Titanium alloy flux-cored wire with good forming performance and preparation method and application of titanium alloy flux-cored wire

By adding flux core powder and magnesium fluoride to titanium alloy welding wire, combined with forming rollers and drawing processes, the problems of poor fluidity and cracks during titanium alloy welding are solved, and high-quality welding forming and anti-oxidation effects are achieved.

CN118752117APending Publication Date: 2024-10-11HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410823644.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Titanium alloys tend to form large molten pools during welding. The molten pool temperature is high, and the metal in the weld and heat-affected zone stays at high temperatures for a long time, resulting in grain growth, reduced joint plasticity and toughness, and prone to cracks and flow. Poor performance and difficult to form.

Method used

The flux-cored powder is combined with TA1 titanium ribbon. The flux-cored powder is composed of vanadium powder, aluminum powder, molybdenum powder, iron powder and magnesium fluoride. Titanium alloy flux-cored wire with good forming performance is prepared through forming roll and drawing process. Reduce the melting point of the welding wire, improve fluidity, and generate protective gas through magnesium fluoride to prevent oxidation and corrosion.

Benefits of technology

It effectively reduces the melting point of the welding wire, expands the welding process window, improves weld bead formation, reduces the risk of cracks, and forms a high-quality welded joint without pores and unfused defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752117A_ABST
    Figure CN118752117A_ABST
Patent Text Reader

Abstract

The invention discloses flux core powder. The flux core powder is prepared by mixing the following components in percentage by mass: 4-6% of vanadium powder, 6-10% of aluminum powder, 1-2% of molybdenum powder, 1-4% of iron powder, 1-3% of magnesium fluoride and the balance of titanium powder. The invention further discloses the titanium alloy flux-cored wire with the good forming performance and a preparation method and application of the titanium alloy flux-cored wire. The preparation process of the titanium alloy flux-cored wire is simple, a smelting procedure is not needed, the component proportion can be flexibly adjusted, and welding seam forming can be improved through formula adjustment. Deposited metal formed after welding is free of air holes, free of incomplete fusion and other defects and good in forming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding materials, and in particular relates to a titanium alloy flux-cored welding wire with good forming performance and a preparation method and application thereof. Background Art

[0002] Titanium alloys have the characteristics of low density, high specific strength, and excellent corrosion resistance. They are widely used in aerospace, shipbuilding, medical health and other fields. The design and development of high-performance titanium alloys has always been a research hotspot. However, titanium alloys have a high melting point, poor thermal conductivity, and poor fluidity. They are prone to forming a large molten pool during welding. The molten pool temperature is high, and the metal in the weld and heat-affected zone stays at high temperature for a long time. The grains tend to grow significantly, the plasticity and toughness of the joints are reduced, and cracks are very likely to occur.

[0003] Therefore, it is of practical significance to develop a titanium alloy flux-cored welding wire with good forming performance. Summary of the invention

[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a flux-cored powder and a titanium alloy flux-cored welding wire with good forming performance.

[0005] The technical problem that the present invention also aims to solve is to provide a method for preparing a titanium alloy flux-cored welding wire with good forming performance.

[0006] The technical problem that the present invention also aims to solve is to provide the application of flux-cored powder and the titanium alloy flux-cored welding wire with good forming performance in welding.

[0007] The final technical problem to be solved by the present invention is to provide a deposited metal.

[0008] Technical solution: In order to solve the above technical problems, the present invention provides a core powder, which is a mixture of the following components by mass fraction: 4% to 6% vanadium powder, 6% to 10% aluminum powder, 1% to 2% molybdenum powder, 1% to 4% iron powder, 1% to 3% magnesium fluoride and the remainder is titanium powder.

[0009] Wherein, the particle size of the aluminum powder and titanium powder is 200-250 meshes, and the particle size of the vanadium powder, molybdenum powder, iron powder and magnesium fluoride is 200-300 meshes.

[0010] The present invention also provides a titanium alloy flux-cored welding wire with good forming performance. The flux-cored welding wire is composed of a TA1 titanium strip and flux-cored powder filled therein.

[0011] The flux core powder accounts for 20-30% of the total weight of the titanium alloy flux cored welding wire.

[0012] The thickness of the TA1 titanium strip is 0.4 mm to 0.6 mm, and the chemical composition and its mass percentage are: N: ≤0.03%, H: 0.015%, and the balance is Ti.

[0013] Wherein, the diameter of the titanium alloy flux-cored welding wire is 1.2 mm to 2.4 mm.

