Monodisperse nanoscale sodium titanium phosphate material as well as preparation method and application thereof

Through the sol-gel method and sintering process, monodisperse nanoscale sodium titanium phosphate materials are prepared, which solves the problems of large particle size and serious agglomeration in sodium-ion battery cathode materials, improves the ionic conductivity and cycle stability of the material, and simplifies the process and reduce costs.

CN118754084APending Publication Date: 2024-10-11HEFEI GUOXUAN HIGH TECH POWER ENERGY CO LTD CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410943374.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The coating process of sodium fast ion conductors in existing sodium-ion battery cathode materials has problems such as large particle size and serious agglomeration, which affects the ionic conductivity and cycle stability of the material. In addition, the liquid phase method is commonly used to produce waste liquid, which is complex and costly. .

Method used

The sol-gel method is used to prepare nanoscale sodium titanium phosphate materials, which are sintered at high temperature in a protective atmosphere to form a three-dimensional carbon wrapping network to avoid particle agglomeration, and then sintered at low temperature in an oxidizing atmosphere to remove the carbon network to obtain monodispersed nanoscale sodium titanium phosphate. Material.

Benefits of technology

The uniform small particle size and narrow particle size distribution of nanoscale sodium titanium phosphate material are achieved, the ionic conductivity and cycle stability of the material are improved, the process complexity and cost are reduced, and it is suitable for coating of sodium ion battery cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754084A_ABST
    Figure CN118754084A_ABST
Patent Text Reader

Abstract

The invention relates to a monodisperse nanoscale sodium titanium phosphate material and a preparation method and application thereof.The preparation method comprises the following steps that S1, an acid complexing agent is added into water and stirred until the acid complexing agent is completely dissolved, then a titanium source, a phosphorus source, a sodium source and an alcohol solvent are sequentially added, stirring is conducted, pH is adjusted, and lyosol is obtained; s2, the lyosol is dried, and dried gel is obtained; s3, sintering the xerogel for the first time under a protective atmosphere to obtain a carbon-coated nano-scale sodium titanium phosphate material precursor; and S4, carrying out second sintering on the carbon-coated nano-scale sodium titanium phosphate material precursor in an oxidizing atmosphere to obtain the monodisperse nano-scale sodium titanium phosphate material. The sodium titanium phosphate material prepared by the method provided by the invention has a monodisperse small particle size, and solves the problems of large particle size and serious agglomeration of the sodium titanium phosphate material in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium fast ion conductor materials, and in particular to a monodisperse nanometer-level sodium titanium phosphate material and a preparation method and application thereof. Background Art

[0002] By coating the surface of the electrode material and slowing down the side reaction between the electrode material and the electrolyte, the cycle stability of the positive electrode material of the sodium ion battery can be effectively improved. In particular, coating the positive electrode material with a sodium fast ion conductor can further improve the ionic conductivity of the material. At present, the literature generally uses a liquid phase method to coat the positive electrode material of the sodium ion battery with a fast ion conductor, but this will produce a large amount of waste liquid, while affecting the residual alkali of the positive electrode material, which is not convenient for the electrical properties of the positive electrode material. Developing a solid phase method to coat the positive electrode material will be more convenient and feasible, and will be conducive to process scale-up. In the solid phase coating process, the particle size and agglomeration degree of the sodium fast ion conductor will greatly affect the coating effect, which urgently requires the development of a method for preparing monodisperse, small-sized (within 100nm) sodium fast ion conductors.

