Modified silica fume and application thereof

Through the preheating, high-temperature carbonization and cooling treatment of microsilica powder, its resistivity is significantly improved, which solves the problems of current leakage and temperature unevenness in the graphitization furnace caused by traditional microsilica powder, and improves the operating efficiency and safety of the equipment.

CN118754128APending Publication Date: 2024-10-11CHONGQING EASTSTAR HIGH TEMPERATURE MATERIAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410933020.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The resistivity of traditional microsilica powder is too low, resulting in low operating efficiency, poor safety and short service life of the graphitization furnace, and there are problems such as current leakage and temperature unevenness.

Method used

Through preheating, high-temperature carbonization and cooling, modified microsilica powder with significantly increased resistivity is prepared. The specific steps include preheating at 200℃-700℃ for 6h-18h, and high-temperature carbonization at 700℃

Benefits of technology

The resistivity of the modified microsilica powder increased by approximately 52.1%, effectively reducing current leakage, improving temperature uniformity, and increasing the safety and service life of the graphitization furnace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754128A_ABST
    Figure CN118754128A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of micro-silicon powder processing, and particularly relates to modified micro-silicon powder and application thereof. The preparation method of the modified micro-silicon powder comprises the following steps: treating micro-silicon powder under a preheating condition to obtain preheated micro-silicon powder, treating the preheated micro-silicon powder under a high-temperature carbonization condition to obtain high-temperature carbonized micro-silicon powder, and cooling the high-temperature carbonized micro-silicon powder under a cooling treatment condition to obtain the modified micro-silicon powder. The resistivity of the modified micro-silicon powder can be increased by about 52.1% compared with that of unmodified micro-silicon powder, and when the modified micro-silicon powder serves as a furnace bottom material of a graphitization furnace, the situation of current leakage of the unmodified micro-silicon powder graphitization furnace can be effectively reduced, the situation of uneven temperature is improved, safety is improved, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microsilica powder processing, and specifically relates to modified microsilica powder and application thereof. Background Art

[0002] Graphitization furnace is a key equipment used to graphitize materials with high carbon content (such as coke or carbon black) at high temperature, and is a common equipment in the current industrial field. However, the operating efficiency and safety of the graphitization furnace will be affected by the performance of the furnace bottom material, especially the resistivity of the microsilicon powder in the furnace bottom material.

[0003] The resistivity of the existing furnace bottom material is low, resulting in a low resistivity of the overall furnace bottom material. The low resistivity of the furnace bottom material will cause the following problems: (1) Current leakage is prone to occur during operation (graphitization furnaces usually use electric current for heating during the heating process. If the resistance of the furnace bottom material is too low, it may cause current leakage into the furnace bottom material), which not only leads to energy waste, but also poses a great hidden danger to the stable operation of the furnace and the safety of operators; (2) The low resistivity of the microsilicon powder will cause the current to flow unevenly in the microsilicon powder, resulting in uneven temperature distribution inside the graphitization furnace and unstable temperature inside the furnace, which will have an adverse effect on the quality of graphitization treatment, especially when processing materials with high precision or high performance requirements. This temperature non-uniformity has become a problem that cannot be ignored; in addition, the temperature non-uniformity also significantly increases the safety risk of the graphitization furnace; (3) The aging and damage of the internal materials of the furnace caused by current leakage and temperature non-uniformity increase the maintenance cost of the furnace and shorten its service life.

[0004] In summary, the shortcomings of traditional microsilica powder materials in terms of resistivity have seriously restricted the performance and use effect of graphitization furnaces. Therefore, developing a new material that can significantly improve the resistivity of microsilica powder is of great significance for improving the operating efficiency, safety and service life of graphitization furnaces. Summary of the invention

[0005] In order to achieve the above object, the present invention can adopt the following technical solutions:

[0006] On the one hand, the present invention provides a modified microsilica powder, and its preparation method comprises: (1) preheating treatment: treating the microsilica powder under preheating conditions to obtain preheated microsilica powder, and the preheating conditions include: gradually increasing heating for 6h-18h in a temperature environment of 200℃-700℃; (2) high-temperature carbonization treatment: treating the preheated microsilica powder under high-temperature carbonization conditions to obtain high-temperature carbonized microsilica powder, and the high-temperature carbonization conditions include: first gradually increasing heating for 7h-21h in a temperature environment of 700℃<temperature≤1250℃; and then decreasing heating for 4h-12h in a temperature environment of 1200℃ to 1000℃; (3) cooling treatment: cooling the high-temperature carbonized microsilica powder under cooling treatment conditions to obtain modified microsilica powder, and the cooling treatment conditions include: decreasing cooling for 6h-18h in a temperature environment of 900℃ to 100℃.

