Boron nitride nanotube prepared with assistance of carbon fibers and method

The carbon fiber-assisted preparation of boron nitride nanotubes solves the problems of boron source waste and high cost in the chemical vapor deposition method, and achieves efficient and uniform nanotube preparation, which is suitable for a variety of high-temperature and electronic device applications.

CN118754064AActive Publication Date: 2024-10-11SHANDONG JINGYI NEW MATERIALS CO LTD +1

Patent Information

Application Number
CN202411120186.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-11
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

In the existing technology, the preparation of boron nitride nanotubes by chemical vapor deposition involves waste of boron sources, high costs, and low preparation efficiency, which limits the wide application of boron nitride nanotubes.

Method used

Using a carbon fiber-assisted preparation method, the carbon fiber is impregnated with a magnesium salt solution to form a magnesium ion adsorption layer, and then boric acid is added in a water bath for ammoniation treatment to generate boron nitride nanotubes, which avoids the addition of external boron sources and simplifies the process. .

Benefits of technology

It improves the preparation efficiency and uniformity of boron nitride nanotubes, reduces equipment costs and process complexity, realizes large-scale industrial production, and is suitable for high-temperature and high-frequency electronic devices and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754064A_ABST
    Figure CN118754064A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nanotube materials, and particularly relates to a carbon fiber-assisted boron nitride nanotube and method, the carbon fiber-assisted boron nitride nanotube preparation method comprises the following steps: (1) carbon fiber pretreatment; (2) processing a boron nitride nanotube precursor; and (3) precursor ammonification. According to the preparation method of the boron nitride nanotube, an external boron source does not need to be additionally added as a catalyst, the growth difficulty is small, and the product is uniform; the preparation process is simple, the requirement for equipment is low, controllability is high, collection is easy, industrialization is easy to achieve, the equipment cost is greatly saved, the used chemical raw materials are low in price and easy to obtain, and the prepared boron nitride nanotube can be applied to the fields of thermal interface materials, high-thermal-conductivity insulating materials and high-temperature solid lubricants and has wide application prospects. The method can be applied to the fields of high-frequency high-integration electronic devices, communication base stations, data centers, aerospace and national defense military industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanotube materials, and in particular relates to a carbon fiber-assisted preparation method of a boron nitride nanotube. Background Art

[0002] Boron nitride nanotubes (BNNTs) are structurally similar to carbon nanotubes (CNTs). Both BNNTs and CNTs share inherent properties, such as exceptional specific stiffness and strength, a superior Young's modulus, and high thermal conductivity. Despite these similarities, the polarity of the BN bond imparts distinct electronic properties to BNNTs. BNNTs possess a large bandgap (approximately 5.9 eV), making them wide-bandgap semiconductors. Their electrical properties are unaffected by changes in diameter or chirality, unlike CNTs, whose electrical properties are characterized by chirality. This property of BNNTs holds promise for a wide range of applications in short-wavelength light-emitting devices, UV detection, and high-temperature, high-power electronics. Furthermore, compared to CNTs, BNNTs exhibit greater oxidation resistance and chemical stability, making them more suitable for high-temperature applications. BNNTs also exhibit other properties, such as piezoelectricity, biocompatibility, excellent absorption of UV radiation, and neutron shielding. Therefore, large-scale production of high-purity and high-quality BNNTs is essential to meet these applications.

[0003] BNNTs are a highly promising aerospace material, but only a few institutions are currently able to mass-produce them. The high-quality synthesis of BNNTs remains a challenge for both academia and industry. In-depth research into the properties and large-scale applications of BNNTs is only possible with the availability of mature manufacturing methods. Researchers have investigated several methods for BNNT growth, including arc discharge, laser ablation, template-based methods, thermal plasma, and chemical vapor deposition. Chemical vapor deposition is considered an ideal research approach due to its low cost and high controllability. However, current chemical vapor deposition methods for the production of boron nitride nanotubes typically involve depositing a gaseous active boron source onto a growth substrate by reacting boron and boron oxide with metal oxides at high temperatures. This gas-phase reaction results in significant waste of boron source, resulting in low yields, making BNNT production difficult and expensive, and severely limiting their application. Furthermore, compared to existing technologies, there are currently no patents or literature reports on the use of carbon fibers as an auxiliary material in the preparation of boron nitride nanotube structures. Summary of the Invention

[0004] In view of the shortcomings of the above-mentioned prior art, the present invention provides a method and method for preparing boron nitride nanotubes assisted by carbon fibers. The specific technical solution is as follows: A method for preparing boron nitride nanotubes assisted by carbon fiber comprises the following steps: (1) Carbon fiber pretreatment: Mix magnesium salt and solvent and stir to dissolve to obtain magnesium salt solution, then immerse carbon fiber in magnesium salt solution and stir thoroughly, and dry after immersion to obtain carbon fiber adsorbed with magnesium ions, which is recorded as Mg@CFs; (2) Treatment of boron nitride nanotube precursor: dissolve boric acid in deionized water, add Mg@CFs to the boric acid solution, heat and stir in a water bath, and then take out and fully dry to obtain a boric acid-containing Mg@CFs precursor; (3) Precursor amination: The Mg@CFs precursor containing boric acid is placed in an inert atmosphere, heated, and then ammonia gas is introduced for amination treatment, and then naturally cooled to room temperature to obtain boron nitride nanotubes.