[0003] NASICON sodium ion conductor NaTi2(PO4)3 has excellent stability, high ionic conductivity (~10 -4 s / cm) is an excellent material for surface coating of positive electrode materials of sodium ion batteries. At present, the conventional methods for synthesizing NaTi2(PO4)3 mainly include: solid phase reaction method and sol-gel method. However, the particle size of NaTi2(PO4)3 prepared by these synthesis methods is usually large (greater than 100nm) and the agglomerates are serious. For example, the patent with publication number CN109205585A provides a method for preparing sodium titanium phosphate, and the prepared sodium titanium phosphate material is a micro-nano material, whose primary particle NTP is 30-800nm, and its secondary particle NTP is 1-3μm, and the size of the synthesized ion is relatively large. For another example, the patent with publication number CN116504954A provides a positive electrode material, a preparation method thereof and a sodium ion battery. By synthesizing porous layered oxides, the contact area with the coating layer is increased and the uniformity of the coating is improved, but the process control is harsh and the preparation cost is high, which is not conducive to the industrialization of low-cost sodium electric materials. For example, the patent with publication number CN115064681B provides a method for preparing a carbon-coated sodium titanium phosphate material. The preparation method can improve the controllability of the carbon-coated sodium titanium phosphate preparation method to a certain extent, but cannot control the distribution morphology of sodium titanium phosphate. As a coating material, the excessive carbon content affects the coating uniformity with the electrode material. Summary of the invention

[0004] Based on this, the purpose of the present invention is to provide a monodisperse nano-scale sodium titanium phosphate material and a preparation method and application thereof, so as to solve the problems of large particle size and serious agglomeration of the sodium titanium phosphate material in the prior art. The preparation method is controllable and easy to adjust and scale up, which greatly avoids the agglomeration and growth of sodium titanium phosphate molecules during the sintering process. The nano-sodium titanium phosphate has high uniformity and a narrow particle size distribution range.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing a monodisperse nanoscale sodium titanium phosphate material, which comprises the following steps:

[0007] S1. The acidic complexing agent is added to water and stirred until completely dissolved, and then a titanium source, a phosphorus source, a sodium source, and an alcohol solvent are added in sequence, stirred and the pH is adjusted to obtain a liquid sol;

[0008] S2. drying the liquid sol to obtain a dry gel;

[0009] S3. The dry gel is first sintered under a protective atmosphere to obtain a carbon-encapsulated nanoscale sodium titanium phosphate material precursor;

[0010] S4. The carbon-wrapped nano-scale sodium titanium phosphate material precursor is subjected to a second sintering in an oxidizing atmosphere to obtain a monodisperse nano-scale sodium titanium phosphate material.

[0011] The preparation method of the invention firstly adopts the sol-gel method to achieve uniform mixing of raw materials at the molecular level to obtain a liquid sol, and then dries it into a dry gel, which can reduce the sodium titanium phosphate phase formation temperature required for the first sintering, reduce the diffusion mass transfer rate between particles, and avoid the growth of sodium titanium phosphate particles; then, the phase is formed by high-temperature sintering in a protective atmosphere, and organic matter is decomposed to form a three-dimensional cross-linked carbon encapsulation network. The formed three-dimensional cross-linked carbon encapsulation network avoids contact between sodium titanium phosphate particles and avoids agglomeration of particles, thereby limiting the growth of sodium titanium phosphate particles; finally, the carbon network is removed by sintering in an oxidizing atmosphere, thereby forming monodisperse nanometer-level sodium titanium phosphate particles. The sodium titanium phosphate material prepared by the method of the invention has a small monodisperse particle size, and solves the problems of large particle size and serious agglomeration of the sodium titanium phosphate material in the prior art.

[0012] As a further improvement of the above solution of the present invention, the average particle size D50 of the monodisperse nano-scale sodium titanium phosphate material is 10-40 nm.

[0013] The sodium titanium phosphate material prepared by the method of the present invention has a small monodisperse particle size, which solves the problem of large particle size and serious agglomeration of the sodium titanium phosphate material in the prior art.

