Preparation method of graphene oxide

By applying a constant current through an electrochemical reaction device to separate and intercalate graphite sheets, combined with the chemical oxidation method, the problems of pollution, danger and low yield in the preparation of graphene oxide are solved, and efficient and low-cost preparation of graphene oxide is achieved. , suitable for large-scale production.

CN118754114APending Publication Date: 2024-10-11TSINGHUA SHENZHEN INTERNATIONAL GRADUATE SCHOOL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410980085.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Among the existing methods for preparing graphene oxide, the chemical oxidation method has the problems of high pollution, danger and low yield. The electrochemical method is difficult to achieve large-scale preparation due to insufficient oxidation and reduced conductivity of electrode materials.

Method used

Using an electrochemical reaction device, a constant current is applied through the cathode and anode plates to partially separate and intercalate the graphite flakes. Then, the graphite is oxidized by heating and oxidizing it in a mixed solution containing oxidant and acid, controlling the voltage and the use of intercalation agent. Efficient preparation of alkenes.

Benefits of technology

It achieves efficient, rapid and low-cost preparation of graphene oxide, reduces the amount of oxidant and acid, simplifies the production process, increases output and product purity, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754114A_ABST
    Figure CN118754114A_ABST
Patent Text Reader

Abstract

A preparation method of graphene oxide comprises the steps that an electrochemical reaction device is provided, the electrochemical reaction device comprises a cathode plate, an anode plate and electrolyte, the cathode plate comprises an inert cathode, the anode plate comprises an inert anode and graphite arranged on the surface of the inert anode, and the electrolyte comprises an intercalator; applying a constant current with the current density of 10-100mA / g to the cathode plate and the anode plate, so that the sheet layers of the graphite are at least partially separated, the intercalator enters the space between the at least partially separated sheet layers of the graphite, and the voltage between the cathode plate and the anode plate reaches 2-5V to obtain intercalated graphite; placing the intercalated graphite in a mixed solution containing an oxidizing agent and an acid, adding water into the mixed solution, and heating to oxidize the intercalated graphite; and separating the mixed solution to obtain the graphene oxide. According to the preparation method, the graphite can be fully oxidized under the condition of a small amount of oxidizing agent and acid, the time required by chemical oxidation can be shortened, and a complicated impurity removal procedure can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of graphene preparation, and in particular to a method for preparing graphene oxide with high efficiency. Background Art

[0002] Graphene oxide (GO) is an important graphene-derived material. Since graphene oxide can remain in a peeled state in water in the form of a single atomic layer, it can form a thin film and further be reduced to graphene. It is generally regarded as an important precursor of graphene-based materials. At present, chemical oxidation methods represented by the Hummers method are generally used for mass production of graphene oxide. However, there are still many problems with the commonly used chemical oxidation methods. For example, the use of excessive oxidants and acids to ensure complete oxidation will lead to excessive residual impurities that need to be removed, increase the cost and time in the production process, and bring high pollution and danger. The electrochemical method for preparing graphene oxide is a green and environmentally friendly method that uses electrical energy instead of strong oxidants in chemical oxidation. However, the ordinary electrochemical oxidation method will cause the overall conductivity of the electrode material to decrease due to the generation of graphene oxide during the preparation process. The electrode contact problem cannot be avoided during the large-scale preparation process, which will lead to the problems of insufficient oxidation and low yield of the prepared graphene oxide. Summary of the invention

[0003] In view of this, it is necessary to provide an efficient, fast and low-cost method for preparing graphene oxide to achieve large-scale preparation of graphene oxide.

[0004] An electrochemical reaction device is provided, comprising a cathode plate, an anode plate and an electrolyte, wherein the cathode plate comprises an inert cathode, the anode plate comprises an inert anode and graphite arranged on the surface of the inert anode, and the electrolyte comprises an intercalation agent; a constant current with a current density of 10 to 100 mA / g is applied to the cathode plate and the anode plate to separate the graphite sheets at least partially, the intercalation agent enters between the at least partially separated graphite sheets, and the voltage between the cathode plate and the anode plate reaches 2 to 5 V, thereby obtaining intercalated graphite; the intercalated graphite is placed in a mixed solution containing an oxidant and an acid, water is added to the mixed solution and the mixture is heated to oxidize the intercalated graphite; and the graphene oxide is separated from the mixed solution to obtain the graphene oxide.

[0005] In some possible implementations, the inert cathode is selected from one of a titanium-tantalum-iridium alloy and a tungsten rod, and the inert anode is selected from one of a titanium-tantalum-iridium alloy and a tungsten rod.

