Method for preparing battery-grade iron phosphate and recycling gold, copper and cobalt from sulfuric-acid residues

Through the mixed leaching method of sulfuric acid slag, phosphoric acid solution and elemental iron, combined with the precipitation reaction of oxidant to adjust the pH value, the problem of impurities in sulfuric acid slag affecting the purity of iron phosphate and the cumbersome steps of recovering gold, copper and cobalt are solved, and the production of high-purity iron phosphate is realized. Production and efficient recovery of gold, copper and cobalt reduce production costs.

CN118754073AActive Publication Date: 2024-10-11WUHAN INST OF TECH

Patent Information

Application Number
CN202411001679.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In the existing technology, the application of sulfuric acid slag in the steel industry is limited, and the impurities in the sulfuric acid slag affect the purity of iron phosphate. The steps for recovering gold, copper, and cobalt are cumbersome, and its resource value cannot be fully utilized.

Method used

The mixed leaching method of sulfuric acid residue, phosphoric acid solution and elemental iron is used, and the pH value is adjusted by an oxidant to perform a precipitation reaction to generate high-purity iron phosphate, and the leaching residue is used for the recovery of gold, copper and cobalt, simplifying the process flow.

Benefits of technology

It improves the purity of iron phosphate and the recovery rate of gold, copper and cobalt, reduces production costs, simplifies the process flow, and achieves efficient utilization of sulfuric acid residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754073A_ABST
    Figure CN118754073A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt from sulfuric-acid residues. The method comprises the following steps: mixing the sulfuric-acid residues with a phosphoric acid solution and elemental iron, and leaching to obtain a ferrous dihydrogen phosphate leaching solution and leaching residues; an oxidizing agent is added into the ferrous dihydrogen phosphate leachate, the pH is adjusted, a precipitation reaction is conducted, iron phosphate dehydrate precipitate and a phosphoric acid solution are obtained, and the iron phosphate dehydrate precipitate is calcined to obtain iron phosphate; the leaching residues are used for recycling gold, copper and cobalt. The method is high in iron recovery rate, the obtained iron phosphate is high in purity, meanwhile, gold, copper and cobalt in the sulfuric-acid residues can be effectively recovered, the process is simple, cost is low, and the method is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing ferric phosphate, and in particular to a method for preparing battery-grade ferric phosphate by utilizing sulfuric acid slag and recovering gold, copper and cobalt, and belongs to the field of new energy battery materials. Background Art

[0002] Sulfuric acid slag is a byproduct of pyrite acid production. Its main component is iron oxide. Every ton of sulfuric acid produced produces about 0.5 tons of sulphuric acid slag. my country produces about 20 million tons of sulphuric acid slag each year, and most of it is used as steel raw materials. The iron grade of sulphuric acid slag is generally between 55% and 60%. In addition to iron, it also contains impurities such as silicon, calcium, magnesium and non-ferrous metals. When used as an ironmaking raw material, these impurity elements will affect the smelting process. Therefore, the application of sulphuric acid slag in the steel industry is very limited and cannot be fully utilized as a resource.

[0003] With the rapid development of the new energy industry, the production capacity of lithium iron phosphate materials has expanded rapidly. Among them, iron phosphate, as a precursor of lithium iron phosphate materials, has also been the focus of attention. The methods for synthesizing battery-grade iron phosphate mainly include liquid phase precipitation, hydrothermal synthesis, sol-gel, air oxidation and controlled crystallization, among which the most widely used is liquid phase precipitation. In the liquid phase precipitation method, cheap iron source is an important link in controlling its production cost. As a cheap iron-containing secondary resource, sulfuric acid slag has a large output and a wide distribution range. If sulfuric acid slag can be used as an iron source for iron phosphate production, it can not only reduce the production cost of iron phosphate, but also increase the value of sulfuric acid slag. Previous studies have used sulfuric acid slag as an iron source for direct phosphoric acid leaching to prepare iron phosphate products. However, in this process, the silicon component impurities in the sulfuric acid slag cannot be dissolved in phosphoric acid, and will precipitate together with dihydrate iron phosphate, affecting the purity of iron phosphate. Hydrofluoric acid is required for subsequent impurity removal, and the process is complicated.