[0014] As a further improvement of the above scheme of the present invention, in step S1, the molar ratio of the sodium source, the titanium source and the phosphorus source is 1:2:3, so that the molar ratio of the sodium source, the titanium source and the phosphorus source conforms to the following chemical formula: NaTi2(PO4)3; which can improve the particle size uniformity of the monodisperse nanoscale sodium titanium phosphate material;

[0015] And / or, in step S1, the sum of the molar numbers of the acidic complexing agent and the alcohol solvent is M1, and the sum of the molar numbers of the metal cations in the liquid sol is M2, M1:M2=(2-8):1; preferably, the molar ratio of the acidic complexing agent to the alcohol solvent is 1:1; more preferably, the mass concentration of the acidic complexing agent aqueous solution is 40-60wt%; in the liquid sol preparation process of the present invention, the acidic complexing agent is ionized and chelated with the metal cations to make the metal cations uniformly dispersed, and finally esterified and cross-linked with alcohols to form a three-dimensional network. The distance between the metal ions and the carbon content in the network can be adjusted by the molar ratio of the sum of the molar numbers of the acidic complexing agent and the alcohol solvent to the metal cations in the liquid sol, and the particle size of the sintered product can be controlled. When sintering under a protective atmosphere, it can further ensure that the organic matter is decomposed to form a three-dimensional carbon-wrapped network, inhibit the growth of sodium titanium phosphate particles, and block the mutual contact between particles;

[0016] And / or, in step S1, adjusting the pH is to add ammonia water to adjust the pH to 6-8; for adjusting the relative speed of hydrolysis and polycondensation.

[0017] As a further improvement of the above scheme of the present invention, in step S1, the sodium source is at least one of sodium carbonate, sodium nitrate, sodium hydroxide and sodium oxide;

[0018] And / or, in step S1, the titanium source is at least one of titanic acid, tetraethyl titanate, tetrabutyl titanate and isopropyl titanate; different titanium sources will form Ti-O compounds and different hydrolysis condensation networks after hydrolysis, and different hydrolysis condensation networks also have the effect of controlling particle size;

[0019] And / or, in step S1, the phosphorus source is at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate; phosphoric acid as the phosphorus source does not contain ammonium ions, and is very easy to absorb water in the air, which will have a certain impact on the subsequent raw material ratio; while diammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate as the phosphorus source, the ammonium ions generated by hydrolysis will subsequently produce ammonium salts or ammonia gas at high temperature, which is more troublesome to handle;

[0020] And / or, in step S1, the acidic complexing agent is at least one of citric acid, malic acid, malonic acid, succinic acid, succinic acid, glycolic acid, aminoacetic acid, lactic acid, tartaric acid and ethylenediaminetetraacetic acid;

[0021] And / or, in step S1, the alcohol solvent is at least one of anhydrous ethanol, ethylene glycol and propylene glycol.

[0022] The carbon-coated network formed by pyrolysis of the acidic complexing agent and the alcohol solvent after esterification has a more significant effect on the refinement of the sodium titanium phosphate particles.

[0023] As a further improvement of the above solution of the present invention, in step S2, the drying is carried out at 80-140° C. for 10-48 hours.

[0024] As a further improvement of the above scheme of the present invention, in step S3, the method of the first sintering is: heating the dry gel to 350-450° C. and sintering for 2-10 hours under a protective atmosphere, and then heating to 650-850° C. and sintering for 2-20 hours;

[0025] And / or, the protective atmosphere is a nitrogen atmosphere, an argon atmosphere or a helium atmosphere.

[0026] As a further improvement of the above solution of the present invention, in step S4, the second sintering method is: heating the carbon-wrapped nano-scale sodium titanium phosphate material precursor to 300-500° C. in an oxidizing gas atmosphere and sintering for 5-72 hours;

[0027] And / or, the oxidizing atmosphere is an air atmosphere, an oxygen atmosphere, or a mixed atmosphere of oxygen and nitrogen.

