely crushed product enters the screening I operation;
[0080] The screening size of the screening operation I is 42mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the secondary crushing product is P 80 =20mm, the product of the medium crushing operation returns to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II;
[0081] The screening size of the screening II operation is 10mm. The screened product obtained by the screening II operation enters the photoelectric sorting I operation. The ore blocks with a spot coefficient greater than 0.5% in the photoelectric sorting I operation are high-sulfur products. The photoelectric sorting I operation selects the high-sulfur ore particles to obtain the first high-sulfur product. The ore particles not selected by the photoelectric sorting I operation are the first low-sulfur product, i.e., crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 =6.5mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening II operation, and then enters the screening III operation;
[0082] The screening size of the screening III operation is 3.2mm. The over-screen product obtained by the screening III operation enters the photoelectric sorting II operation. The ore blocks with a spot coefficient greater than 0.5% selected by the photoelectric sorting II operation are high-sulfur products. The photoelectric sorting II operation selects the high-sulfur ore particles to obtain the second high-sulfur product. The products not selected by the photoelectric sorting II operation are the second low-sulfur product, i.e., fine gravel. The obtained second high-sulfur product is returned to the above-mentioned fine crushing operation and enters the screening III operation after fine crushing; the under-screen product obtained by the screening III operation enters the screening IV operation;
[0083] The screening size of the screening IV operation is 1.5mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The heavy medium sorting uses ferrosilicon powder as the sorting medium. The specific gravity of the heavy medium liquid is controlled at 2.7. The high-density product obtained by the heavy medium sorting is the third high-sulfur product, and the low-density product obtained by the heavy medium sorting is the third low-sulfur product, i.e., coarse sand; the third high-sulfur product is subjected to rod milling operation to obtain a rod mill product with a particle size of P 80 =0.28mm;
[0084] S2: The undersize products obtained from the screening IV operation, the rod mill products and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation;
[0085] The grading particle size of hydraulic classification I is 0.28mm. The sand settling products of hydraulic classification I enter the spiral chute for sorting. The spiral chute uses a cubic parabola cross section. Type chute, pitch and diameter ratio is 0.55, feed concentration is 32%, first heavy mineral product, first intermediate product and first light mineral product are obtained respectively, first intermediate product enters suspended vibration cone gravity separation operation, suspended vibration cone concentrator is selected Type, feed ore concentration 24%, disk rotation period 230 seconds, vibration frequency 5.8Hz, respectively obtain the second heaviest mineral product, the second intermediate product and the second light mineral product, the first heaviest mineral product and the second heaviest mineral product are combined to obtain coarse sulfur concentrate, the first light mineral product and the second light mineral product are combined to obtain medium sand;
[0086] The overflow product of hydraulic classification I operation enters hydraulic classification II operation. The classification particle size of hydraulic classification II operation is 0.063mm. The sand settling product of hydraulic classification II operation is combined with the second intermediate product and then ball milled. The particle size of the product of ball milling operation is P 80 =0.056mm, the ball-milled product is returned to the hydraulic classification II operation for re-classification;
[0087] The overflow product of hydraulic classification II operation enters the sulfur flotation operation, and the sulfur flotation operation carries out one roughing selection, two scavenging selections and one fine selection. The collector used is butyrate with a dosage of 48g / t (based on the mass of flotation feed), and the frother is No. 2 oil with a dosage of 24g / t (based on the mass of flotation feed). The concentrate product of the sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of the sulfur flotation operation is fine sand.
[0088] The flotation indexes obtained in this example are shown in Table 4 below.
[0089] Table 4
[0090]
[0091] The sulfur content of crushed stone, fine gravel, coarse sand, medium sand and fine sand products in Table 4 all meet the requirements for construction sand and gravel; the sulfur grade of coarse-grained sulfur concentrate and fine-grained sulfur concentrate all meet the requirements of sulfur concentrate products, and the overall sulfur recovery rate is 94.65%. The heavy metal ion content in the tail water (the sum of the sedimentation water and filtered water of each product) generated during the production process is as follows: Cu content = 0.27 mg / L, Pb content = 0.64 mg / L, Zn content = 0.14 mg / L, COD content = 18.83 mg / L, which can be recycled.
