Catalyst carrier macroporous silica gel and preparation method thereof

By using pH indicator liquid and template agent in the silica gel preparation process to control the reaction process, the problem of difficulty in grasping the primary gel point and high cost was solved. Carrier macroporous silica gel with large pore volume and high specific surface area was prepared, which improved the Catalytic performance and skeleton strength.

CN118754137AActive Publication Date: 2024-10-11QINGDAO MAKALL GROUP CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410768393.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-11
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing macroporous silica gel preparation methods have problems such as difficulty in grasping the primary gel point, high cost, and wide pore size distribution, which affect catalytic performance.

Method used

By adding a pH indicator solution and a template agent to the reaction system, the reaction process is controlled by using the gel micronucleus indicating effect of the pH indicator solution and the pore expanding effect of the template agent to prepare a carrier macropore with large pore volume and high specific surface area. Silicone.

Benefits of technology

It achieves accurate control of the condensation point, reduces costs, increases the pore volume and specific surface area of ​​silica gel, and improves the skeleton strength, making it suitable for polyolefin catalyst carriers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004893312860000081
    Figure BDA0004893312860000081
  • Figure BDA0004893312860000082
    Figure BDA0004893312860000082
  • Figure BDA0004893312860000091
    Figure BDA0004893312860000091
Patent Text Reader

Abstract

The invention discloses a catalyst carrier macroporous silica gel and a preparation method thereof.The preparation method comprises the following steps that S1, PH indicating liquid and a template agent are added into inorganic acid, and after the mixture is stirred to be uniform, the solution shows the first color; s2, adding a silicate solution, when the color of a system changes, namely primary micronuclei are formed, and adding more than three times of water to quickly disperse the primary micronuclei; s3, continuing to add the silicate solution, stopping adding after the color of the system changes again, uniformly stirring at a constant temperature, and then adding acid to promote the stability of a particle skeleton; and S4, sequentially carrying out acid pickling, water washing, pulping, spray drying and high-temperature calcination on the system to obtain the catalyst carrier macroporous silica gel. The preparation method of the catalyst carrier macroporous silica gel has the advantages of sensitive and rapid detection, high accuracy and strong operability, and the prepared silica gel has a large pore volume, a large specific surface and a wide application range, and can be used as a carrier silica gel of a catalyst in the polyolefin field and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic materials, and in particular to a catalyst carrier macroporous silica gel and a preparation method thereof. Background Art

[0002] Silica gel is mainly used as a catalyst and catalyst carrier in the petrochemical industry. It plays a very important role in catalyst components. The internal pore structure of silica gel has a very important influence on the morphology of polymers. At present, most of the catalyst carrier silica gel used in the polyolefin industry is imported, and domestic substitution is imperative.

[0003] The existing macroporous silica gel is mainly prepared by adjusting the addition method and reaction conditions of silicate and acid to make silicate react with acid, which has the following problems: the primary gel has more small pores, the silica gel pore size distribution is wider, and the catalytic performance is affected; for example, in the patent with application number CN200610129489.8, water glass and inorganic acid are reacted in a certain ratio to produce a macroporous silica gel carrier for ethylene polymerization catalyst at a pH of 2-4. Secondly, other existing methods for preparing macroporous carrier silica gel have the problem that the primary gel point appears quickly and is difficult to grasp, which is not conducive to the dispersion of the primary gel; for example, the patent with publication number CN102745698 B discloses a method for preparing carrier silica gel, which forms a primary gel with an inorganic acid at pH = 2-4 by adding a silicate solution, and then forms a secondary and tertiary gel at pH = 7-9 and pH = 10-12, and prepares a macroporous silica gel carrier by repeated gelation. In this method, the initial gelation point of the macroporous silica gel appears quickly and is difficult to grasp, and it is difficult to accurately judge the key point of the gel reaction; and the preparation cost of the above-mentioned macroporous silica gel is relatively high, therefore, the existing technology needs to be further improved. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for preparing macroporous silica gel as a catalyst carrier, which has easier condensation points to grasp, simpler operation and lower cost, and the prepared product, wherein the macroporous catalyst carrier silica gel is prepared by the gel micronucleus indicating effect of the pH indicator liquid and the pore expanding effect of the template agent.