[0028] In the preparation process of the present invention, one inert gas atmosphere sintering and one oxidative atmosphere sintering are adopted. In the inert atmosphere sintering, the dry gel is first pyrolyzed to form a three-dimensional cross-linked carbon-wrapped network, thereby avoiding contact between sodium titanium phosphate particles and avoiding agglomeration of particles. Subsequently, low-temperature sintering is performed in an oxidative atmosphere to remove the carbon network. Due to the low temperature, mass transfer is difficult to occur between the sodium titanium phosphate particles, thereby avoiding the growth of particles, thereby obtaining a monodisperse nanometer-grade sodium titanium phosphate material. In order to more evenly control the sintering temperature, in a preferred embodiment, in the first sintering, the heating temperature rise rate is 1-4°C / min, and in the second sintering, the heating temperature rise rate is 0.05-2°C / min. The sodium titanium phosphate material prepared under the above conditions has a smaller particle size, a narrower particle size distribution, and fewer agglomerates, and the average particle size D50 of the monodisperse nanometer-grade sodium titanium phosphate material is 10-40nm.

[0029] The present invention provides a monodisperse nano-scale sodium titanium phosphate material, which is prepared by the above-mentioned preparation method.

[0030] The monodisperse nanometer-scale sodium titanium phosphate material provided by the present invention uses the preparation method of the present invention, so the obtained sodium titanium phosphate material has a nanometer-scale particle size, and the average particle size D50 of the monodisperse nanometer-scale sodium titanium phosphate material is 10-40nm.

[0031] The present invention provides an application of the monodisperse nanoscale sodium titanium phosphate material as described above in a sodium ion battery positive electrode composite material.

[0032] As a further improvement of the above scheme of the present invention, the application includes the following steps: stirring and mixing the monodisperse nanoscale sodium titanium phosphate material with the sodium ion battery positive electrode material to obtain a mixture; heating the mixture in an oxygen atmosphere to react to obtain a sodium ion battery positive electrode composite material. Preferably, the sodium ion battery positive electrode material is NaNiFeCuMnTiO2; more preferably, the stirring and mixing time is 10-24h; more preferably, the heating reaction temperature is 400-700℃ and the time is 1-10h. More preferably, in the sodium ion battery positive electrode composite material, the weight ratio of the monodisperse nanoscale sodium titanium phosphate material and the sodium ion battery positive electrode material is (0-0.002):1.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The present invention firstly adopts the sol-gel method to achieve uniform mixing of raw materials at the molecular level to obtain a liquid sol, which is then dried into a dry gel, thereby reducing the sodium titanium phosphate phase formation temperature required for the first sintering, reducing the diffusion mass transfer rate between particles, and avoiding the growth of sodium titanium phosphate particles; then, the phase is formed by high-temperature sintering in a protective atmosphere, and organic matter is decomposed to form a three-dimensional cross-linked carbon encapsulation network. The formed three-dimensional cross-linked carbon encapsulation network avoids contact between sodium titanium phosphate particles and avoids agglomeration of particles, thereby limiting the growth of sodium titanium phosphate particles; finally, the carbon network is removed by sintering in an oxidizing atmosphere, thereby forming monodisperse nanoscale sodium titanium phosphate particles. The sodium titanium phosphate material prepared by the method of the present invention has a small monodisperse particle size, which solves the problem of large particle size and serious agglomeration of the sodium titanium phosphate material in the prior art.

[0035] 2. The preparation method of the present invention adopts a solid-phase sintering synthesis process, which has good repeatability, controllable process and easy adjustment and amplification, which greatly avoids the agglomeration and growth of sodium titanium phosphate molecules during the sintering process. The nano sodium titanium phosphate has high uniformity and a narrow particle size distribution range. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The X-ray diffraction pattern of the monodisperse nano-sized sodium titanium phosphate material prepared in Example 1 of the present invention;

[0037] Figure 2TEM images of the monodisperse nano-sized sodium titanium phosphate material prepared in Example 1 of the present invention at different magnifications;

[0038] Figure 3 This is a particle size distribution bar graph of the monodisperse nanoscale sodium titanium phosphate material prepared in Example 1 of the present invention;

[0039] Figure 4 TEM images of the sodium titanium phosphate material prepared in Comparative Example 1 of the present invention at different magnifications;

[0040] Figure 5 TEM images of the monodisperse nano-sized sodium titanium phosphate material prepared in Example 2 of the present invention at different magnifications;

[0041] Figure 6 This is a particle size distribution bar graph of the monodisperse nanoscale sodium titanium phosphate material prepared in Example 2 of the present invention;