[0007] Another aspect of the present invention provides a graphitization furnace bottom material, which includes the modified microsilica powder of the present invention.

[0008] Another aspect of the present invention provides an application of the modified microsilica powder in the present invention in improving the refractory performance of a graphitization furnace.

[0009] Preferably, the above-mentioned application may include one of the following applications: (a) application of modified microsilica powder as furnace bottom material in improving the refractory performance of graphitization furnace; (b) application of furnace bottom material prepared with modified microsilica powder as one of the raw materials in improving the refractory performance of graphitization furnace.

[0010] The beneficial effects of the present invention include at least: the resistivity of the modified microsilica powder provided by the present invention can reach 6710uΩ·m, which is about 52.1% higher than that of the unmodified microsilica powder (4413uΩ·m). Compared with the unmodified microsilica powder as the bottom material of the graphitization furnace, the modified microsilica powder can be used as the bottom material of the graphitization furnace, which can effectively reduce the current leakage of the unmodified microsilica powder graphitization furnace, improve the temperature unevenness, and improve the safety and increase the service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a plan view of the kiln car of the carbonization tunnel kiln in the present invention, wherein A1 is kiln body 1; A2 is kiln body 2; A3 is kiln body 3; A4 is kiln body 4; A5 is kiln body 5; A6 is kiln body 6; A7 is kiln body 7; A8 is kiln body 8;

[0012] Figure 2 This is a physical picture of the microsilica powder in the present invention. DETAILED DESCRIPTION

[0013] The examples are provided to better illustrate the present invention, but the present invention is not limited to the examples. Therefore, those skilled in the art may make non-essential improvements and adjustments to the implementation scheme according to the above invention content, which still fall within the protection scope of the present invention.

[0014] The terms used herein are only used to describe specific embodiments and are not intended to limit the present disclosure. Unless the context has a significantly different meaning, expressions in the singular include expressions in the plural. As used herein, it should be understood that terms such as "include", "have", "include" are intended to indicate the presence of features, numbers, operations, materials, or combinations. The terms of the present invention are disclosed in the specification, and are not intended to exclude the possibility that one or more other features, numbers, operations, materials, or combinations thereof may exist or may be added. As used herein, " / " may be interpreted as "and" or "or", depending on the circumstances.

[0015] The embodiment of the present invention provides a modified microsilica powder, and the preparation method thereof comprises: (1) preheating treatment: treating the microsilica powder under preheating conditions to obtain preheated microsilica powder, the preheating conditions comprising: gradually increasing heating for 6h-18h in a temperature environment of 200℃-700℃; (2) high-temperature carbonization treatment: treating the preheated microsilica powder under high-temperature carbonization conditions to obtain high-temperature carbonized microsilica powder, the high-temperature carbonization conditions comprising: first gradually increasing heating for 7h-21h in a temperature environment of 700℃<temperature≤1250℃; then decreasing heating for 4h-12h in a temperature environment of 1200℃ to 1000℃; (3) cooling treatment: cooling the high-temperature carbonized microsilica powder under cooling treatment conditions to obtain modified microsilica powder, the cooling treatment conditions comprising: gradually cooling for 6h-18h in a temperature environment of 900℃ to 100℃.

[0016] Microsilica fume is also known as silica fume or condensed silica fume. The dust collected from the flue gas of electric furnace by bag filter in the production of industrial silicon and ferrosilicon is generally called microsilica fume, also known as silica fume. Its particle size is extremely fine, and its composition is mainly silicon dioxide. It has low density, high specific resistance, strong cohesion, strong adhesion, and is not easy to settle. With the increase of industrial silicon and ferrosilicon production, the amount of microsilica fume generated is also increasing.