[0014] The present invention also provides a method for preparing the titanium alloy flux-cored welding wire with good forming performance, comprising the following steps:

[0015] (1) using a forming roller to roll the TA1 titanium strip into a U-shape, and then adding the flux core powder into the U-shaped groove according to 20-30% of the total weight of the welding wire;

[0016] (2) The U-shaped groove is closed to wrap the powder core in it, and the wire is drawn and reduced in diameter step by step through a wire drawing die until the diameter reaches 1.2 to 2.4 mm to obtain the final product.

[0017] The invention also provides application of the flux-cored powder and the titanium alloy flux-cored welding wire with good forming performance in welding.

[0018] Wherein, the welding current is 150-170A, the welding voltage is 21-25V, and the welding speed is 0.4m / min.

[0019] The main functions of each component in the above-mentioned drug core are as follows:

[0020] Aluminum powder: Aluminum powder added to welding wire can help lower the melting point of weld metal and enhance the fluidity of weld metal, thereby facilitating the formation of the weld.

[0021] Larger particle size can reduce specific surface area, reduce friction between powder particles, reduce agglomeration, and improve fluidity. It can be seen from the above technical solution and the brief description of the functions of each component in the flux core that the present invention effectively reduces the melting point of the welding wire, expands the welding process window, and effectively reduces the surface tension of the weld bead by adding self-fluxing alloy elements such as aluminum to the flux core, effectively improving the weld bead forming. At the same time, aluminum powder has a high affinity for oxygen, and can react with oxides to generate slag that is easy to remove during welding, while playing a role in refining grains and improving the crack resistance of welded joints. In addition, the particle size of aluminum powder and titanium powder is 200-250 mesh, and the particle size of vanadium powder, molybdenum powder, iron powder, silicon powder, and magnesium fluoride is 200-300 mesh. Powder particles with small particle size have large specific surface area, high surface energy, and strong attraction between particles, which are prone to friction and affect fluidity. Larger particle size will reduce the contact surface between particles, reduce friction, and have better fluidity. At the same time, when the particle size is larger, due to the smaller surface area, the interaction forces such as van der Waals force between particles are reduced, so the agglomeration phenomenon is also reduced accordingly. However, too large a particle size reduces the reaction activity and reduces the welding efficiency. During the welding process, magnesium fluoride can generate shielding gas to protect the welding area from the influence of ambient gas, thereby ensuring the quality of the weld. In addition, magnesium fluoride can also improve the stability of the welding arc, prevent the interruption of the welding arc during welding, and improve the quality of the weld formation.

[0022] The present invention also provides a deposited metal, which is obtained after welding the welding wire, and its chemical composition and mass percentage include: V: 3.5% to 6.5%, Al: 6% to 10%, Mo: 1% to 2%, Fe: 1.6% to 2.8%, Mg: 0.05% to 0.1%, and the remainder is Ti.

[0023] Mechanism of the invention: The welding wire provided by the invention reduces the specific surface area, reduces the agglomeration phenomenon, and improves the fluidity by adding a core component with a larger particle size. At the same time, adding more self-fluxing alloy elements such as aluminum powder to the core effectively reduces the melting point of the welding wire, expands the welding process window, and effectively reduces the surface tension of the weld. At the same time, magnesium fluoride can improve the stability of the welding wire when it is melted, prevent oxidation and corrosion, and improve the weld formation.

[0024] Beneficial effects: Compared with the prior art, the present invention has the following advantages: the preparation process of the titanium alloy flux-cored welding wire of the present invention is simple, no smelting process is required, the composition ratio can be flexibly adjusted, and it is beneficial to improve the weld formation by adjusting the formula. The deposited metal formed after welding of the present invention has no defects such as pores and incomplete fusion, and has good formation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The macroscopic morphology of the weld overlay layer formed by the welding of the present invention;

[0026] Figure 2 The cross-sectional metallographic structure diagram of weld formation;

[0027] Figure 3 This is a macroscopic morphology of the weld overlay layer formed in Comparative Example 1;

[0028] Figure 4 This is a macroscopic morphology diagram of the weld overlay layer formed in Comparative Example 2. DETAILED DESCRIPTION

[0029] The present invention can be better understood according to the following examples. However, the specific core component ratios, process conditions and results described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims. Among them, the core components used in the following examples have the following mass percentage ranges: 4% to 6% vanadium powder, 6% to 10% aluminum powder, 1% to 2% molybdenum powder, 1% to 4% iron powder, 1% to 3% magnesium fluoride and the balance is titanium powder, and the filling rate of the core is 20% to 30%. The particle size of aluminum powder and titanium powder is 200 to 250 mesh, and the particle size of vanadium powder, molybdenum powder and iron powder is 200 to 300 mesh.