[0042] Figure 7 TEM images of the sodium ion battery cathode composite material prepared in Example 3 of the present invention at different magnifications;

[0043] Figure 8 This is a graph showing the cycling performance results of a button cell of a test example of the present invention at a current density of 0.5C. DETAILED DESCRIPTION

[0044] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0046] Example 1

[0047] This embodiment provides a monodisperse nanoscale sodium titanium phosphate material, the preparation method of which includes the following steps:

[0048] S1. Weigh sodium carbonate, tetrabutyl titanate, and ammonium dihydrogen phosphate according to the molar ratio of Na:Ti:P = 1:2:3; at the same time, weigh citric acid:ethylene glycol:(Na + +Ti 4+ )=1:1:1, weigh citric acid and ethylene glycol;

[0049] S2. The citric acid prepared in step S1 is prepared into a citric acid aqueous solution with a mass concentration of 50wt%, and tetrabutyl titanate is added to the citric acid solution under continuous stirring, followed by continuous stirring for 1h; sodium carbonate and diammonium hydrogen phosphate are added under continuous stirring, followed by continuous stirring for 1h; ethylene glycol is added under continuous stirring, followed by continuous stirring for 1h; and then, aqueous ammonia is added under continuous stirring to adjust the pH to 7 to obtain a neutral liquid sol;

[0050] S3. The neutral liquid sol obtained in step S2 is placed in an oven and dried at 110° C. for 24 h to obtain a dry gel;

[0051] S4. The dry gel obtained in step S3 is first sintered in an air atmosphere, the temperature is increased to 400°C at a heating rate of 2°C / min and sintered for 5h, and then the temperature is increased to 700°C at a heating rate of 1°C / min and sintered for 10h to obtain a carbon-encapsulated nanoscale sodium titanium phosphate material precursor;

[0052] S5. Take 100g of the carbon-encapsulated nanoscale sodium titanium phosphate material precursor obtained in step S4 and perform a second sintering in an oxygen atmosphere. First, heat the temperature to 300℃ at a heating rate of 1℃ / min and pre-sinter for 5h. Then, heat the temperature to 350℃ at a heating rate of 0.1℃ / min and sinter for 10h. Then, heat the temperature to 400℃ at a heating rate of 0.1℃ / min and sinter for 10h. Then, heat the temperature to 450℃ at a heating rate of 0.1℃ / min and sinter for 10h. Then, heat the temperature to 475℃ at a heating rate of 0.1℃ / min and sinter for 10h to obtain a monodisperse nanoscale sodium titanium phosphate material.

[0053] The monodisperse nanoscale sodium titanium phosphate material powder prepared in this example was subjected to an X-ray diffraction test using an X-ray powder diffractometer (SmartLab) from Rigaku Corporation of Japan: a Cu target was used, a target voltage of 40 kV, a target current of 150 mA, Kα radiation, a scanning speed of 3° / min, a scattering slit of 1°, and a receiving slot of 0.15 mm. The XRD image of the monodisperse nanoscale sodium titanium phosphate material prepared in this example is shown in FIG. Figure 1 As shown, from Figure 1 It can be seen that the diffraction peak position of the monodisperse nanoscale sodium titanium phosphate material prepared in this embodiment is consistent with the XRD standard card of sodium titanium phosphate (JCPDS NO.97-008-0426), and the diffraction peak is sharp and has no impurity peaks, indicating that the prepared sodium titanium phosphate has high purity and good crystallinity.

[0054] The morphology of the composite sample was observed using a Japanese Hitachi H7650 transmission electron microscope at a voltage of 100 kV. The TEM image of the monodisperse nanoscale sodium titanium phosphate material prepared in this example is shown in FIG. Figure 2 As shown, from Figure 2It can be seen that the sodium titanium phosphate particles are spherical particles with uniform particle size. The statistical particle size distribution bar graph is as follows Figure 3 As shown, from Figure 3 It can be seen that the average particle size D50 of the sodium titanium phosphate material prepared in this embodiment is 10-15 nm.