[0017] Microsilica fume is a smoky gray ultrafine powder. With the change of carbon content, the color changes slightly. The whiteness is 40-50 and the capacity is about 200kg / m 3 , true density 2.2g / cm 3 Most of the microsilica particles are smaller than 1μm, with the finest being 0.01μm. The specific surface area measured by nitrogen adsorption method is 26-36m 2 / g, its fineness and specific surface area are about 80-100 times that of cement and 50-70 times that of fly ash.

[0018] During the formation process, due to the surface tension during the phase change, the microsilica powder forms amorphous spherical particles with a smooth surface. Some are agglomerates of multiple spherical particles stuck together. It is a volcanic ash material with a large specific surface area and high activity. The tiny spheres of materials mixed with microsilica can play a lubricating role.

[0019] The composition of microsilica powder was observed by polarizing microscope. Except for a small amount of carbon powder and crystalline SiO2 powder, the main components were amorphous phase. The test results of X-ray diffraction method also showed that microsilica powder contained a small amount of SiO2 crystals, and most of them were amorphous SiO2. The results of scanning electron microscope observation showed that microsilica powder was composed of spherical particles of varying sizes below 5μm.

[0020] In some examples, the preparation method of the modified microsilica powder may include: (1) preheating treatment: preheating the microsilica powder in the temperature environment of T1, T2, T3, T4, T5 and T6 in sequence to obtain preheated microsilica powder, wherein T1, T2, T3, T4, T5 and T6 are successively increased from 200°C to 700°C, and the treatment time of each temperature is 1h≤t≤3h; (2) high temperature carbonization treatment: preheating the microsilica powder in the temperature environment of T7, T8, T9, T10, T11, T12 and T13 in sequence, and then heating and carbonizing the preheated microsilica powder in the temperature environment of T14, T15, T16 and T17 in a decreasing temperature manner to obtain high temperature carbonized microsilica powder, wherein T7, T8, T9, T10, T11, T12 and T13 are successively increased, and the treatment time of each temperature is 1h≤t≤3h. 8. T9, T10, T11, T12, and T13 are increased in sequence at 700°C < temperature ≤ 1250°C, and the treatment time at each temperature is 1h≤t≤3h; T14, T15, T16, and T17 are decreased in sequence at 1200°C to 1000°C, and the treatment time at each temperature is 1h≤t≤3h; (3) Cooling treatment: the high-temperature carbonized microsilica powder is cooled in sequence at T18, T19, T20, T21, T22, and T23 to obtain modified microsilica powder; T18, T19, T20, T21, T22, and T23 are decreased in sequence at 900°C to 100°C, and the treatment time at each temperature is 1h≤t≤3h.

[0021] It should be noted that the treatment time at each temperature from T1 to T23 has a great influence on the resistivity of the prepared modified microsilica powder, especially when the treatment time at each temperature is 2h, the resistivity of the prepared modified microsilica powder is significantly improved compared with other times. For example, under certain conditions, it increased by about 12.3% compared with 1.5h, and decreased by about 12.4% for 2.5 hours compared with 2h.

[0022] It should also be noted that during the preheating treatment and high-temperature carbonization treatment, the temperature increase can be a linear change or an irregular random increase; similarly, during the cooling treatment, the temperature decrease can be a linear change or an irregular random change.

[0023] In some examples, in the above preheating treatment, 200℃≤T1<300℃, 300℃≤T2<400℃, 400℃≤T3<450℃, 450℃≤T4<500℃, 500℃≤T5<600℃, 600℃≤T6≤700℃; in the above high temperature carbonization treatment, 700℃≤T7<800℃, 800℃≤T8<950℃, 950℃≤T9<1000℃, 1000℃≤T10<1100℃, 1100℃≤T11<1150℃, 1150℃≤T12<1300℃ T12<1200℃, 1200℃≤T13<1250℃, 1000℃≤T14<1200℃, 1000℃≤T15<1200℃, 1000℃≤T16<1200℃, 1000℃≤T17<1200℃; in the above cooling treatment, 700℃≤T18≤900℃, 600℃≤T19<700℃, 300℃≤T20<600℃, 200℃≤T21<300℃, 150℃≤T22<200℃, and 100℃≤T23<150℃.

[0024] It should be noted that T1 to T23 can be changed according to the temperature range mentioned above, and the performance (especially resistivity) of the modified microsilica powder prepared under this temperature change is better than that of other temperature changes, especially the resistivity is higher than that of other temperature changes.