[0006] In some possible implementations, "applying a constant current with a current density of 10 to 100 mA / g to the cathode plate and the anode plate to at least partially separate the graphite sheets from each other" includes that under the action of the constant current, the edges of the graphite open, so that the graphite sheets are at least partially separated from each other.

[0007] In some possible implementations, the separation includes adding a hydrogen peroxide solution to the mixed solution for reaction to obtain a dispersion containing graphene oxide, and filtering and centrifuging the dispersion containing graphene oxide to obtain the graphene oxide, wherein the graphene oxide is in powder form.

[0008] In some possible implementations, the graphite is selected from one or more of natural graphite, artificial graphite, and flake graphite powder with a mesh size of 5000 to 50.

[0009] In some possible implementations, the anode plate further includes a polymer fabric, and the polymer fabric wraps the graphite.

[0010] In some possible implementations, the intercalant is selected from one of concentrated sulfuric acid, concentrated nitric acid, perchloric acid, acetic acid, phosphoric acid and hydrochloric acid.

[0011] In some possible implementations, the oxidant is selected from one of potassium permanganate, potassium chlorate, potassium dichromate and concentrated nitric acid, and the acid is selected from one of concentrated sulfuric acid, concentrated nitric acid and fuming nitric acid.

[0012] In some possible implementations, the mass ratio of the oxidant to the intercalated graphite is 0.5:1 to 4:1.

[0013] In some possible implementations, the concentration of the acid is 80% to 98%.

[0014] In the present application, under the action of the intercalation agent and the current, the edges of the graphite sheets are gradually opened, and the intercalation agent molecules are able to enter the graphite layers to form intercalated graphite; in the subsequent chemical oxidation, since the intercalation agent molecules have been inserted into the graphite layers, the graphite can be fully oxidized under the conditions of a relatively small amount of oxidant and acid, which is conducive to shortening the time required for chemical oxidation and avoiding complicated impurity removal procedures. In addition, the present application can increase the preparation yield of intercalated graphite by adjusting the scale of the electrochemical intercalation device by placing the graphite raw material on the surface of the inert anode for electrochemical intercalation reaction. The present application also makes the voltage between the plates during electrochemical intercalation 2 to 5V, so that the graphite reaches a suitable electrochemical intercalation degree, which helps to further reduce the amount of oxidant and acid required for subsequent chemical reactions.

[0015] In addition, the preparation method of the present application is easy to operate, and the electrochemical and chemical oxidation processes can be carried out separately. The intercalated graphite obtained by the electrochemical process can be stored in a sealed environment, and the intercalated graphite can be added as a reactant during chemical oxidation, which can save time and cost. Compared with the traditional method, which requires a complete process from intercalation to oxidation, it is more flexible. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1A This is the X-ray diffraction pattern of the electrochemical intercalated graphite provided in Example 1 of the present application.

[0017] Figure 1B This is the X-ray diffraction pattern of the electrochemical intercalated graphite provided in Example 2 of the present application.

[0018] Figure 1C This is the X-ray diffraction pattern of the electrochemical intercalated graphite provided in Example 3 of the present application.

[0019] Figure 1D This is the X-ray diffraction pattern of the electrochemical intercalated graphite provided in Example 4 of the present application.

[0020] Figure 1E This is the X-ray diffraction pattern of the electrochemical intercalated graphite provided in Example 5 of the present application.

[0021] Figure 2A This is the X-ray diffraction pattern of the powder obtained from the graphene oxide dispersion provided in Example 1 of the present application.

[0022] Figure 2B This is the X-ray diffraction pattern of the powder obtained from the graphene oxide dispersion provided in Example 2 of the present application.

[0023] Figure 2C This is the X-ray diffraction pattern of the powder obtained from the graphene oxide dispersion provided in Example 3 of the present application.

[0024] Figure 2D This is the X-ray diffraction pattern of the powder obtained from the graphene oxide dispersion provided in Example 4 of the present application.

[0025] Figure 2E This is the X-ray diffraction pattern of the powder obtained from the graphene oxide dispersion provided in Example 5 of the present application.

[0026] Figure 3A This is the X-ray photoelectron energy spectrum of the powder obtained from the graphene oxide dispersion provided in Example 1 of the present application.

[0027] Figure 3B This is the X-ray photoelectron energy spectrum of the powder obtained from the graphene oxide dispersion provided in Example 2 of the present application.

[0028] Figure 3CThis is the X-ray photoelectron energy spectrum of the powder obtained from the graphene oxide dispersion provided in Example 3 of the present application.

[0029] Figure 3D This is the X-ray photoelectron energy spectrum of the powder obtained from the graphene oxide dispersion provided in Example 4 of the present application.

[0030] Figure 3E This is the X-ray photoelectron energy spectrum of the powder obtained from the graphene oxide dispersion provided in Example 5 of the present application.