[0092] Example 5
[0093] This embodiment provides a method for the coordinated treatment of sulfur-containing tailings and sulfur-containing waste rock. The sulfur-containing tailings and the sulfur-containing waste rock are both from a mining enterprise in Wangzigou, Zhouzhi County, Shaanxi Province. The sulfur grades of the sulfur-containing tailings and the sulfur-containing waste rock are 1.17% and 0.86%, respectively. The mass ratio of the sulfur-containing tailings to the sulfur-containing waste rock is 1:1. The process flow of the treatment method is shown in Figure 1 As shown, the specific steps are as follows:
[0094] S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =60mm, the coarsely crushed product enters the screening I operation;
[0095] The screening size of the screening operation I is 45mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the product of the secondary crushing operation is P 80 =25mm, the product of the medium crushing operation returns to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II;
[0096] The screening size of the screening II operation is 15mm. The screened product obtained by the screening II operation enters the photoelectric sorting I operation. The ore blocks with a spot coefficient greater than 0.5% in the photoelectric sorting I operation are high-sulfur products. The photoelectric sorting I operation selects the high-sulfur ore particles to obtain the first high-sulfur product. The ones not selected by the photoelectric sorting I operation are the first low-sulfur product, i.e., crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 =6.5mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening II operation, and then enters the screening III operation;
[0097] The screening size of the screening III operation is 3.6mm. The over-screen product obtained by the screening III operation enters the photoelectric sorting II operation. The ore blocks with a spot coefficient greater than 0.5% selected by the photoelectric sorting II operation are high-sulfur products. The photoelectric sorting II operation selects the high-sulfur ore particles to obtain the second high-sulfur product. The products not selected by the photoelectric sorting II operation are the second low-sulfur product, i.e., fine gravel. The obtained second high-sulfur product is returned to the above-mentioned fine crushing operation and enters the screening III operation after fine crushing; the under-screen product obtained by the screening III operation enters the screening IV operation;
[0098] The screening size of the screening IV operation is 1.5mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The heavy medium sorting uses ferrosilicon powder as the sorting medium. The specific gravity of the heavy medium liquid is controlled at 2.65. The high-density product obtained by the heavy medium sorting is the third high-sulfur product, and the low-density product obtained by the heavy medium sorting is the third low-sulfur product, i.e., coarse sand; the third high-sulfur product is subjected to rod milling operation to obtain a rod mill product with a particle size of P 80 =0.28mm;
[0099] S2: The undersize products obtained from the screening IV operation, the rod mill products and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation;
[0100] The grading particle size of hydraulic classification I is 0.28mm. The sand settling products of hydraulic classification I enter the spiral chute for sorting. The spiral chute uses a cubic parabola cross section. Type chute, pitch and diameter ratio is 0.65, feed concentration is 38%, first heavy mineral product, first intermediate product and first light mineral product are obtained respectively, first intermediate product enters suspended vibration cone gravity separation operation, suspended vibration cone concentrator is selected Type, feed ore concentration 24%, disk rotation period 225 seconds, vibration frequency 6.2Hz, respectively obtain the second heaviest mineral product, the second intermediate product and the second light mineral product, the first heaviest mineral product and the second heaviest mineral product are combined to obtain coarse-grained sulfur concentrate, the first light mineral product and the second light mineral product are combined to obtain medium sand;
[0101] The overflow product of hydraulic classification I operation enters hydraulic classification II operation. The classification particle size of hydraulic classification II operation is 0.074mm. The sedimentation product of hydraulic classification II operation is combined with the second intermediate product and then ball milled. The particle size of the product of ball milling operation is P 80 =0.048mm, the ball-milled product is returned to the hydraulic classification II operation for re-classification;
[0102] The overflow product of hydraulic classification II operation enters the sulfur flotation operation, and the sulfur flotation operation carries out one roughing selection, one scavenging selection and one fine selection. The collector used is butyrate with a dosage of 20g / t (based on the mass of flotation feed), and the frother is No. 2 oil with a dosage of 12g / t (based on the mass of flotation feed). The concentrate product of the sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of the sulfur flotation operation is fine sand.
[0103] The flotation indexes obtained in this example are shown in Table 5 below.
[0104] Table 5
[0105]
[0106] The sulfur content of crushed stone, fine gravel, coarse sand, medium sand and fine sand products in Table 5 all meet the requirements of building sand and gravel; the sulfur grade of coarse-grained sulfur concentrate and fine-grained sulfur concentrate all meet the requirements of sulfur concentrate products, and the overall sulfur recovery rate is 82.53%. The heavy metal ion content in the tail water (the sum of the sedimentation water and filtered water of each product) generated during the production process is as follows: Cu content = 0.35 mg / L, Pb content = 0.08 mg / L, Zn content = 0.18 mg / L, COD content = 13.24 mg / L, which can be recycled.