[0025] It should also be noted that in the above-mentioned high-temperature carbonization treatment, after the temperature in the high-temperature zone reaches the set temperature, a cooling range needs to be set in the high-temperature zone to slowly reduce the carbonization temperature to ensure the stability of the material and avoid safety problems.

[0026] It should also be noted that, in the present invention, 6 intervals are set for preheating treatment, 11 intervals are set for high-temperature carbonization treatment, and 6 intervals are set for cooling treatment, which can ensure that the microsilica powder is fully heated at high temperature to obtain high-temperature carbonized microsilica powder.

[0027] In some examples, in the above-mentioned preheating treatment, T1 is 277°C, T2 is 349°C, T3 is 401°C, T4 is 450°C, T5 is 555°C, and T6 is 637°C; in the above-mentioned high-temperature carbonization treatment, T7 is 790°C, T8 is 920°C, T9 is 993°C, T10 is 1058°C, T11 is 1133°C, T12 is 1175°C, T13 is 1213°C, T14 is 1194°C, T15 is 1184°C, T16 is 1101°C, and T17 is 1011°C; in the above-mentioned cooling treatment, T18 is 855°C, T19 is 662°C, T20 is 539°C, T21 is 278°C, T22 is 186°C, and T23 is 119°C.

[0028] It should be noted that, T1 to T23 changes according to the above-mentioned temperature, and the performance (especially resistivity) of the modified microsilica powder prepared under this temperature change is better than other temperature changes, especially the resistivity is higher than other temperature changes. Under this temperature change, the resistivity of the prepared modified microsilica powder can reach 6710uΩ·m, which is about 52.1% higher than that of the unmodified microsilica powder (4413uΩ·m).

[0029] In some examples, the preparation method may include: using a carbonization tunnel kiln to sequentially perform preheating treatment, high temperature treatment and cold treatment on the microsilica powder, including loading the microsilica powder into the carbonization tunnel kiln, and then laying a sedimentation plate cover on it, laying refractory wool on the cover for insulation, and finally sending it into the tunnel kiln for preheating treatment, high temperature treatment and cold treatment.

[0030] It should be noted that in the present invention, a carbonization tunnel kiln can be used to modify the microsilica powder. The carbonization tunnel kiln is a carbonization tunnel kiln known in the art. There are multiple kiln cars in the carbonization tunnel kiln. A single kiln car is Figure 1 As shown, it is composed of multiple kiln bodies (A1-A8), and the carbonization tunnel kiln is composed of 33 kiln cars (the kiln car is a circulating body, connected head to tail, 50% of the kiln cars are located in the kiln, and 50% of the kiln cars are located outside the kiln on the return line). The kiln bodies of a single kiln car are evenly divided, and the nozzles are ignited and heated in the fire channel. The kiln car is pushed forward to the next section at a certain interval; the kiln body is a rectangular block made of refractory bricks with an open top. There is a certain gap between the kiln bodies. The gap between two adjacent kiln bodies forms a fire channel. The bottom of the kiln body adopts an overhead design to ensure that there is a certain height between the kiln body and the kiln car to form a fire channel. The bottom fire channels are connected to each other to increase the heating area and improve the heating speed. Load the microsilica powder into the carbonization tunnel kiln. The loading needs to ensure that the material in each grid is relatively uniform. After it is full, lay a sedimentation plate cover on it, and lay refractory wool on the cover for insulation. Ensure that each grid of refractory wool is laid flat. After laying, step on the edge of the asbestos tightly to ensure sealing. Then send it into the carbonization tunnel kiln, and use natural gas to pre-carbonize the microsilica powder at high temperature to obtain modified microsilica powder.

[0031] It should also be noted that there are many ways to modify and adjust the temperature of microsilica powder using a carbonization tunnel kiln, such as igniting the burner to increase the temperature and turning off the fire to reduce the temperature; using a top-space car to enter the kiln to reduce the temperature; opening or closing the kiln door to increase or decrease the temperature; for example, the natural gas pressure is adjusted to control the temperature, but the pressure cannot be lower than the set value. Too low pressure will cause insufficient natural gas supply and affect the temperature rise in the kiln. In addition, a combustion-supporting fan can also be used during the heating process, and the combustion-supporting fan can also adjust the temperature. Specifically, the normal combustion-supporting air pressure can be 1.8KPa. By adjusting the frequency to control the delivery air pressure and coordinating with the natural gas pressure, the rise and fall of the temperature can be effectively controlled. In addition, during the carbonization process, the oxygen content in the carbonization tunnel kiln needs to be observed in real time, and it must be controlled below 21%. Too high an oxygen content proves that the carbonization tunnel kiln is not burning fully.