[0004] In addition, when currently sulfuric acid slag is used to recover gold, copper and cobalt, iron needs to be removed first and then gold, copper and cobalt are separated, and the steps are cumbersome. The present invention can prepare iron phosphate and effectively separate gold, copper and cobalt at the same time, simplifying the recovery steps and improving the separation recovery rate of each element.

[0005] Therefore, the development of a simple method for preparing battery-grade iron phosphate using sulfuric acid slag as an iron source and recovering gold, copper and cobalt is of great significance to the sustainable development of my country's chemical and new energy industries. Summary of the invention

[0006] In view of the defects of the prior art, the purpose of the present invention is to provide a method for preparing battery-grade iron phosphate using sulfuric acid slag and recovering gold, copper and cobalt. The method can improve the recovery rate of iron in sulfuric acid slag, and the obtained iron phosphate has high purity and can be directly used for battery preparation. At the same time, gold, copper and cobalt can be effectively recovered. The method is simple, low-cost and suitable for industrial production.

[0007] In order to achieve the above technical purpose, the present invention provides a method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag. The method comprises the following steps: mixing sulfuric acid slag with a phosphoric acid solution and elemental iron for leaching to obtain a ferrous dihydrogen phosphate leaching solution and leaching slag; adding an oxidant to the ferrous dihydrogen phosphate leaching solution and adjusting the pH to carry out a precipitation reaction to obtain a dihydrate iron phosphate precipitate and a phosphoric acid solution; the dihydrate iron phosphate precipitate is calcined to obtain iron phosphate; and the leaching slag is used to recover gold, copper and cobalt.

[0008] The invention cleverly utilizes the reducing property of elemental iron, reduces trivalent iron in the sulfuric acid slag to divalent iron in the phosphoric acid leaching process, and reacts with phosphoric acid to generate ferrous dihydrogen phosphate, so that all iron components in the raw material are converted into soluble ferrous dihydrogen phosphate salt, while silicon, calcium impurities, copper, cobalt and other components are insoluble; on the other hand, the entry of elemental iron into the system can reduce ionic gold, copper and cobalt elements in the solution to elemental gold, copper and cobalt, thereby reducing the loss rate of gold, copper and cobalt in the leaching process, improving the content and recovery rate of gold, copper and cobalt in the leaching slag, and also making the iron component in the sulfuric acid slag highly selectively leached to obtain a high-purity ferrous dihydrogen phosphate solution, while the gold, copper and cobalt in the leaching slag are enriched and can be directly used for separating and recovering gold, copper and cobalt.

[0009] As a preferred solution, the molar ratio of Fe2O3 to phosphoric acid and elemental iron in the sulfuric acid slag is 1:6-10:1.5-3.

[0010] As a preferred solution, during the leaching process, the concentration of the phosphoric acid solution is 3-8 mol / L, the liquid-solid ratio is 6-15 ml / g, the temperature is 30-100° C., more preferably 60-100° C., and the time is 2-6 h.

[0011] As a preferred solution, the oxidant includes at least one of hydrogen peroxide, air and oxygen.

[0012] As a preferred solution, when the oxidant is hydrogen peroxide, the molar ratio of H2O2 to ferrous dihydrogen phosphate in the hydrogen peroxide is 1:2 to 2.5.

[0013] As a preferred solution, when the oxidant is air or oxygen, the gas flow rate is 50 to 200 mL / min.

[0014] As a preferred solution, the precipitation reaction process is: stirring the reaction at a temperature of 60 to 80° C. for 1 to 3 hours. Stirring the reaction at a temperature of 60 to 80° C. until the iron content in the solution does not exceed 0.4 g / L, the precipitation reaction is complete.

[0015] As a preferred solution, after the precipitation reaction is completed, the iron content in the solution is ≤0.4 g / L.

[0016] As a preferred solution, the calcination conditions are: temperature of 500-700° C. and time of 60-180 min.