[0055] Comparative Example 1

[0056] This comparative example proposes a sodium titanium phosphate material, and its preparation method comprises the following steps:

[0057] S1. Weigh sodium carbonate, tetrabutyl titanate, and ammonium dihydrogen phosphate according to the molar ratio of Na:Ti:P = 1:2:3; at the same time, weigh citric acid:ethylene glycol:(Na + +Ti 4+ )=1:1:1, weigh citric acid and ethylene glycol;

[0058] S2. The citric acid prepared in step S1 is prepared into a citric acid aqueous solution with a mass concentration of 50wt%, and tetrabutyl titanate is added to the citric acid solution under continuous stirring, followed by continuous stirring for 1h; sodium carbonate and diammonium hydrogen phosphate are added under continuous stirring, followed by continuous stirring for 1h; ethylene glycol is added under continuous stirring, followed by continuous stirring for 1h; and then, aqueous ammonia is added under continuous stirring to adjust the pH to 7 to obtain a neutral liquid sol;

[0059] S3. The neutral liquid sol obtained in step S2 is placed in an oven and dried at 110° C. for 24 h to obtain a dry gel;

[0060] S4. The dry gel obtained in step S3 is heated to 700° C. in air at a heating rate of 3° C. / min and sintered for 2 h to obtain sodium titanium phosphate particles.

[0061] The morphology of the sodium titanium phosphate material prepared in this comparative example was observed using a Japanese Hitachi H7650 transmission electron microscope at a voltage of 100 kV. The TEM image of the monodisperse nanoscale sodium titanium phosphate material prepared in this comparative example is shown in FIG. Figure 4 As shown, from Figure 4 It can be seen that the average particle size D50 of the sodium titanium phosphate material prepared in this comparative example is above 100 nm.

[0062] Example 2

[0063] This embodiment provides a monodisperse nanoscale sodium titanium phosphate material, the preparation method of which includes the following steps:

[0064] S1. Weigh sodium carbonate, tetrabutyl titanate, and ammonium dihydrogen phosphate according to the molar ratio of Na:Ti:P = 1:2:3; at the same time, weigh citric acid:ethylene glycol:(Na + +Ti4+ )=1:1:1, weigh citric acid and ethylene glycol;

[0065] S2. The citric acid prepared in step S1 is prepared into a citric acid aqueous solution with a mass concentration of 50wt%, and tetrabutyl titanate is added to the citric acid solution under continuous stirring, followed by continuous stirring for 1h; sodium carbonate and diammonium hydrogen phosphate are added under continuous stirring, followed by continuous stirring for 1h; ethylene glycol is added under continuous stirring, followed by continuous stirring for 1h; and then, aqueous ammonia is added under continuous stirring to adjust the pH to 7 to obtain a neutral liquid sol;

[0066] S3. The neutral liquid sol obtained in step S2 is placed in an oven and dried at 110° C. for 24 h to obtain a dry gel;

[0067] S4. The dry gel obtained in step S3 is first sintered in an air atmosphere, the temperature is increased to 400°C at a heating rate of 2°C / min and sintered for 5h, and then the temperature is increased to 700°C at a heating rate of 1°C / min and sintered for 10h to obtain a carbon-encapsulated nanoscale sodium titanium phosphate material precursor;

[0068] S5. Take 500g of the carbon-encapsulated nanoscale sodium titanium phosphate material precursor obtained in step S4 and perform a second sintering in an oxygen atmosphere. First, heat the temperature to 300℃ at a heating rate of 1℃ / min and pre-sinter for 5h. Then, heat the temperature to 350℃ at a heating rate of 0.3℃ / min and sinter for 10h. Then, heat the temperature to 400℃ at a heating rate of 0.3℃ / min and sinter for 10h. Then, heat the temperature to 450℃ at a heating rate of 0.3℃ / min and sinter for 10h. Then, heat the temperature to 475℃ at a heating rate of 0.3℃ / min and sinter for 10h to obtain a monodisperse nanoscale sodium titanium phosphate material.