[0032] The embodiment of the present invention further provides a graphitization furnace bottom material, which includes the modified microsilica powder of the present invention.

[0033] It should be noted that in the bottom material of the graphitization furnace, the mass proportion of microsilica powder or modified microsilica powder is generally 20-25%, and the remaining material is carbon black. The volatiles or residual tar-like substances on the surface of carbon black will form an insulating film on the surface of carbon black and reduce the conductivity of carbon black.

[0034] It should also be noted that, as mentioned above, the resistivity of the modified microsilica powder in the present invention can reach 6710uΩ·m, which is about 52.1% higher than that of the unmodified microsilica powder (4413uΩ·m). Therefore, it can be used as the bottom material or bottom material component of the graphitization furnace. Compared with the unmodified microsilica powder as the bottom material of the graphitization furnace, using it as the bottom material or bottom material component of the graphitization furnace can effectively reduce the current leakage of the unmodified microsilica powder graphitization furnace, improve the temperature unevenness, and improve the safety and increase the service life.

[0035] An embodiment of the present invention also provides an application of the modified microsilica powder in the present invention in improving the refractory performance of a graphitization furnace.

[0036] It should be noted that the modified microsilica powder in the present invention reduces agglomeration during the preparation process, and due to the poor thermal conductivity of the powder, the resistivity is increased, thereby improving the fire resistance.

[0037] In some examples, the above-mentioned applications may include one of the following applications: (a) application of modified microsilica powder as a furnace bottom material in improving the refractory performance of a graphitization furnace; (b) application of a furnace bottom material prepared by using modified microsilica powder as one of the raw materials in improving the refractory performance of a graphitization furnace.

[0038] The beneficial effects of the present invention include at least: the resistivity of the modified microsilica powder provided by the present invention can reach 6710uΩ·m, which is about 52.1% higher than that of the unmodified microsilica powder (4413uΩ·m). Compared with the unmodified microsilica powder as the bottom material of the graphitization furnace, the modified microsilica powder can be used as the bottom material of the graphitization furnace, which can effectively reduce the current leakage of the unmodified microsilica powder graphitization furnace, improve the temperature unevenness, and improve the safety and increase the service life.

[0039] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.

[0040] 1. Preparation of Microsilica Powder / Modified Microsilica Powder

[0041] Example 1

[0042] A new material for graphitization furnace, which is used for heat insulation protection of the bottom of graphitization furnace. Microsilica powder is carbonized in air by using carbonization tunnel kiln to obtain modified microsilica powder (see Figure 2 ), including:

[0043] (1) Pre-carbonization treatment: The microsilica powder is treated in the preheating zone of the carbonization tunnel kiln to obtain pre-carbonized microsilica powder. The temperatures of the six small intervals in the preheating zone are T1, T2, T3, T4, T5 and T6 from left to right. T1 is set to 277°C, T2 is set to 349°C, T3 is set to 401°C, T4 is set to 450°C, T5 is set to 555°C, and T6 is set to 637°C. The kiln car moves to the next small interval every 2 hours, and the total residence time is 6 hours.

[0044] (2) High temperature carbonization treatment: the pre-carbonized microsilica powder is transferred to the high temperature zone of the preheating zone in the carbonization tunnel kiln for treatment to obtain high temperature carbonized microsilica powder. The temperatures of the 11 small intervals in the high temperature zone are T7, T8, T9, T10, T11, T12, T13, T14, T15, T16 and T17 from left to right. T7 is set to 790°C, T8 to 920°C, T9 to 993°C, T10 to 1058°C, T11 to 1133°C, T12 to 1175°C, T13 to 1213°C, T14 to 1194°C, T15 to 1184°C, T16 to 1101°C, and T17 to 1011°C. The kiln car moves to the next small interval every 2 hours, and the total residence time is 11 hours.