[0017] As a preferred solution, the process of recovering gold, copper and cobalt is as follows: leaching the leached residue with sulfuric acid and then performing solid-liquid separation to obtain a copper-cobalt leaching solution and a gold-containing leaching residue; mixing the copper-cobalt leaching solution with a sodium thiosulfate solution and adjusting the pH to perform a copper precipitation reaction, and then performing solid-liquid separation to obtain copper slag and a cobalt-containing solution; and leaching the gold-containing leaching residue with a gold leaching agent to obtain a gold-containing leaching solution.

[0018] As a preferred solution, in the process of recovering copper and cobalt, the mass concentration of the sodium thiosulfate solution is 8-10%; the amount of sodium thiosulfate in the sodium thiosulfate solution is 2-3 times the molar amount of the copper element; the pH is adjusted to 4.0-6.0, and the pH regulator is sodium carbonate; the temperature is 80-100° C., and the time is 3-4 hours.

[0019] As a preferred solution, the cobalt-containing solution uses a sodium carbonate solution with a mass fraction of 8-10% as a precipitant, adjusts the solution pH to 8.0-9.0, reacts at room temperature with stirring for 3-4 hours, and then separates the solid and liquid to obtain cobalt slag.

[0020] As a preferred solution, the gold leaching agent includes at least one of cyanide, thiosulfate and thiourea.

[0021] As a preferred solution, the molar dosage of the gold leaching agent is determined according to the content of gold element in the sulfate slag, and the dosage is 1.2 to 1.5 times the theoretical dosage.

[0022] As a preferred solution, the leaching temperature of the gold-containing leaching slag is 20-70° C., and the leaching time is 6-10 hours.

[0023] As a preferred solution, in the desorption solution, the mass concentration of sodium chloride is 1-5%, and the mass concentration of sodium hydroxide is 1-2%.

[0024] As a preferred solution, the gold mud is dried and melted to obtain elemental gold.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The present invention uses sulfuric acid slag as an iron source and prepares a high-value-added battery-grade iron phosphate product through a phosphoric acid reduction leaching-oxidation precipitation-roasting dehydration process. Compared with the traditional iron phosphate production process, the present invention has the advantages of a wide source of raw materials and low cost, thereby realizing the high-value-added utilization of industrial by-products.

[0027] (2) The present invention adds an iron reducing agent during the phosphoric acid leaching process, ingeniously utilizes the reducing property of elemental iron, and reduces the trivalent iron ions generated during the acid leaching process to divalent iron ions, thereby causing them to react with phosphate to generate soluble ferrous dihydrogen phosphate, while the impurity components in the sulfate slag do not dissolve into the leaching slag, thereby achieving the phase transformation of iron and phosphorus and the removal of impurities in one step.

[0028] (3) While obtaining the iron phosphate product, the present invention can directly use the leaching residue obtained in the phosphoric acid reduction leaching process to separate and recover gold, copper and cobalt. The gold, copper and cobalt grades in the leaching residue are greatly improved compared with the sulfate residue raw material. In the subsequent recovery process, the reagent consumption can be reduced, and the gold, copper and cobalt ion concentration of the system can be increased, which greatly simplifies the process of recovering gold, copper and cobalt using sulfate residue and significantly improves the resource utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0030] Figure 1 The present invention is a process flow chart for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag.

[0031] Figure 2 This is the XRD diagram of the leached residue obtained after reduction leaching of the sulfuric acid residue in Example 1.

[0032] Figure 3 This is the XRD spectrum of the iron phosphate dihydrate prepared in Example 1.

[0033] Figure 4 This is the SEM image of the iron phosphate dihydrate prepared in Example 2.

[0034] Figure 5 This is the XRD diagram of the leached residue obtained after reduction leaching of the sulfuric acid residue in Comparative Example 1. DETAILED DESCRIPTION

[0035] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] This embodiment uses sulfuric acid slag from a sulfuric acid plant with an iron content of 60.87%. The other main components are shown in Table 1.