[0030] Example 1

[0031] A titanium alloy flux-cored welding wire with good forming performance comprises a TA1 titanium strip and a flux core, wherein the flux core is filled in the titanium strip, and the flux core components are prepared according to the following mass percentages: 4.2% vanadium powder, 6% aluminum powder, 1% molybdenum powder, 1.5% iron powder, 1% magnesium fluoride and the balance titanium powder, wherein the particle size of the aluminum powder and the titanium powder is 200 mesh, and the particle size of the vanadium powder, the molybdenum powder and the iron powder is 200 mesh. The various powders are placed in a powder mixer and mixed for 40 minutes, and then the mixed powder is added into a U-shaped 21×0.5mm TA1 titanium strip groove, and the filling rate is 28%. The U-shaped groove is then closed to wrap the flux powder therein. Then, the wire is passed through wire drawing dies with diameters of 4.2mm, 3.8mm, 3.5mm, 3.2mm, 2.8mm, 2.4mm and 2.0mm, and is drawn and reduced in diameter one by one, and finally a product with a diameter of 2.0mm is obtained. The welding current is 160A, the welding voltage is 24V, and the welding speed is 0.4m / min. The macroscopic morphology of the cladding layer is shown in Figure 1 , beautiful shape. Figure 2 The cross-sectional structure has no defects such as pores and unfused metal. The deposited metal forming conditions are shown in Table 1.

[0032] Example 2

[0033] A titanium alloy flux-cored welding wire with good forming performance comprises a TA1 titanium strip and a flux core, wherein the flux core is filled in the titanium strip, and the flux core components are prepared according to the following mass percentages: 5.0% vanadium powder, 8% aluminum powder, 1.5% molybdenum powder, 1.3% iron powder, 2% magnesium fluoride and the balance titanium powder, wherein the particle size of the aluminum powder and the titanium powder is 220 mesh, and the particle size of the vanadium powder, the molybdenum powder and the iron powder is 250 mesh. The various powders are placed in a powder mixer and mixed for 40 minutes, and then the mixed powder is added into a U-shaped 21×0.5mm TA1 titanium strip groove, and the filling rate is 25%. The U-shaped groove is then closed to wrap the flux powder therein. Then, it was passed through wire drawing dies with diameters of 4.2mm, 3.8mm, 3.5mm, 3.2mm, 2.8mm, 2.4mm, 2.0mm, 1.6mm, and 1.2mm, and was drawn and reduced in diameter one by one, and finally a product with a diameter of 1.2mm was obtained. The welding current was 150A, the welding voltage was 21V, and the welding speed was 0.4m / min. The deposited metal forming conditions are shown in Table 1.

[0034] Example 3

[0035] A titanium alloy flux-cored welding wire with good forming performance comprises a TA1 titanium strip and a flux core, wherein the flux core is filled in the titanium strip, and the flux core components are prepared according to the following mass percentages: 6% vanadium powder, 10% aluminum powder, 2% molybdenum powder, 1.8% iron powder, 3% magnesium fluoride and the balance titanium powder, wherein the particle size of the aluminum powder and the titanium powder is 250 mesh, and the particle size of the vanadium powder, the molybdenum powder and the iron powder is 300 mesh. The various powders are placed in a powder mixer and mixed for 40 minutes, and then the mixed powder is added into a U-shaped 21×0.5mm TA1 titanium strip groove, and the filling rate is 30%. The U-shaped groove is then closed to wrap the flux powder therein. Then, the wire is passed through wire drawing dies with diameters of 4.2mm, 3.8mm, 3.5mm, 3.2mm, 2.8mm and 2.4mm, and is drawn and reduced in diameter one by one, and finally a product with a diameter of 2.4mm is obtained. The welding current is 170A, the welding voltage is 25V, and the welding speed is 0.4m / min. The deposited metal forming conditions are shown in Table 1.

[0036] Comparative Example 1

[0037] A titanium alloy flux-cored welding wire with good forming performance comprises a TA1 titanium strip and a flux core, wherein the flux core is filled in the titanium strip, and the flux core components are prepared according to the following mass percentages: 4% vanadium powder, 6% aluminum powder, 1% molybdenum powder, 1.8% iron powder, 4% magnesium fluoride and the balance titanium powder, wherein the particle size of the aluminum powder and the titanium powder is 250 mesh, and the particle size of the vanadium powder, the molybdenum powder and the iron powder is 300 mesh. The various powders are placed in a powder mixer and mixed for 40 minutes, and then the mixed powder is added into a U-shaped 21×0.5mm TA1 titanium strip groove, and the filling rate is 30%. The U-shaped groove is then closed to wrap the flux powder therein. Then, the wire is passed through wire drawing dies with diameters of 4.2mm, 3.8mm, 3.5mm, 3.2mm, 2.8mm, 2.4mm and 2.0mm, and is drawn and reduced in diameter one by one, and finally a product with a diameter of 2.0mm is obtained. The welding current is 160A, the welding voltage is 23V, and the welding speed is 0.4m / min. The deposited metal forming conditions are shown in Table 1 and Figure 3 .