[0045] (3) Cooling treatment: The high-temperature carbonized microsilica powder is transferred to the cooling zone in the carbonization tunnel kiln for treatment to obtain modified microsilica powder. The temperatures of the six small intervals in the cooling zone are T18, T19, T20, T21, T22 and T23 from left to right. T18 is set to 855°C, T19 to 662°C, T20 to 539°C, T21 to 278°C, T22 to 186°C, and T23 to 119°C. The kiln car moves to the next small interval every 2 hours, and the total residence time is 6 hours.

[0046] Example 2

[0047] The kiln car moves to the next small interval in the preheating zone every 1 hour and 30 minutes, with a total residence time of 9 hours; the kiln car moves to the next small interval in the high temperature zone every 1 hour and 30 minutes, with a total residence time of 16 hours and 30 minutes; the kiln car moves to the next small interval in the cooling zone every 1 hour and 30 minutes, with a total residence time of 9 hours. Other steps are the same as in Example 1.

[0048] Example 3

[0049] The kiln car moves to the next small interval in the preheating zone every 2 hours, with a total residence time of 12 hours; the kiln car moves to the next small interval in the high temperature zone every 2 hours, with a total residence time of 22 hours; the kiln car moves to the next small interval in the cooling zone every 2 hours, with a total residence time of 12 hours. The other steps are the same as in Example 1.

[0050] Example 4

[0051] The kiln car moves to the next small interval in the preheating zone every 2 hours and 30 minutes, with a total residence time of 15 hours; the kiln car moves to the next small interval in the high temperature zone every 2 hours and 30 minutes, with a total residence time of 27 hours and 30 minutes; the kiln car moves to the next small interval in the cooling zone every 2 hours and 30 minutes, with a total residence time of 15 hours. Other steps are the same as in Example 1.

[0052] Example 5

[0053] The kiln car moves to the next small interval in the preheating zone every 3 hours, with a total residence time of 18 hours; the kiln car moves to the next small interval in the high temperature zone every 3 hours, with a total residence time of 33 hours; the kiln car moves to the next small interval in the cooling zone every 3 hours, with a total residence time of 18 hours. The other steps are the same as in Example 1.

[0054] Comparative Example 1

[0055] The microsilica powder that has not been pre-carbonized is used as comparative example 1.

[0056] 2. Performance test of microsilica fume / modified microsilica fume

[0057] The moisture content, ash content, volatile matter, sulfur content and resistivity of the modified microsilica fume in Example 1, Comparative Examples 1 to 4 and the microsilica fume in Comparative Example 5 were tested respectively.

[0058] The moisture content is determined by the principle of loss on drying method. The sample is quickly heated by the heating system so that the moisture in the sample can be completely evaporated in a short time without affecting the tissue composition of the sample itself. Specifically, the weighing bottle with a constant mass is weighed in the center of the balance (the error value is 2g±0.0002), and the mass of the weighing bottle and the sample are recorded. After weighing, it is placed in a 110℃±5℃ electric blast drying oven at a constant temperature for 2 hours, taken out and placed in a dryer for about 0.5 hours, placed in a balance for weighing and recording, and then the test results are calculated;

[0059] The ash content is determined by weighing the sample in a porcelain crucible, placing it in a muffle furnace and burning it until all carbon-containing substances are oxidized, placing the crucible in a dryer to cool and weigh it, and finally calculating the ash content; specifically, the porcelain crucible is weighed in the center of a balance (error value 1g±0.0002 / 3g±0.0002, and the mass of the porcelain crucible and the net weight of the sample are recorded. After weighing, it is placed in a muffle furnace at 950℃±25℃ and calcined for 3h, then taken out and placed in a dryer for about 0.5h, placed in a balance for weighing and recording, and then the test result is calculated;

[0060] Volatile matter refers to the organic matter and part of the mineral matter in coal that is pyrolyzed into gas after being heated for 7 minutes in an airtight manner under specified conditions, including the escape of liquid generated at room temperature, which reduces the mass. The percentage of the lost mass to the coal volume is deducted from the moisture content of the coal sample. Specifically, the covered crucible is weighed 1g in the center of the balance, and the mass of the covered crucible and the net weight of the sample are recorded. After weighing, it is placed in a 900℃ intelligent muffle furnace and burned for 7 minutes. After being taken out of the furnace and cooled for 5-6 minutes, it is placed in a dryer for about 0.5h, and then weighed and recorded on a balance, and the test results are calculated.