[0031] Figure 4A This is a scanning electron microscope image of the powder obtained from the graphene oxide dispersion provided in Example 1 of the present application.

[0032] Figure 4B This is a scanning electron microscope image of the powder obtained from the graphene oxide dispersion provided in Example 2 of the present application.

[0033] Figure 4C This is a scanning electron microscope image of the powder obtained from the graphene oxide dispersion provided in Example 3 of the present application.

[0034] Figure 5 (a) is the X-ray diffraction pattern of 100 mesh graphite provided in Comparative Example 1 of the present application; Figure 5 (b) is the X-ray diffraction pattern of the powder obtained from the dispersion provided in Comparative Example 1 of the present application.

[0035] Figure 6 (a) is the test result of preparing graphene oxide in Comparative Example 2 of the present application; Figure 6 (b) is the test result of the acid concentration required for preparing graphene oxide in this application using Comparative Example 2 as a control.

[0036] Figure 7 (a) is the test result of preparing graphene oxide in Comparative Example 3 of the present application; Figure 7 (b) is the test result of the acid concentration required for preparing graphene oxide in this application using Comparative Example 3 as a control.

[0037] Figure 8 (a) is the test result of preparing graphene oxide in Comparative Example 4 of the present application; Figure 8 (b) is the test result of the amount of oxidant required for preparing graphene oxide in this application using Comparative Example 4 as a reference.

[0038] Fig. 9 (a) is the test result of preparing graphene oxide in Comparative Example 5 of the present application; Fig. 9 (b) is the test result of the amount of oxidant required for preparing graphene oxide in this application using Comparative Example 5 as a reference. DETAILED DESCRIPTION

[0039] The embodiments of the present invention are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention; it should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present application; in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other; many specific details are explained in the following description to facilitate a full understanding of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0040] An embodiment of the present application provides a method for preparing graphene oxide, the preparation method comprising:

[0041] The first step is to provide an electrochemical reaction device, wherein the electrochemical reaction device comprises a cathode plate, an anode plate and an electrolyte, wherein the cathode plate comprises an inert cathode, the anode plate comprises an inert anode and graphite disposed on the surface of the inert anode, and the electrolyte comprises an intercalant.

[0042] In some embodiments, the inert cathode or the inert anode is selected from one of a titanium-tantalum-iridium alloy and a tungsten rod. This is beneficial to reduce side reactions during the power-on process. When platinum or stainless steel is used as the plate material, it is possible to catalyze and intensify the electrolysis of water to produce hydrogen, intensify side reactions, affect the reaction process, and be detrimental to the electrochemical intercalation process of graphite.

[0043] At the same time, in the related art, the electrochemical oxidation process generally uses processed products such as graphite paper or graphite rods as reaction anodes. Graphite paper and graphite rods are made by chemical and high-temperature expansion and rolling treatment. They have high high-temperature stability and conductivity, and can maintain good electrical contact during the electrochemical reaction. However, the yield of electrochemical oxidation using graphite paper or graphite rods as electrodes is low, usually in the order of hundreds of milligrams. At the same time, since binders and other additives are added to graphite paper and graphite rods during the preparation process, impurities in the raw materials reduce the purity of the product graphene oxide. This application forms an anode by placing graphite on the surface of a titanium tantalum iridium alloy or a tungsten rod. Compared with directly using graphite paper or graphite rods as anodes, it is possible to directly prepare electrochemical intercalated graphite using graphite powder as a raw material, without having to go through the preparation of graphite paper or graphite rods, reducing the cost of raw materials. At the same time, by adjusting the scale of the electrochemical intercalation device, the preparation yield of intercalated graphite can be effectively increased, and the single maximum can reach kilograms, which helps to increase the yield of graphite oxidation. In some embodiments, the graphite powder can be attached to the surface of the inert anode by applying a certain pressure through pressing. Such a setting can enable the graphite powder to maintain good and stable contact during the electrochemical process, and the graphite powder pressed on the surface of the inert anode can fully react during the entire electrochemical process.

[0044] In some embodiments, the graphite is selected from one or more of natural graphite, artificial graphite, and flake graphite powder with a mesh size of 5000 to 50.

[0045] In some embodiments, the anode plate further includes a polymer fabric, wherein the polymer fabric wraps the graphite.

[0046] The polymer fabric may be polypropylene flannel to prevent the powder from detaching from the electrode. When the graphite reaction product needs to be collected, the polypropylene flannel can be removed for collection.

[0047] In some embodiments, the intercalant is selected from one of concentrated sulfuric acid, concentrated nitric acid, perchloric acid, acetic acid, phosphoric acid and hydrochloric acid.