[0038] Table 1 Main chemical components of sulfuric acid slag / %

[0039]

[0040] This was used as the raw material for the phosphoric acid reduction leaching test. The molar ratio of Fe2O3, phosphoric acid, and reducing agent in the sulfate slag was controlled to be 1:8:1.6, the reducing agent was elemental iron powder, the phosphoric acid concentration was 5 mol / L, the liquid-solid ratio was 8 ml / g, and the leaching temperature was controlled at 70°C. After 4 hours of leaching, the iron component in the sulfate slag was basically converted into soluble ferrous dihydrogen phosphate, and the main components of the leached slag were siliceous gangue and insoluble metals such as gold, copper, and cobalt (( Figure 2 The leached residue is shown in Table 2, which can be used for subsequent extraction of valuable metals.

[0041] Table 2 Chemical composition analysis of reduction leaching residue / %

[0042]

[0043] After solid-liquid separation, a slightly excess amount of 25% mass concentration hydrogen peroxide was added to the ferrous dihydrogen phosphate solution, wherein the molar ratio of Fe2O3 to H2O2 was 1:1.7; the reaction temperature of the hydrogen peroxide oxidation step was controlled at 60°C and stirred for 3 hours until the iron ion content of the supernatant was less than 0.4g / L. After solid-liquid separation, the obtained dihydrated iron phosphate product (( Figure 3 The product was calcined at 550°C for 2 hours to obtain an iron phosphate product with an iron recovery rate of 76.63%. The chemical composition of the iron phosphate product is shown in Table 3.

[0044] Table 3 All element analysis of iron phosphate / %

[0045]

[0046] The leaching residue obtained during phosphoric acid leaching is used to recover gold, copper and cobalt:

[0047] The leaching residue was mixed with 1 mol / L sulfuric acid at a solid-liquid mass ratio of 1:3 for 3 hours to obtain a copper-cobalt leaching solution and a gold-containing leaching residue. Sodium thiosulfate with a mass concentration of 10% was added to the copper-cobalt leaching solution, and the amount was twice the concentration of copper ions. Sodium carbonate was used as a pH adjuster, and the pH value of the mixed solution was adjusted to 5. The stirring temperature was 80°C and the stirring time was 3 hours. Finally, copper precipitate residue and cobalt-rich solution were obtained, and the copper recovery rate was 68.23%.

[0048] Sodium carbonate with a mass concentration of 9% was added as a precipitant to the cobalt-rich solution, and the pH value of the solution was adjusted to 8. After stirring at room temperature for 4 hours, solid-liquid separation was performed to obtain cobalt precipitate slag, and the cobalt recovery rate was 59.25%.

[0049] The gold-containing leaching residue was mixed and stirred with 0.3 mol / L sodium thiosulfate solution, with a solid-liquid mass ratio of 1:4, a system pH value of 10.5, a stirring time of 6 hours, and a stirring temperature of 40°C, and then the solid-liquid separation was performed to obtain a gold leaching solution, and the gold leaching solution was adsorbed on activated carbon, with an activated carbon dosage of 10 g / L and a stirring time of 24 hours. The mixed solution was then solid-liquid separated to obtain a gold-loaded carbon solid phase, and then a 5wt% NaCl and 2wt% NaOH mixed desorption solution was used to desorb the gold-loaded carbon, with a desorption solution dosage of 0.05 L / g and a desorption time of 24 hours to obtain a gold-rich solution, which was electrolytically treated to obtain gold mud, wherein the gold recovery rate was 62.25%.

[0050] Example 2

[0051] This embodiment still uses the above-mentioned sulphuric acid slag, with an iron grade of 60.87%. The other main components are shown in Table 1. This is the raw material for the phosphoric acid reduction leaching test. The molar ratio of Fe2O3, phosphoric acid and reducing agent in the sulphuric acid slag is controlled to be 1:10:1.5. The reducing agent is reduced iron powder, the phosphoric acid concentration is 4 mol / L, the liquid-solid ratio is 15 ml / g, and the leaching temperature is controlled at 90°C. After 5 hours of leaching, the iron components in the sulphuric acid slag have basically been converted into soluble ferrous dihydrogen phosphate. The main components of the leached slag are siliceous gangue and insoluble metals such as gold, copper and cobalt, which can be used for subsequent extraction of valuable metals. After solid-liquid separation, a slightly excess of 25% mass concentration hydrogen peroxide is added to the ferrous dihydrogen phosphate solution, and the molar ratio of Fe2O3 to hydrogen peroxide is 1:1.7. The reaction temperature of the hydrogen peroxide oxidation step is controlled to 60°C and stirred for 4 hours until the iron ion content of the supernatant is less than 0.4g / L. After solid-liquid separation, the obtained dihydrated iron phosphate product (( Figure 4 The ferric phosphate product was finally obtained by calcining at 600°C for 2 hours. The chemical composition of the ferric phosphate product is shown in Table 4.