[0061] Sulfur content refers to the combustion and decomposition of carbon material samples in the air under the action of catalysts. The sulfur in the carbon material generates sulfur oxides, of which sulfur dioxide is absorbed by potassium iodide solution and is measured by iodine produced by electrolysis in potassium iodide solution. The total sulfur content in the carbon material is calculated based on the amount of electricity consumed by electrolysis. Specifically, it includes: weighing the porcelain crucible in the center of the balance (the error value is 0.0500g±0.0002), recording the net weight of the sample and entering it into the sulfur content instrument software for detection;

[0062] The resistivity measuring instrument consists of two parts: mechanical pressure and electronic measurement. The mechanical pressure part uses a pressure sensor, a turbine jack rotates to pressurize, and a spring is installed to maintain constant pressure. The electronic measurement part uses a single-chip microcomputer and a special software is designed to make the measured results intuitively displayed and directly printed, so as to realize automatic measurement; specifically, it includes: taking out a clean weighing paper, weighing the prepared sample (0.3-0.5mm) 3.4g-3.4010g, and then calibrating the preheated instrument with a standard sample. Formal resistivity test: Pour the weighed sample into the sample tube and shake it gently to flatten it, cover the sensor top cover, press the pressure zeroing key (FZ) and (F) keys in turn, and slowly rotate the pressure bolt after the digital display shows "0". When the pressure digital display reaches 784N (Newton force), observe the value indicated by the dial indicator, press the (HD) key, and the display will be "0". Enter the value indicated by the dial indicator from the keyboard, and press the (P) key to display the resistivity of the sample being tested.

[0063] The results are shown in Table 1 below.

[0064] Table 1 Performance comparison of different modified microsilica powder and unmodified microsilica powder

[0065]

[0066] It can be seen from Table 1 above that the moisture, volatile matter and sulfur content of the modified microsilica powder modified by carbonization are much lower than those of the microsilica powder that has not been carbonized, so the safety of the microsilica powder after carbonization treatment is higher than that of the microsilica powder that has not been carbonized; in addition, the ash content of the modified microsilica powder is not much different from that of the unmodified microsilica powder, that is, the modified microsilica powder has little effect on the purity of the microsilica powder; in addition, the resistivity of the modified microsilica powder is much higher than that of the microsilica powder treated by carbonization. Moreover, during the carbonization process, as the interval time of each cell increases, the moisture, ash, volatile matter and sulfur content all change, especially the resistivity change is particularly obvious. As the interval time of each cell increases, the resistance first increases and then decreases, and increases sharply at 2h, from 5976uΩ·m at 1.5h to 6710uΩ·m at 2h, an increase of about 12.3%. After 2h, the resistivity decreases sharply, from 6710uΩ·m to 5881uΩ·m, a decrease of about 12.4%; in addition, the modified microsilica powder after carbonization is not easy to agglomerate. Therefore, the present invention combines the changes in resistivity and moisture, ash, volatile matter and sulfur content, selects the interval time of each cell to be 2h, and the prepared modified microsilica powder has a higher resistivity, which is significantly better than other interval times, and is about 52.1% higher than the unmodified microsilica powder. It can be used as the bottom material of the graphitization furnace, effectively solving the defects of current leakage, uneven temperature, low safety and short life of the graphitization furnace.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be covered by the scope of the claims of the present invention.

Claims

1. A modified microsilica powder, It is characterized in that The preparation method thereof comprises: (1) Preheating treatment: treating the microsilica powder under preheating conditions to obtain preheated microsilica powder, the preheating conditions including: gradually heating at a temperature of 200° C. to 700° C. for 6 h to 18 h; (2) High temperature carbonization treatment: The preheated microsilica powder is treated under high temperature carbonization conditions to obtain high temperature carbonized microsilica powder. The high temperature carbonization conditions include: firstly increasing heating for 7h-21h at a temperature environment of 700°C < temperature ≤ 1250°C; then decreasing heating for 4h-12h at a temperature environment of 1200°C to 1000°C; (3) Cooling treatment: Cooling the high-temperature carbonized microsilica powder under cooling treatment conditions to obtain modified microsilica powder. The cooling treatment conditions include: cooling down in a temperature environment of 900°C to 100°C for 6h-18h.