[0005] The present invention prepares boron nitride nanotubes with the assistance of carbon fibers. The carbon fibers absorb magnesium ions and attach a layer of boric acid, causing the carbon fibers to crack at high temperatures and derive boron nitride nanotubes. The prepared boron nitride nanotubes are grown by cracking the carbon fibers. The production efficiency is high, the cost is controllable, and the boron nitride nanotubes can meet the needs of large-scale industrial production.

[0006] Furthermore, in the step (1), the mass ratio of the carbon fiber to the magnesium salt is 1:1-100.

[0007] Furthermore, in step (1), the magnesium salt may be, but is not limited to, magnesium chloride hexahydrate, anhydrous magnesium chloride, magnesium sulfate heptahydrate, anhydrous magnesium sulfate, magnesium nitrate hexahydrate, anhydrous magnesium nitrate, and the like.

[0008] Furthermore, in step (1), the solvent may be, but is not limited to, deionized water, anhydrous ethanol, anhydrous methanol and isopropanol.

[0009] Furthermore, in step (1), the concentration of the magnesium salt solution is 0.1-50 mol / L.

[0010] Furthermore, in the step (1), the immersion time is 1 to 48 hours, and the drying temperature is 40 to 200°C.

[0011] Furthermore, in step (2), the concentration of the boric acid solution is 0.1-50 mol / L.

[0012] Furthermore, in step (2), the water bath heating temperature is 30-100°C, and the drying temperature is 40-200°C.

[0013] Furthermore, in step (3), the inert gas used is a protective atmosphere such as nitrogen, argon, helium, neon or radon.

[0014] Furthermore, in step (3), the temperature is raised to 1000-1800°C at a rate of 1-15°C / min, and the ammoniation treatment time is 1-20 hours.

[0015] Furthermore, in step (3), the boric acid-containing Mg@CFs is placed in a crucible, and the crucible can be but is not limited to an alumina crucible, a silicon nitride crucible or a boron nitride crucible.

[0016] The beneficial effects of the present invention are: The carbon fiber-assisted method for preparing boron nitride nanotubes of the present invention does not require the addition of an external boron source as a catalyst, has low growth difficulty, and produces uniform products compared to conventional chemical vapor deposition methods. Compared to conventional methods, the preparation process is simple, solving the problems of expensive equipment and complex processes, requiring low equipment requirements, being highly controllable and easy to collect, and being easy to industrialize, thereby greatly saving equipment costs. The chemical raw materials used are inexpensive and readily available, and the prepared boron nitride nanotubes can be applied in the fields of thermal interface materials, high thermal conductivity insulating materials, and high-temperature solid lubricants, and can be applied in high-frequency and high-integration electronic devices, communication base stations, data centers, aerospace, and national defense military industries. Furthermore, compared to the prior art, the carbon fiber-assisted boron nitride nanotubes and methods according to the embodiments of the present invention are highly controllable, easy to prepare, simple to operate, and easy to mass-produce, and have good flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the SEM image of the sample prepared in Example 1 of the present invention; Figure 2 This is the X-ray diffraction (XRD) pattern of the sample prepared in Example 1 of the present invention; Figure 3 This is a Fourier transform infrared (FTIR) spectrum of the sample prepared in Example 1 of the present invention; Figure 4 This is the SEM image of the sample prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0018] The principles and features of the present invention are described below with reference to examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0019] Example 1: A method for preparing boron nitride nanotubes assisted by carbon fiber comprises the following steps: (1) Carbon fiber pretreatment: 1 g of carbon fiber was immersed in 3 mol / L magnesium chloride hexahydrate methanol solution, stirred thoroughly, and allowed to stand for 12 h. The carbon fiber was taken out and washed with methanol three times, and then dried at 65 °C for 12 h to obtain carbon fiber adsorbed with magnesium ions, which was recorded as Mg@CFs. (2) Treatment of boron nitride nanotube precursor: 0.5 g Mg@CFs was placed in a 1 mol / L boric acid solution, stirred in an 80 °C water bath, and then taken out and dried at 65 °C for 12 h to obtain a boric acid-containing Mg@CFs precursor. (3) Precursor amination: The prepared Mg@CFs precursor powder was placed in an alumina crucible and continuously heated to 1400°C in a 100 sccm nitrogen atmosphere at a heating rate of 2°C / min. The nitrogen was then switched to 100 sccm ammonia for ammonia treatment for 5 h. After the reaction was completed, the ammonia was switched to 100 sccm nitrogen and the mixture was cooled to room temperature and then taken out to obtain boron nitride nanotubes.