[0052] Table 4 Main chemical components of iron phosphate / %

[0053]

[0054] The leaching residue was mixed with 1 mol / L sulfuric acid at a solid-liquid mass ratio of 1:4 and stirred for 4 hours to obtain a copper-cobalt leaching solution and a gold-containing leaching residue. Sodium thiosulfate with a mass concentration of 10% was added to the leaching solution, and the amount was 2.5 times the concentration of copper ions. Sodium carbonate was used as a pH adjuster, and the pH value of the mixed solution was adjusted to 5. The stirring temperature was 90°C and the stirring time was 3 hours. Finally, copper precipitate residue and cobalt-rich solution were obtained, and the copper recovery rate was 70.68%.

[0055] Sodium carbonate with a mass concentration of 9% was added as a precipitant to the cobalt-rich solution, and the pH value of the solution was adjusted to 9. After stirring at room temperature for 4 hours, solid-liquid separation was performed to obtain cobalt precipitate slag, and the cobalt recovery rate was 61.23%.

[0056] The gold-containing leaching residue was mixed and stirred with 0.4 mol / L sodium thiosulfate solution, with a solid-liquid mass ratio of 1:4, a system pH value of 10.5, a stirring time of 6 hours, and a stirring temperature of 50°C, and then the solid-liquid separation was performed to obtain a gold leaching solution, and the gold leaching solution was adsorbed on activated carbon, with an activated carbon dosage of 10 g / L and a stirring time of 12 hours. The mixed solution was then solid-liquid separated to obtain a gold-loaded carbon solid phase, and then a 5wt% NaCl and 2wt% NaOH mixed desorption solution was used to desorb the gold-loaded carbon, with a desorption solution dosage of 0.05 L / g and a desorption time of 12 hours to obtain a gold-rich solution, which was electrolytically treated to obtain gold mud, wherein the gold recovery rate was 60.17%.

[0057] Example 3

[0058] This embodiment uses sulfuric acid slag from a certain factory with an iron grade of 63.45%. The other main components are shown in Table 5.

[0059] Table 5 Main chemical components of sulfuric acid slag / %

[0060]

[0061] This was used as a raw material for a phosphoric acid reduction leaching test. The molar ratio of Fe2O3, phosphoric acid, and reducing agent in the iron concentrate was controlled to be 1:9:1.5, the reducing agent was reduced iron powder, the phosphoric acid concentration was 6 mol / L, the liquid-solid ratio was 6 ml / g, and the leaching temperature was controlled at 90°C. After 5 hours of leaching, the iron components in the sulfate slag were basically converted into soluble ferrous dihydrogen phosphate, and the main components of the leached slag were siliceous gangue and insoluble metals such as gold, copper, and cobalt, which can be used for subsequent extraction of valuable metals. After solid-liquid separation, air was introduced into the ferrous dihydrogen phosphate solution, and the reaction temperature of the oxidation step was controlled at 70°C, and it was stirred until the iron ion content of the supernatant was less than 0.4 g / L. After solid-liquid separation, the obtained dihydrated iron phosphate product was calcined at 600°C for 2 hours to finally obtain an iron phosphate product. The chemical composition of the iron phosphate product is shown in Table 6.

[0062] Table 6 Main chemical composition of iron phosphate / %

[0063]

[0064] The leaching residue was mixed with 1 mol / L sulfuric acid at a solid-liquid mass ratio of 1:2 and stirred for 3 hours to obtain a copper-cobalt leaching solution and a gold-containing leaching residue. Sodium thiosulfate with a mass concentration of 8% was added to the leaching solution, and the amount was twice the concentration of copper ions. Sodium carbonate was used as a pH adjuster, and the pH value of the mixed solution was adjusted to 5. The stirring temperature was 80°C and the stirring time was 3 hours. Finally, copper precipitate residue and cobalt-rich solution were obtained, and the copper recovery rate was 65.52%.