[0038] Comparative Example 2

[0039] A titanium alloy flux-cored welding wire with good forming performance comprises a TA1 titanium strip and a flux core, wherein the flux core is filled in the titanium strip, and the flux core components are prepared according to the following mass percentages: 5% vanadium powder, 6% aluminum powder, 1% molybdenum powder, 1.4% iron powder, 0.5% magnesium fluoride and the balance titanium powder, wherein the particle size of the aluminum powder and the titanium powder is 250 mesh, and the particle size of the vanadium powder, the molybdenum powder and the iron powder is 300 mesh. The various powders are placed in a powder mixer and mixed for 40 minutes, and then the mixed powder is added into a U-shaped 21×0.5mm TA1 titanium strip groove, and the filling rate is 30%. The U-shaped groove is then closed to wrap the flux powder therein. Then, the wire is passed through wire drawing dies with diameters of 4.2mm, 3.8mm, 3.5mm, 3.2mm, 2.8mm, 2.4mm and 2.0mm, and is drawn and reduced in diameter one by one, and finally a product with a diameter of 2.0mm is obtained. The welding current is 160A, the welding voltage is 23V, and the welding speed is 0.4m / min. The deposited metal forming conditions are shown in Table 1 and Figure 4 .

[0040] Table 1 Deposited metal forming conditions

[0041] Forming Example 1 No pores, no unfused defects, good forming Example 2 No pores, no unfused defects, good forming Example 3 No pores, no unfused defects, good forming Comparative Example 1 There are pores, no defects such as unfused, and good forming Comparative Example 2 No pores, no unfused defects, poor forming

[0042] From Table 1, Figure 3 and Figure 4 It can be seen that although the addition of magnesium fluoride can improve the stability of the welding wire during melting, prevent oxidation and corrosion, and improve the weld bead formation, when it is less than 1%, pores ( Figure 3 ), when it is higher than 3%, the powder fluidity deteriorates during the preparation of welding wire, destroys the uniformity of the core component, and the forming is also deteriorated ( Figure 4 ).

Claims

1. A drug core powder, characterized in that: The core powder is mixed with the following components by mass fraction: 4% to 6% vanadium powder, 6% to 10% aluminum powder, 1% to 2% molybdenum powder, 1% to 4% iron powder, 1% to 3% magnesium fluoride and the balance is titanium powder.

2. The drug core powder according to claim 1, characterized in that: The particle sizes of the aluminum powder and titanium powder are 200-250 meshes, and the particle sizes of the vanadium powder, molybdenum powder, iron powder and magnesium fluoride are 200-300 meshes.

3. A titanium alloy flux-cored welding wire with good forming performance, characterized in that: The flux-cored welding wire is composed of a TA1 titanium strip and the flux-cored powder according to claim 1 or 2 filled therein.

4. The titanium alloy flux-cored welding wire with good formability according to claim 3, characterized in that: The flux core powder accounts for 20-30% of the total weight of the titanium alloy flux cored welding wire.

5. The titanium alloy flux-cored welding wire with good formability according to claim 3, characterized in that: The TA1 titanium strip has a thickness of 0.4 mm to 0.6 mm, and its chemical composition and mass percentage are: N: ≤0.03%, H: 0.015%, and the balance is Ti.

6. The titanium alloy flux-cored welding wire with good formability according to claim 3, characterized in that: The diameter of the titanium alloy flux-cored welding wire is 1.2 mm to 2.4 mm.

7. The method for preparing a titanium alloy flux-cored welding wire with good formability according to any one of claims 3 to 6, characterized in that: The following steps are involved: (1) Rolling the TA1 titanium strip into a U-shape using a forming roller, and then adding the flux core powder into the U-shaped groove at a rate of 20-30% of the total weight of the welding wire; (2) The U-shaped groove is closed to wrap the powder core inside, and the wire is drawn and reduced in diameter through a wire drawing die, and finally the diameter reaches 1.2 to 2.4 mm to obtain the final product.

8. Use of the flux-cored powder according to claim 1 or 2 and the titanium alloy flux-cored welding wire with good formability according to any one of claims 3 to 6 in welding.

9. The use according to claim 8, characterized in that: The welding current is 150-170A, the welding voltage is 21-25V, and the welding speed is 0.4m / min.

10. A deposited metal, characterized in that: The deposited metal is obtained after welding the welding wire according to any one of claims 3 to 6, and its chemical composition and its mass percentage include: V: 3.5% to 6.5%, Al: 6% to 10%, Mo: 1% to 2%, Fe: 1.6% to 2.8%, Mg: 0.05% to 0.1%, and the balance is Ti.