[0048] The present application uses an intercalant as an electrolyte, and the electrolyte can be reused multiple times to reduce the generation of waste liquid.

[0049] The second step: applying a constant current with a current density of 10 to 100 mA / g to the cathode plate and the anode plate, so that the graphite sheets are at least partially separated from each other, the intercalation agent enters between the at least partially separated graphite sheets, and the voltage between the cathode plate and the anode plate reaches 2 to 5 V, thereby obtaining intercalated graphite.

[0050] In some embodiments, "applying a constant current with a current density of 10 to 100 mA / g to the cathode plate and the anode plate to at least partially separate the graphite sheets from each other" includes that under the action of the constant current, the edges of the graphite open, so that the graphite sheets are at least partially separated from each other.

[0051] Graphite is composed of sp 2 The carbon atoms are densely packed and hybridized. Under the action of the electric field, the hydroxide ions generated by the electrolysis of water act as strong nucleophiles to attack the sp atoms at the edges and grain boundaries of graphite. 2 The hybridized carbon atoms cause the hydroxylation of two adjacent carbon atoms, which promotes the interlayer expansion and depolarization of the edge graphite. At the same time, the gas produced by the electrolysis of water further promotes the exfoliation of graphite, prompting the intercalation of electrolyte ions and water molecules to form intercalated graphite.

[0052] In the process of preparing graphene oxide by a single electrochemical method, graphite is converted into graphene oxide under the action of electric current. After reaching a certain reaction stage, the conductivity will begin to decrease, affecting the electrode contact, and the reaction becomes unstable, which makes it difficult for graphite to be fully oxidized. In the electrochemical process of the present application, the cathode plate and the anode plate are energized, and under the action of a constant current, a relatively low initial voltage (such as less than 1V) is generated between the plates. As the electrochemical intercalation reaction proceeds, the voltage between the plates increases during the process of graphite being converted into the intercalated graphite. The present application infers the extent of the electrochemical intercalation reaction based on the real-time voltage, and finds that when the voltage between the plates reaches 2 to 5V, that is, the electrochemical intercalation reaction is terminated within the voltage range, it is beneficial to control the current and the intercalation agent to achieve a suitable degree of exfoliation of the graphite, thereby further reducing the acid concentration and the amount of oxidant required in the subsequent chemical oxidation treatment. Specifically, by taking intercalated graphite when the voltage between the plates is 2 to 5 V as a reactant for chemical oxidation, the obtained graphene oxide can reach an oxidation degree equivalent to or even higher than that under lower voltage conditions by using a lower concentration of acid or less oxidant.

[0053] It should also be noted that, in the electrochemical intercalation reaction completed by applying a constant voltage and controlling the power-on time, during the electrochemical intercalation reaction, as the graphite is transformed, the resistance increases, and under constant voltage, the current decreases, and at this time, the energy required for the graphite to continue to transform is higher, so the decreasing current is not conducive to maintaining the stability of the electrochemical intercalation process. It is also difficult to infer the degree of graphite intercalation through such conditional control, and there is a potential risk of excessive power-on and waste of energy. In comparison, the present application focuses more on controlling the degree of electrochemical intercalation of graphite, and since the electrochemical intercalation reaction is carried out under the action of current, applying a constant current and using real-time voltage to infer the degree of electrochemical intercalation reaction can more accurately judge the actual state of graphite intercalation.

[0054] Step 3: placing the intercalated graphite in a mixed solution containing an oxidant and an acid, adding water to the mixed solution and heating the mixed solution to oxidize the intercalated graphite.

[0055] Because the distance between graphite layers is enlarged under the action of electric field and intercalant in advance, electrostatic effect is generated between the internal intercalant and oxidant, which is conducive to accelerating the entry of oxidant into graphite interlayers. Under the action of water and high temperature, the graphene sheets are evenly loaded with oxygen-containing functional groups, so that the intercalated graphite can be oxidized more rapidly to obtain fully and evenly oxidized graphene oxide. By improving the reaction efficiency and shortening the reaction process, the amount of oxidant and acid is saved. Compared with the preparation of graphene oxide by single chemical oxidation, the preparation method of the present application can save about half of the amount of oxidant and acid, reducing the preparation cost and the difficulty of impurity removal.

[0056] In some embodiments, the oxidant is selected from one of potassium permanganate, potassium chlorate, potassium dichromate and concentrated nitric acid, and the acid is selected from one of concentrated sulfuric acid, concentrated nitric acid and fuming nitric acid.

[0057] In some embodiments, the mass ratio of the oxidant to the intercalated graphite is 0.5:1 to 4:1.