2. The modified microsilica powder according to claim 1, It is characterized in that (1) Preheating treatment: preheating the microsilica powder in the temperature environment of T1, T2, T3, T4, T5 and T6 in sequence to obtain preheated microsilica powder, wherein T1, T2, T3, T4, T5 and T6 are increased in sequence from 200°C to 700°C, and the treatment time at each temperature is 1h≤t≤3h; (2) High temperature carbonization treatment: the preheated microsilica powder is heated in turn at T7, T8, T9, T10, T11, T12, and T13 temperature environments, and then heated and carbonized at T14, T15, T16, and T17 temperature environments to obtain high temperature carbonized microsilica powder. T7, T8, T9, T10, T11, T12, and T13 are increased in turn at 700°C < ≤ 1250°C, and the treatment time for each temperature is 1h ≤ t ≤ 3h; T14, T15, T16, and T17 are decreased in turn at 1200°C to 1000°C, and the treatment time for each temperature is 1h ≤ t ≤ 3h; (3) Cooling treatment: The high-temperature carbonized microsilica powder is cooled in the temperature environment of T18, T19, T20, T21, T22 and T23 in sequence to obtain modified microsilica powder. T18, T19, T20, T21, T22 and T23 decrease in sequence from 900°C to 100°C, and the treatment time at each temperature is 1h≤t≤3h.

3. The modified microsilica powder according to claim 2, It is characterized in that In the preheating treatment, high-temperature carbonization treatment and cooling treatment, the treatment time at each temperature is 2 hours.

4. The modified microsilica powder according to claim 2 or 3, It is characterized in that In the preheating treatment, 200℃≤T1<300℃, 300℃≤T2<400℃, 400℃≤T3<450℃, 450℃≤T4<500℃, 500℃≤T5<600℃, 600℃≤T6≤700℃; In the high temperature carbonization treatment, 700℃<T7<800℃, 800℃≤T8<950℃, 950℃≤T9<1000℃, 1000℃≤T10<1100℃, 1100℃≤T11<1150℃, 1150℃≤T12<1200℃, 1200℃≤T13<1250℃, 1000℃≤T14<1200℃, 1000℃≤T15<1200℃, 1000℃≤T16<1200℃, 1000℃≤T17<1200℃; During the cooling treatment, 700℃≤T18≤900℃, 600℃≤T19<700℃, 300℃≤T20<600℃, 200℃≤T21<300℃, 150℃≤T22<200℃, 100℃≤T23<150℃.

5. The modified microsilica powder according to claim 4, It is characterized in that In the preheating treatment, T1 is 277℃, T2 is 349℃, T3 is 401℃, T4 is 450℃, T5 is 555℃, and T6 is 637℃; in the high temperature carbonization treatment, T7 is 790℃, T8 is 920℃, T9 is 993℃, T10 is 1058℃, T11 is 1133℃, T12 is 1175℃, T13 is 1213℃, T14 is 1194℃, T15 is 1184℃, T16 is 1101℃, and T17 is 1011℃; in the cooling treatment, T18 is 855℃, T19 is 662°C, T20 is 539°C, T21 is 278°C, T22 is 186°C, and T23 is 119°C.

6. The modified microsilica powder according to any one of claims 1 to 5, It is characterized in that The preparation method includes: using a carbonization tunnel kiln to sequentially perform preheating treatment, high temperature treatment and cold treatment on the microsilica powder, including loading the microsilica powder into the carbonization tunnel kiln, then laying a sedimentation plate cover on it, laying refractory wool on the cover for insulation, and finally sending it into the tunnel kiln for preheating treatment, high temperature treatment and cold treatment.

7. Graphitization furnace bottom material, It is characterized in that The modified microsilica powder comprises the modified microsilica powder as described in any one of claims 1 to 5.

8. Use of the modified microsilica powder according to any one of claims 1 to 5 in improving the refractory performance of a graphitization furnace.

9. The use according to claim 8, It is characterized in that The application includes one of the following applications: (a) application of modified microsilica powder as furnace bottom material in improving the refractory performance of graphitization furnace; (b) application of furnace bottom material prepared by using modified microsilica powder as one of the raw materials in improving the refractory performance of graphitization furnace.

Citation Information

Patent Citations