[0065] 8% mass concentration of sodium carbonate was added as a precipitant to the cobalt-rich solution, and the pH value of the solution was adjusted to 8. After stirring at room temperature for 3 hours, solid-liquid separation was carried out to obtain cobalt precipitate slag, and the cobalt recovery rate was 56.53%.

[0066] The gold-containing leaching residue was mixed and stirred with 25kg / t thiourea solution, with a solid-liquid mass ratio of 1:4, a system pH value of 1.5, a stirring time of 5 hours, and a stirring temperature of 30°C, and then the solid-liquid separation was performed to obtain a gold leaching solution, and the gold leaching solution was adsorbed on activated carbon, with an activated carbon dosage of 15g / L and a stirring time of 24 hours. The mixed solution was then separated from the solid and liquid to obtain a gold-loaded carbon solid phase, and then the gold-loaded carbon was desorbed using a mixed desorption solution of 5% NaCl and 2% NaOH, with a desorption solution dosage of 0.1L / g and a desorption time of 24 hours to obtain a gold-rich solution, which was electrolytically treated to obtain gold mud, wherein the gold recovery rate was 69.42%.

[0067] Comparative Example 1

[0068] This comparative example uses the sulfate slag in Example 1 as a raw material to carry out a phosphoric acid reduction leaching test. The molar ratio of Fe2O3, phosphoric acid, and reducing agent in the sulfate slag is controlled to be 1:8:1, the reducing agent is elemental iron powder, the phosphoric acid concentration is 5 mol / L, the liquid-solid ratio is 8 ml / g, the leaching temperature is controlled at 70°C, and the leaching time is 4 hours. In this comparative example, the molar ratio of Fe2O3 to elemental iron powder in the sulfate slag is 1:1, which is the theoretical ratio. In the actual leaching process, since the elemental iron powder itself will also react with phosphoric acid to generate ferrous dihydrogen phosphate, there is not enough elemental iron to reduce the trivalent iron ions generated by the reaction of Fe2O3 and phosphoric acid, resulting in insufficient reaction of the sulfate slag, and part of the iron remains in the leaching slag ( Figure 5 The chemical composition of the leached residue is shown in Table 7.

[0069] Table 7 Chemical composition analysis of reduction leaching residue / %

[0070]

[0071] After solid-liquid separation, a slightly excess amount of 25% mass concentration hydrogen peroxide was added to the ferrous dihydrogen phosphate solution, wherein the molar ratio of Fe2O3 to H2O2 was 1:1.7; the reaction temperature of the hydrogen peroxide oxidation step was controlled at 60°C and stirred for 3 hours until the iron ion content of the supernatant was less than 0.4 g / L. After solid-liquid separation, the obtained dihydrated iron phosphate product was calcined at 550°C for 2 hours to finally obtain an iron phosphate product, wherein the iron recovery rate was 73.68%; the chemical composition of the iron phosphate product is shown in Table 8.

[0072] Table 8 All element analysis of iron phosphate / %

[0073]

[0074] The leaching residue obtained during phosphoric acid leaching is used to recover gold, copper and cobalt:

[0075] The leaching residue was mixed with 1 mol / L sulfuric acid at a solid-liquid mass ratio of 1:3 for 3 hours to obtain a copper-cobalt leaching solution and a gold-containing leaching residue. Sodium thiosulfate with a mass concentration of 10% was added to the copper-cobalt leaching solution, and the amount was twice the concentration of copper ions. Sodium carbonate was used as a pH adjuster, and the pH value of the mixed solution was adjusted to 5. The stirring temperature was 80°C and the stirring time was 3 hours. Finally, copper precipitate residue and cobalt-rich solution were obtained, and the copper recovery rate was 29.36%.

[0076] 9% mass concentration of sodium carbonate was added as a precipitant to the cobalt-rich solution, and the pH value of the solution was adjusted to 8. After stirring at room temperature for 4 hours, solid-liquid separation was performed to obtain cobalt precipitate slag, and the cobalt recovery rate was 19.63%.