[0058] Such a setting is conducive to the full oxidation of intercalated graphite to form graphene oxide, avoiding excessive oxidant and waste of preparation. In the preparation of graphene oxide by a single chemical oxidation method, it is generally necessary to set at least 4 times the mass of graphite in potassium permanganate to ensure full oxidation of graphite. This application is conducive to saving the amount of oxidant on the basis of pre-intercalation. Furthermore, this application also controls the intercalation conditions to facilitate the full oxidation of graphene under the action of a smaller amount of oxidant.

[0059] In some embodiments, the acid concentration is 80% to 98%.

[0060] During the chemical oxidation of graphite, the acid provides an acidic environment to maintain the intercalated graphite structure. In order to fully oxidize the graphite, the present application utilizes pre-intercalated graphite, eliminating the intercalation step in the original oxidation process, thereby reducing the volume of sulfuric acid used in the reaction process. The present application also controls the intercalation conditions, which is conducive to the preparation of fully oxidized graphene oxide in a lower concentration acid environment, thereby reducing the concentration and amount of the required acid and avoiding excessive acid and waste of preparation.

[0061] In some embodiments, the oxidant is mixed with the acid at 0-10°C to obtain the mixed solution, the intercalated graphite is placed before the mixed solution, and the preparation method further includes: adjusting the temperature of the mixed solution to 10-40°C.

[0062] Presetting the temperature range of the mixed solution is beneficial to promoting the diffusion of the oxidant in the mixed solution between graphite layers, thereby facilitating the full chemical oxidation.

[0063] Step 4: Separating the graphene oxide from the mixed solution.

[0064] In some embodiments, the separation includes adding a hydrogen peroxide solution to the mixed solution, terminating the reaction to obtain a dispersion containing graphene oxide, and filtering and centrifuging the dispersion containing graphene oxide to obtain the graphene oxide, wherein the graphene oxide is in powder form.

[0065] The purpose of adding hydrogen peroxide is to react with the remaining potassium permanganate in the reaction system to terminate the chemical oxidation reaction and facilitate the separation of graphene oxide products.

[0066] This application uses graphite powder as raw material, and graphite is sequentially treated with electrochemical intercalation and chemical oxidation. Electrochemical intercalation uses graphite as the anode material, and the cathode uses an inert electrode. Under the action of current and intercalation agent, the edges of the graphite sheets are gradually opened, and the intercalation agent molecules are able to enter the graphite interlayers to form intercalated graphite. In chemical oxidation, since the intercalation agent molecules are already inserted between the graphite layers, only a small amount of oxidant and acid is required to achieve full oxidation of the product. This method can effectively reduce the amount of oxidant and acid used in the preparation process of graphene oxide, and the acid of electrochemical intercalation can be recycled, effectively reducing production costs and improving the safety of the reaction process, and can be used for large-scale production of graphene oxide.

[0067] The scheme of the present invention will be explained below in conjunction with the embodiments. Those skilled in the art will understand that the following examples are only used to explain the present invention and cannot be understood as limiting the present invention. Unless otherwise stated, the reagents, software and instruments not specifically stated in the following embodiments are all conventional commercial products or open source.

[0068] Embodiment 1:

[0069] The 100-mesh natural graphite is used as the raw material, the electrochemical intercalation process uses titanium-tantalum-iridium alloy as the anode inert electrode, polypropylene flannel as the polymer fabric, 98% concentrated sulfuric acid as the intercalation agent, and titanium-iridium-tantalum alloy as the cathode inert electrode. The oxidation process uses potassium permanganate as the oxidant and 98% concentrated sulfuric acid as the acid.

[0070] The first step: take 6g of 100-mesh natural graphite powder and press it on a titanium-tantalum-iridium alloy plate at a pressure of 20MPa. Put the plate into a polypropylene flannel to prevent the powder from detaching from the electrode. Place the prepared anode electrode and the titanium-tantalum-iridium inert cathode in 60mL of 98% sulfuric acid intercalation agent. Pass a constant current of 10mA / g through the electrode to make the voltage reach 3V to obtain electrochemical intercalation graphite, and the electrochemical intercalation sulfuric acid can be recycled.

[0071] Step 2: Add 72 mL of 98% concentrated sulfuric acid into a 500 mL beaker, add 12 g of potassium permanganate into 72 mL of 98% concentrated sulfuric acid in a 10°C water bath, raise the temperature to 35°C, and then place the first-order intercalated graphite obtained by electrochemical intercalation into the reaction system.

[0072] Step 3: After reacting for 1 hour, add 56 mL of deionized water to the system and heat to 98 °C for 20 minutes.

[0073] Step 4: Add 50 mL of dilute hydrogen peroxide solution into the beaker to terminate the reaction and obtain a dispersion containing graphene oxide.