[0069] The morphology of the monodisperse nanoscale sodium titanium phosphate material prepared in this embodiment was observed using a Japanese Hitachi H7650 transmission electron microscope, and the observation voltage was 100 kV. The TEM image of the monodisperse nanoscale sodium titanium phosphate material prepared in this embodiment is as follows: Figure 5 The statistical particle size distribution histogram is shown in Figure 6 As shown, from Figure 5 , Figure 6 It can be seen that compared with Example 1, when the amount of sample synthesized by the reaction is enlarged from 100g to 500g, the heating rate increases, and the heat accumulated in the carbon oxidation process is too fast and cannot be released in time, resulting in the sodium titanium phosphate particle size increasing to 30-40nm compared with Example 1, but can still be controlled within 100nm.

[0070] Example 3

[0071] The present embodiment provides a sodium ion battery positive electrode composite material, and the preparation method thereof comprises the following steps: stirring and mixing the sodium titanium phosphate nanoparticles obtained in Example 1 with NaNiFeCuMnTiO2 for 24 hours, and reacting them in an oxygen atmosphere at 600°C for 10 hours to obtain the sodium ion battery positive electrode composite material. In the present embodiment, the coating amount of the sodium titanium phosphate nanoparticles is 0.1% of the mass of the NaNiFeCuMnTiO2 single crystal material.

[0072] The morphology of the sodium ion battery positive electrode composite material prepared in this embodiment was observed using a Japanese Hitachi H7650 transmission electron microscope, and the observation voltage was 100 kV. The TEM image of the sodium ion battery positive electrode composite material prepared in this embodiment is as follows: Figure 7 As shown, from Figure 7 It can be seen that the sodium titanium phosphate particles form a uniform coating layer on the surface of the positive electrode material. This stable fast ion conductor layer avoids direct contact between the positive electrode material and the electrolyte, slows down the side reactions between the positive electrode material and the electrolyte during the charge and discharge cycle, thereby improving the cycle stability of the battery.

[0073] Example 4

[0074] The present embodiment provides a sodium ion battery positive electrode composite material, and the preparation method thereof comprises the following steps: stirring and mixing the sodium titanium phosphate nanoparticles obtained in Example 1 with NaNiFeCuMnTiO2 for 24 hours, and reacting them in an oxygen atmosphere at 600°C for 10 hours to obtain the sodium ion battery positive electrode composite material. In the present embodiment, the coating amount of the sodium titanium phosphate nanoparticles is 0.15% of the mass of the NaNiFeCuMnTiO2 single crystal material.

[0075] Comparative Example 2

[0076] This comparative example provides a sodium ion battery positive electrode composite material, and its preparation method comprises the following steps: reacting NaNiFeCuMnTiO2 of the same mass as that of Example 3 in an oxygen atmosphere at 600°C for 10 hours to obtain a sodium ion battery positive electrode composite material.

[0077] Test Case

[0078] The sodium ion battery positive electrode composite materials prepared in Example 3, Example 4 and Comparative Example 3 were mixed with conductive carbon black and binder PVDF in a mass ratio of 8:1:1, and metal Na was used as the negative electrode and 1.0 mol / L NaClO4 (the solvent was a mixed solvent of EC+DEC with a volume ratio of 1:1) was used as the electrolyte to assemble into CR2016 type button batteries. The cycle stability of the button battery was measured at a current density of 0.5C. The test results are shown in FIG. Figure 8 As shown, from Figure 8It can be seen that after 50 cycles of charge and discharge at a current density of 0.5C, the cycle stability of the sodium ion battery positive electrode material coated with sodium titanium phosphate in Examples 3 and 4 is improved by 4.3%-5.5% compared with that of the sodium titanium phosphate-free positive electrode material in Comparative Example 2.