[0107] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for co-processing sulfur-containing tailings and sulfur-containing waste rock, characterized in that: Includes steps: S1: The sulfur-containing waste rock is firstly crushed to a particle size of P 80 =50~80mm, the coarsely crushed product enters the screening I operation; The screening size of the screening operation I is 30-55 mm. The screened product obtained from the screening operation I enters the secondary crushing operation. The particle size of the product of the secondary crushing operation is P 80 =15-30mm, the product of the medium crushing operation is returned to the screening operation I for screening, and the undersize product obtained from the screening operation I enters the screening operation II; The screening size of the screening II operation is 10-15 mm. The screened product obtained from the screening II operation enters the photoelectric sorting I operation. The photoelectric sorting I operation obtains the first high-sulfur product and the first low-sulfur product respectively. The first low-sulfur product is crushed stone. The first high-sulfur product enters the fine crushing operation. The particle size of the fine crushing product is P 80 =5~8mm, the product obtained from the fine crushing operation is combined with the undersize product obtained from the screening II operation, and then enters the screening III operation; The screening size of the screening III operation is 3-5 mm. The screened product obtained from the screening III operation enters the photoelectric sorting II operation. The photoelectric sorting II operation obtains the second high-sulfur product and the second low-sulfur product respectively. The obtained second low-sulfur product is fine gravel. The obtained second high-sulfur product is returned to the fine crushing operation and enters the screening III operation after fine crushing; the screened product obtained from the screening III operation enters the screening IV operation; The screening size of the screening IV operation is 0.5-2mm. The screened product obtained by the screening IV operation enters the heavy medium sorting operation. The specific gravity of the heavy medium liquid is controlled at 2.5-2.
8. The heavy medium sorting obtains the third high sulfur product and the third low sulfur product respectively. The third low sulfur product is coarse sand; the third high sulfur product is subjected to rod milling operation to obtain a rod mill product with a particle size of P 80 =0.2~0.5mm; S2: The undersize product obtained from the screening IV operation, the rod mill product and the sulfur-containing tailings are mixed and enter the hydraulic classification I operation; The classification particle size of hydraulic classification I operation is 0.15-0.30mm. The sedimentation product of hydraulic classification I operation enters the spiral chute sorting operation. The spiral chute uses a φ600-800 type chute with a cubic parabola cross-section, a pitch and diameter ratio of 0.5-0.7, and an ore concentration of 30-40%. The first heavy mineral product, the first intermediate product and the first light mineral product are obtained respectively. The first intermediate product enters the suspended vibration cone gravity separation operation. The suspended vibration cone concentrator uses a φ4000 type, with an ore concentration of 20-25%, a disk rotation period of 200-240 seconds, and a vibration frequency of 5.5-6.5Hz. The second heavy mineral product, the second intermediate product and the second light mineral product are obtained respectively. The first heavy mineral product and the second heavy mineral product are combined to obtain a coarse-grained sulfur concentrate, and the first light mineral product and the second light mineral product are combined to obtain medium sand; The overflow product of hydraulic classification I operation enters hydraulic classification II operation, and the classification particle size of hydraulic classification II operation is 0.045~0.10mm. The sedimentation product of hydraulic classification II operation is combined with the second intermediate product and enters the ball milling operation. The particle size of the product of ball milling operation is P 80 = 0.045-0.063 mm, the ball milled product is returned to the hydraulic classification II operation for re-classification; The overflow product of the hydraulic classification II operation enters the sulfur flotation operation. The concentrate product obtained from the sulfur flotation operation is fine-grained sulfur concentrate, and the tailings product of the sulfur flotation operation is fine sand.
2. The method according to claim 1, characterized in that The sulfur grade of the sulfur-containing tailings is 0.60-3.00%.
3. The method according to claim 1, characterized in that The sulfur grade of the sulfur-containing waste rock is 0.70-3.50%.
4. The method according to any one of claims 1 to 3, characterized in that: The mass ratio of the sulfur-containing waste rock to the sulfur-containing tailings is (1-4): (1-3).
5. The method according to claim 1, characterized in that The sulfur content of the crushed stone, fine gravel, coarse sand, medium sand and fine sand is ≤0.50%.
6. The method according to claim 1, characterized in that The sulfur content of the coarse-grained sulfur concentrate is greater than 29.0%.
7. The method according to claim 1, characterized in that The sulfur content of the fine-grained sulfur concentrate is greater than 28.0%.
8. The method according to claim 1, characterized in that The sulfur flotation operation adopts a beneficiation process of 1 roughing selection, 1-2 scavenging selections, and 1-2 cleaning selections, and the collectors used are butyrate and / or kerosene.