[0074] Example 2: The difference from Example 1 is that the 100-mesh natural graphite is replaced with 325-mesh natural graphite, and the pressure in the first step is adjusted to 30 MPa.

[0075] Embodiment 3:

[0076] The difference from Example 1 is that the 100-mesh natural graphite is replaced with 50-mesh natural graphite, and the pressure in the first step is adjusted to 10 MPa.

[0077] Embodiment 4:

[0078] The difference from Example 1 is that in the first step, when the voltage reaches 2V, electrochemical intercalated graphite is obtained.

[0079] Embodiment 5:

[0080] The difference from Example 1 is that in the first step, when the voltage reaches 4 V, electrochemical intercalated graphite is obtained.

[0081] Comparative Example 1:

[0082] The difference from the first embodiment is that in the first step, no power is supplied.

[0083] The present application removes the electrochemical intercalated graphite obtained in the first step of Examples 1-5 from the anode and performs X-ray diffraction characterization on each of them. Figures 1A to 1E The spectrum shows that the electrochemical intercalation graphites of Examples 1-3 and Example 5 have the strongest diffraction peak near 2θ=22.3°, corresponding to the first-order intercalation graphite, and the electrochemical intercalation graphite of Example 4 has the strongest diffraction peak near 2θ=23.9°, corresponding to the second-order intercalation graphite.

[0084] It should be noted that, because graphite has a layered structure and the interlayer force is the van der Waals force, certain molecules and ions can be inserted into the graphite layers to form graphite intercalation compounds. The order of graphite intercalation compounds is defined as the number of graphene layers between two layers of intercalated molecules. The lower the number of intercalation layers, the higher the degree of intercalation. In the electrochemical intercalation process, the higher the degree of graphite intercalation, the higher the corresponding voltage may be. Therefore, the degree of reaction can be inferred based on the real-time voltage, and graphite intercalation compounds of different orders can be obtained by stopping the reaction at a specified voltage.

[0085] The present application respectively carries out X-ray diffraction characterization on the graphene oxide dispersion obtained in the fourth step of Examples 1-5 after filtration, centrifugation and dispersion and exfoliation of the powder, see FIG. 2A to FIG. 2EThe spectra show that the strongest diffraction peaks appear near 2θ=12.4° in Examples 1 and 4-5, and the strongest diffraction peaks appear near 2θ=12.5° in Examples 2-3, respectively, which correspond to the characteristic peaks of the graphene oxide (001) crystal plane, indicating that the components of the powders obtained after the treatment of the graphene oxide dispersion obtained in Examples 1-5 are mainly graphene oxide.

[0086] Furthermore, the present application performed X-ray photoelectron spectroscopy (XPS) characterization on the powders obtained in Examples 1-5, respectively. Figure 3E The graph shows that the carbon-oxygen ratios of the graphene oxides of Examples 1-5 are 2.1, 2.0, 2.2, 2.4 and 2.1, respectively, indicating that the oxidation degree of the graphene oxide in the graphene oxide dispersion obtained by the preparation method of the present application is high and fully oxidized.

[0087] The present application also uses Examples 1-3 as an example to analyze the obtained powder using a scanning electron microscope. FIG. 4A to FIG. 4C The graph shows that the monolayer rate of the powder of Example 1 exceeds 80%, the flake diameter distribution is 1-5 μm, and the flake thickness ranges from 0.9 to 1.8 nm. The monolayer rate of the powder of Example 2 exceeds 80%, the flake diameter distribution is <1 μm, and the flake thickness ranges from 0.9 to 1.6 nm. The monolayer rate of the powder of Example 3 exceeds 70%, the flake diameter distribution is 1-5 μm, and the flake thickness ranges from 1 to 2 nm. This indicates that the graphene oxide in the graphene oxide dispersion obtained by the preparation method of the present application has a high monolayer rate, uniform flake diameter distribution and uniform flake thickness.

[0088] The present application conducted X-ray diffraction characterization on the 100-mesh graphite that was not subjected to electrical treatment in Comparative Example 1. Figure 5 In (a), the spectrum shows that the strongest diffraction peak appears near 2θ=26.5°, corresponding to the characteristic peak of the graphite (002) crystal plane. The present application further performs the same filtration, centrifugation and dispersion stripping treatment steps as in Examples 1-5 on the dispersion prepared in Comparative Example 1 to obtain a powder, and performs X-ray diffraction characterization on the powder, please refer to Figure 5 In (b), the spectrum shows that strong diffraction peaks appear near 2θ=12.5° and 2θ=26.3°, indicating that there is still a large amount of unoxidized graphite in the product of Comparative Example 1 and the overall oxidation degree is low.