[0077] The gold-containing leaching residue was mixed and stirred with 0.3 mol / L sodium thiosulfate solution, with a solid-liquid mass ratio of 1:4, a system pH value of 10.5, a stirring time of 6 hours, and a stirring temperature of 40°C, and then solid-liquid separation was performed to obtain a gold leaching solution, and the gold leaching solution was adsorbed on activated carbon, with an activated carbon dosage of 10 g / L and a stirring time of 24 hours. The mixed solution was then solid-liquid separated to obtain a gold-loaded carbon solid phase, and then a 5wt% NaCl and 2wt% NaOH mixed desorption solution was used to desorb the gold-loaded carbon, with a desorption solution dosage of 0.05 L / g and a desorption time of 24 hours to obtain a gold-rich solution, which was electrolytically treated to obtain gold mud, wherein the gold recovery rate was 24.65%.

[0078] Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing battery-grade iron phosphate using sulfuric acid slag and recovering gold, copper and cobalt, characterized in that: The sulfuric acid slag is mixed with a phosphoric acid solution and elemental iron for leaching to obtain a ferrous dihydrogen phosphate leaching solution and a leaching slag; an oxidant is added to the ferrous dihydrogen phosphate leaching solution for precipitation reaction to obtain a dihydrate ferric phosphate precipitate and a phosphoric acid solution; the dihydrate ferric phosphate precipitate is calcined to obtain ferric phosphate; the leaching slag is used to recover gold, copper and cobalt.

2. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 1, characterized in that: The molar ratio of Fe2O3 to phosphoric acid and elemental iron in the sulfuric acid slag is 1:6-10:1.5-3.

3. A method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt using sulfuric acid slag according to claim 1 or 2, characterized in that: During the leaching process, the concentration of the phosphoric acid solution is 3-8 mol / L, the liquid-solid ratio is 6-15 ml / g, the temperature is 30-100° C., and the time is 2-6 hours.

4. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 1, characterized in that: The oxidant includes at least one of hydrogen peroxide, air and oxygen.

5. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 1 or 4, characterized in that: The precipitation reaction process is: stirring the reaction at a temperature of 60 to 80° C. for 1 to 3 hours.

6. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 1, characterized in that: The calcination conditions are: temperature of 500-700° C. and time of 60-180 min.

7. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 1, characterized in that: The process of recovering gold, copper and cobalt comprises: leaching the leaching residue with sulfuric acid and then performing solid-liquid separation to obtain a copper-cobalt leaching solution and a gold-containing leaching residue; mixing the copper-cobalt leaching solution with a sodium thiosulfate solution and adjusting the pH to perform a copper precipitation reaction, and then performing solid-liquid separation to obtain a copper slag and a cobalt-containing solution; and leaching the gold-containing leaching residue with a gold leaching agent to obtain a gold-containing leaching solution.

8. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 7, characterized in that: The gold leaching agent includes at least one of cyanide, thiosulfate and thiourea.

9. A method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt using sulfuric acid slag according to claim 7 or 8, characterized in that: The gold-containing leaching solution is adsorbed by activated carbon to obtain gold-loaded carbon, the gold-loaded carbon is desorbed by a desorption solution to obtain a gold-rich solution, and the gold-rich solution is electrolytically treated to obtain gold mud.

10. The method for preparing battery-grade iron phosphate and recovering gold, copper and cobalt by using sulfuric acid slag according to claim 9, characterized in that: The desorption liquid is a mixed solution of sodium chloride and sodium hydroxide.

Citation Information

Patent Citations

  • Method used for producing ferric phosphate from yellow phosphorus by-product phosphor iron slag

    CN108101014A

  • Comprehensive utilization method for low-grade copper-cobalt-containing sulfate slag

    CN109609768A

  • Method for preparing battery-grade iron phosphate by using sulfuric acid residues

    CN110002421A

  • Method for preparing battery-grade iron phosphate by using pyrite cinder

    CN115072687A

  • Method for preparing battery-grade lithium iron phosphate from pyrite cinder

    CN116177515A

Cited By

  • Method for preparing iron phosphate by circulating oxygen oxidation and application

    CN120136054A