[0079] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a monodisperse nanoscale sodium titanium phosphate material, characterized in that: It includes the following steps: S1. The acidic complexing agent is added to water and stirred until completely dissolved, and then a titanium source, a phosphorus source, a sodium source, and an alcohol solvent are added in sequence, stirred and the pH is adjusted to obtain a liquid sol; S2. drying the liquid sol to obtain a dry gel; S3. The dry gel is first sintered under a protective atmosphere to obtain a carbon-encapsulated nanoscale sodium titanium phosphate material precursor; S4. The carbon-wrapped nano-scale sodium titanium phosphate material precursor is subjected to a second sintering in an oxidizing atmosphere to obtain a monodisperse nano-scale sodium titanium phosphate material.

2. The method for preparing the monodisperse nanoscale sodium titanium phosphate material according to claim 1, characterized in that: The average particle size D50 of the monodisperse nano-scale sodium titanium phosphate material is 10-40 nm.

3. The method for preparing the monodisperse nanoscale sodium titanium phosphate material according to claim 1, characterized in that: In step S1, the molar ratio of the sodium source, the titanium source and the phosphorus source is 1:2:3; And / or, in step S1, the sum of the moles of the acidic complexing agent and the alcohol solvent is M1, the sum of the moles of the metal cations in the liquid sol is M2, and M1:M2=(2-8):1; And / or, in step S1, adjusting the pH is to add ammonia water to adjust the pH to 6-8.

4. The method for preparing the monodisperse nanoscale sodium titanium phosphate material according to claim 1, characterized in that: In step S1, the sodium source is at least one of sodium carbonate, sodium nitrate, sodium hydroxide and sodium oxide; And / or, in step S1, the titanium source is at least one of titanic acid, tetraethyl titanate, tetrabutyl titanate and isopropyl titanate; and / or, in step S1, the phosphorus source is at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate; And / or, in step S1, the acidic complexing agent is at least one of citric acid, malic acid, malonic acid, succinic acid, succinic acid, glycolic acid, aminoacetic acid, lactic acid, tartaric acid and ethylenediaminetetraacetic acid; And / or, in step S1, the alcohol solvent is at least one of anhydrous ethanol, ethylene glycol and propylene glycol.

5. The method for preparing the monodisperse nanoscale sodium titanium phosphate material according to claim 1, characterized in that: In step S2, the drying is performed at 80-140° C. for 10-48 hours.

6. The method for preparing the monodisperse nanoscale sodium titanium phosphate material according to claim 1, characterized in that: In step S3, the first sintering method is: heating the dry gel to 350-450°C at a heating rate of 1-4°C / min under a protective atmosphere and sintering for 2-10h, and then heating to 650-850°C at a heating rate of 1-4°C / min and sintering for 2-20h; And / or, the protective atmosphere is a nitrogen atmosphere, an argon atmosphere or a helium atmosphere.

7. The method for preparing the monodisperse nanoscale sodium titanium phosphate material according to claim 1, characterized in that: In step S4, the second sintering method is: heating the carbon-wrapped nanoscale sodium titanium phosphate material precursor to 300-500° C. at a heating rate of 0.05-2° C. / min in an oxidizing gas atmosphere and sintering for 5-72 hours; And / or, the oxidizing atmosphere is an air atmosphere, an oxygen atmosphere, or a mixed atmosphere of oxygen and nitrogen.

8. A monodisperse nanoscale sodium titanium phosphate material, characterized in that: The invention is prepared by the preparation method described in any one of claims 1 to 7.

9. Use of the monodisperse nanoscale sodium titanium phosphate material as claimed in claim 8 in a positive electrode composite material for a sodium ion battery.

10. The use of the monodisperse nanoscale sodium titanium phosphate material according to claim 9, characterized in that: The application comprises the following steps: stirring and mixing the monodisperse nano-scale sodium titanium phosphate material and the sodium ion battery positive electrode material to obtain a mixture; heating the mixture in an oxygen atmosphere to react to obtain a sodium ion battery positive electrode composite material.

Citation Information

Patent Citations

  • Nanoscale lithium titanium aluminum phosphate material, and preparation method and application thereof

    CN115403022A