[0089] Table 1. Preparation conditions and step-by-step product characterization results of Examples 1-5 and Comparative Example 1 of the present application

[0090]

[0091] Comparing Examples 1-5 of the present application with Comparative Example 1, it can be shown that compared with a simple chemical oxidation method, the present application performs two-step treatment of graphite, namely electrochemical intercalation and chemical oxidation, in sequence. Under the action of electric current and intercalation agent, the edges of graphite sheets are gradually opened, and intercalation agent molecules are able to enter between graphite layers to form intercalated graphite. In chemical oxidation, since intercalation agent molecules are already inserted between graphite layers, the efficiency of graphite oxidation is significantly improved.

[0092] Comparative Example 2:

[0093] The difference from Example 1 is that in the first step, when the voltage reaches 1.5 V, electrochemical intercalated graphite is obtained; the powder treated with the obtained graphene oxide dispersion is characterized by X-ray photoelectron spectroscopy, and the carbon-oxygen ratio of the graphene oxide is 2.5.

[0094] Comparative Example 3:

[0095] The difference from Comparative Example 2 is that in the second step, the amount of the oxidant potassium permanganate is adjusted to 6 g, that is, the mass ratio of graphite to the oxidant is adjusted from 1:2 to 1:1; the powder treated with the obtained graphene oxide dispersion is characterized by X-ray photoelectron spectroscopy, and the carbon-oxygen ratio of the graphene oxide is 4.0.

[0096] Comparative Example 4:

[0097] The difference from Comparative Example 2 is that in the second step, 98% concentrated sulfuric acid is adjusted to 80% concentrated sulfuric acid; the powder treated with the obtained graphene oxide dispersion is characterized by X-ray photoelectron spectroscopy, and the carbon-oxygen ratio of the graphene oxide is 4.0.

[0098] Comparative Example 5:

[0099] The difference from Comparative Example 2 is that, in the second step, 98% concentrated sulfuric acid is adjusted to 80% concentrated sulfuric acid, and the amount of the oxidant potassium permanganate is adjusted to 9 g, that is, the mass ratio of graphite to the oxidant is adjusted from 1:2 to 1:1.5; the powder treated with the obtained graphene oxide dispersion is characterized by X-ray photoelectron spectroscopy, and the carbon-oxygen ratio of the graphene oxide is 4.4.

[0100] Table 2. Preparation conditions of comparative examples 2-5 of the present application and X-ray photoelectron spectroscopy characterization results of the prepared products

[0101]

[0102] It should be noted that, in the preparation process of the present application, the electrochemical intercalated graphite obtained by making the voltage reach 1.5V corresponds to the third-order intercalated graphite.

[0103] This application uses Comparative Example 2 (the concentration of concentrated sulfuric acid is 98%, the carbon-oxygen ratio of graphene oxide is 2.5, please refer to Figure 6(a)) is used as a control. After the voltage of the electrochemical intercalated graphite is increased from 1.5V in Comparative Example 2 to 3V, the same amount of oxidant potassium permanganate as in Comparative Example 2 is used to prepare graphene oxide. Please refer to Figure 6 (b), the present application found that when the concentration of concentrated sulfuric acid is about 80%, the obtained graphene oxide can reach an oxidation degree equivalent to or even higher than that of Comparative Example 2 (such as a carbon-oxygen ratio of 2.4).

[0104] This application is based on Comparative Example 3 (the concentration of concentrated sulfuric acid is 98%, the carbon-oxygen ratio is 4.0, please refer to Figure 7 (a)) is used as a control, and the voltage when obtaining electrochemical intercalated graphite is increased from 1.5V in Comparative Example 3 to 3V, and the same amount of oxidant potassium permanganate as in Comparative Example 3 is used to prepare graphene oxide, see Figure 7 (b), the present application found that when the concentration of concentrated sulfuric acid is about 80%, the obtained graphene oxide can reach an oxidation degree equivalent to or even higher than that of Comparative Example 3 (such as a carbon-oxygen ratio of 3.9).

[0105] The above results show that on the basis of preparing graphene oxide by sequentially treating graphite with electrochemical intercalation and chemical oxidation, by making the electrochemical intercalation voltage 2-5V, it is beneficial to further reduce the concentration of acid required in the subsequent chemical oxidation treatment.

[0106] The present application also uses Comparative Example 4 (the mass ratio of graphite to oxidant is 1:2, and the carbon-oxygen ratio is 4.0, see Figure 8 (a)) is used as a control, and the voltage when obtaining electrochemical intercalated graphite is increased from 1.5V in Comparative Example 4 to 3V and 2V, and then the same concentration of concentrated sulfuric acid as in Comparative Example 4 is used to prepare graphene oxide, see Figure 8 (b), the present application found that when the graphene oxide obtained under this voltage condition reaches an oxidation degree equivalent to or even higher than that of Comparative Example 4 (such as a carbon-oxygen ratio of 3.6 or 3.8), the amount of oxidant required is significantly less than that of Comparative Example 4.