[0020] Example 2 In this embodiment, in the step (1) of pre-treating the carbon fiber, 1 g of the carbon fiber is immersed in a 3 mol / L magnesium chloride hexahydrate aqueous solution, and the rest is the same as in Example 1.

[0021] like Figure 1 and Figure 4 As shown in the electron microscope photos, the boron nitride nanotubes obtained in Example 1 and Example 2 of the present invention grew well and had high uniformity.

[0022] like Figure 2 As shown in the XRD pattern, the XRD diffraction pattern of the boron nitride nanotubes obtained in Example 1 is a characteristic signal of h-BN, proving that the prepared boron nitride nanotubes are h-BN structures with high purity.

[0023] like Figure 3 As shown in the FTIR spectrum, the boron nitride nanotubes obtained in Example 1 have a FTIR spectrum at 1373 cm −1 and 801 cm −1 The characteristic absorption peak of BN was obtained near 801 cm −1 The BNB bending vibration of BN is 1373 cm −1 The absorption frequency at corresponds to the in-plane stretching vibration of BN, and these two strong absorption peaks are typical h-BN infrared characteristic peaks.

[0024] It can be seen that the method of preparing boron nitride nanotubes with the assistance of carbon fibers of the present invention does not require the addition of an external boron source as a catalyst, and the obtained boron nitride nanotubes have low growth difficulty, good growth, and strong uniformity; in addition, the chemical raw materials used are inexpensive and easily available, the preparation process is simple, the equipment requirements are low, the controllability is strong, and the collection is easy, and it is easy to realize industrialization, which greatly saves equipment costs.

[0025] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing boron nitride nanotubes assisted by carbon fiber, characterized in that: The steps include: (1) Carbon fiber pretreatment: Mix magnesium salt and solvent and stir to dissolve to obtain a magnesium salt solution, then immerse the carbon fiber in the magnesium salt solution and stir thoroughly, and dry after immersion to obtain carbon fiber adsorbed with magnesium ions, recorded as Mg@CFs; (2) Treatment of boron nitride nanotube precursor: dissolve boric acid in deionized water, add Mg@CFs to the boric acid solution, heat and stir in a water bath, and then take out and fully dry to obtain a boric acid-containing Mg@CFs precursor; (3) Precursor amination: The boric acid-containing Mg@CFs precursor is placed in an inert atmosphere, heated, and then ammonia gas is introduced for amination treatment, and then naturally cooled to room temperature to obtain boron nitride nanotubes.

2. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (1), the mass ratio of the carbon fiber to the magnesium salt is 1:1-100.

3. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (1), the magnesium salt is magnesium chloride hexahydrate, magnesium chloride anhydrous, magnesium sulfate heptahydrate, anhydrous magnesium sulfate, magnesium nitrate hexahydrate or anhydrous magnesium nitrate; and the solvent is deionized water, anhydrous ethanol, anhydrous methanol and isopropanol.

4. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (1), the concentration of the magnesium salt solution is 0.1-50 mol / L.

5. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (1), the immersion time is 1 to 48 hours, and the drying temperature is 40 to 200°C.

6. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (2), the concentration of the boric acid solution is 0.1-50 mol / L.

7. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (2), the water bath heating temperature is 30-100°C, and the drying temperature is 40-200°C.

8. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (3), the temperature is raised to 1000-1800°C at a rate of 1-15°C / min, and the ammoniation treatment time is 1-20h.

9. The method for preparing boron nitride nanotubes assisted by carbon fiber according to claim 1, characterized in that: In the step (3), the inert gas used is nitrogen, argon, helium, neon or radon; the boric acid-containing Mg@CFs is placed in a crucible, and the crucible is an alumina crucible, a silicon nitride crucible or a boron nitride crucible.

10. A boron nitride nanotube, characterized in that: The boron nitride nanotubes are prepared by the method for preparing boron nitride nanotubes with the assistance of carbon fibers as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of boron nitride-coated carbon nanotubes

    CN103172050A

  • Preparation method of boron nitride nano tube

    CN103922295A

  • Method for preparing hexagonal boron nitride by taking carbon nanofiber as template

    CN109706550A

  • Preparation method of hexagonal boron nitride nanowire

    CN116040591A

  • Method for manufacturing boron nitride nanotube by using oxide catalyst

    JP2002097004A

Cited By

  • Method for preparing high-length-diameter-ratio boron nitride nanotube by paper pulp template method and application of high-length-diameter-ratio boron nitride nanotube

    CN120483062A

  • Method for preparing high-aspect-ratio boron nitride nanotubes by paper pulp template method and application thereof

    CN120483062B