[0107] The present application also uses Comparative Example 5 (the mass ratio of graphite to oxidant is 1:1.5, and the carbon-oxygen ratio is 4.4, see Fig. 9 (a)) is used as a control. After the voltage when obtaining electrochemical intercalated graphite is increased from 1.5V in Comparative Example 5 to 3V, the same concentration of concentrated sulfuric acid as in Comparative Example 5 is used to prepare graphene oxide. Please refer to Fig. 9 (b), the present application found that when the graphene oxide obtained under this voltage condition reaches an oxidation degree equivalent to or even higher than that of Comparative Example 5 (such as a carbon-oxygen ratio of 3.9), the amount of oxidant required is significantly less than that of Comparative Example 5.

[0108] The above results further indicate that on the basis of preparing graphene oxide by sequentially subjecting graphite to electrochemical intercalation and chemical oxidation, by setting the electrochemical intercalation voltage to 2-5 V, it is beneficial to further reduce the amount of oxidant required in the subsequent chemical oxidation treatment.

[0109] In summary, the graphene oxide preparation method of the present application is conducive to further saving the amount of oxidation reaction preparation, significantly saving preparation costs, shortening the time required for chemical oxidation and avoiding complicated impurity removal processes.

[0110] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.

Claims

1. A method for preparing graphene oxide, It is characterized in that The preparation method comprises: An electrochemical reaction device is provided, the electrochemical reaction device comprising a cathode plate, an anode plate and an electrolyte, the cathode plate comprising an inert cathode, the anode plate comprising an inert anode and graphite disposed on the surface of the inert anode, and the electrolyte comprising an intercalant; Applying a constant current with a current density of 10 to 100 mA / g to the cathode plate and the anode plate, so that the graphite sheets are at least partially separated from each other, the intercalation agent enters between the at least partially separated graphite sheets, and the voltage between the cathode plate and the anode plate reaches 2 to 5 V, thereby obtaining intercalated graphite; placing the intercalated graphite in a mixed solution containing an oxidant and an acid, adding water to the mixed solution and heating the mixed solution to oxidize the intercalated graphite; The graphene oxide is separated from the mixed solution.

2. The preparation method according to claim 1, It is characterized in that The inert cathode is selected from one of a titanium-tantalum-iridium alloy and a tungsten rod, and the inert anode is selected from one of a titanium-tantalum-iridium alloy and a tungsten rod.

3. The preparation method according to claim 1, It is characterized in that "Applying a constant current with a current density of 10 to 100 mA / g to the cathode plate and the anode plate so that the graphite sheets are at least partially separated from each other" includes that under the action of the constant current, the edges of the graphite are opened so that the graphite sheets are at least partially separated from each other.

4. The preparation method according to claim 1, It is characterized in that The separation comprises adding a hydrogen peroxide solution to the mixed solution for reaction to obtain a dispersion containing graphene oxide, and filtering and centrifuging the dispersion containing graphene oxide to obtain the graphene oxide, wherein the graphene oxide is in powder form.

5. The preparation method according to claim 1, It is characterized in that The graphite is selected from one or more of natural graphite, artificial graphite and flake graphite powder with a mesh size of 5000 to 50.

6. The preparation method according to claim 1, It is characterized in that The anode plate further includes a polymer fabric that wraps the graphite.

7. The preparation method according to claim 1, It is characterized in that The intercalant is selected from one of concentrated sulfuric acid, concentrated nitric acid, perchloric acid, acetic acid, phosphoric acid and hydrochloric acid.

8. The preparation method according to claim 1, It is characterized in that The oxidant is selected from one of potassium permanganate, potassium chlorate, potassium dichromate and concentrated nitric acid, and the acid is selected from one of concentrated sulfuric acid, concentrated nitric acid and fuming nitric acid.

9. The preparation method according to claim 1, It is characterized in that The mass ratio of the oxidant to the intercalated graphite is 0.5:1 to 4:

1.

10. The preparation method according to claim 1, It is characterized in that The concentration of the acid is 80% to 98%.

Citation Information

Patent Citations

  • Electrochemically assisted method for preparing monolayer large-size graphene oxide

    CN104108711A

  • Preparation method of large-dimension graphene oxide and large-dimension graphene oxide obtained by method

    CN109534335A

  • Method for preparing graphene oxide by electrolyzing muddy graphite intercalation compound

    CN113816368A

  • Method for preparing graphene oxide through controllable electrolysis by adjusting pressure

    CN115216786A

  • Method for preparing graphene oxide

    CN117699790A