[0005] In order to solve the above problems, the present invention provides the following technical solutions:

[0006] A method for preparing a carrier macroporous silica gel comprises the following steps:

[0007] S1. Add pH indicator solution and template agent to inorganic acid, stir evenly, and keep at constant temperature for 1 to 3 hours until the solution shows the first color;

[0008] S2, add silicate solution, when the color of the system changes, the primary micronucleus is formed, add 3 times more water to make the primary micronucleus disperse quickly;

[0009] S3, continue to add silicate solution, stop adding after the color of the system changes again, stir evenly at constant temperature, and then add acid until the color of the system changes again, thereby stabilizing the particle skeleton;

[0010] S4. Then the system is sequentially subjected to acid washing, water washing, pulping, spray drying and high-temperature calcination to obtain a carrier macroporous silica gel.

[0011] Preferably, S2, add a silicate solution with a weight percentage concentration of 8-25% based on the silicon dioxide content, and when the color of the system changes, the primary micronuclei are formed, and add 3-8 times of water to quickly disperse the primary micronuclei.

[0012] In the above scheme, the raw materials for preparing silica gel are silicate solution, template solution and acid solution. Since a pH indicator solution is added to the system, the color of the system solution changes with the change of pH in the reaction system during the reaction process. By capturing the change of the color of the system, the next step of operation is started, so that the raw materials gradually react with each other to form a gel skeleton.

[0013] The reaction principle is as follows: ① Silicate will hydrolyze in an acidic aqueous solution. According to the ionization equilibrium constant of silicate and the pH stability range, silicate is stable in the range of pH = 2 to 3. When pH > 4, monosilicic acid will begin to condense and form nuclei. The color change point of the selected indicator is consistent with the hydrolysis and condensation point of silicate. The color change of the indicator (about pH = 4) can be used to quickly judge the arrival of the change point, so as to add enough water to the system in time to quickly disperse the primary micronuclei; ② Then continue to add silicate to the system until the color of the solution changes again (about pH = 10 ), during this process, the silicate in the system continues to hydrolyze, forming connecting bridges between local micronuclei, connecting the dispersed micronuclei into a loose and porous structure like a cage; ③ Then add acid solution to the system and treat it at a constant temperature for several hours. The gel skeleton is made more stable by acid treatment, and then add acid to the system until the color of the system changes again (pH = about 3) and then stop adding. The salt in the skeleton is replaced by excess acid to complete the acid washing, so as to facilitate subsequent water washing; ④ The formed gel is subsequently washed with water, dried and calcined at high temperature to obtain a macroporous powdered silica gel product.

[0014] The final macroporous silica gel has a silicon dioxide content of more than 99% and a specific surface area of ​​300m 2 / g, pore volume>1.55cm 3 / g, and the load crushing rate is less than 10%, and the skeleton strength is significantly improved.

[0015] Compared with the existing macroporous silica gel preparation process, which uses a pH meter electrode probe to insert into the reaction system to detect the pH of the system, it not only has the problem of slow detection reaction and insufficient sensitivity, but also affects the accurate judgment of the key points of the reaction due to the condensation of silicate to paste the pH electrode probe; the present application introduces a pH indicator liquid into the system, which has the advantages of sensitive and fast detection and high accuracy, and solves the various problems existing in the above-mentioned prior art. And the above method can timely judge the formation of primary micronuclei, avoid the micronuclei adhering to each other into a jelly-like gel due to untimely water addition and dispersion, which is not conducive to subsequent reactions, resulting in the problem of small pore volume and specific surface area of ​​silica gel products.

[0016] Furthermore, more importantly, the pH indicator liquid preferably used in the present application is mixed with polyethylene glycol in a weight percentage concentration of 5-15%. For example, the dyeing waste liquid mixed with polyethylene glycol surfactants (weight percentage concentration of 5-15%) can be directly used. On the one hand, this scheme recycles the dyeing waste liquid in the production of pH color-changing indicator silica gel (such as the patent for "a pH color-changing indicator silica gel" with application number 202210936482.6), thereby reducing the cost of raw materials; on the other hand, the polyethylene glycol mixed in the dyeing waste liquid can not only disperse the gel micronuclei, but also play a certain role in expanding the pores as a template. During the gelation process, the polyethylene glycol is wrapped in the skeleton, and pores will be generated when it is removed after calcination in the later stage.

[0017] Preferably, in the above-mentioned method for preparing macroporous silica gel, the pH indicator liquid is selected from one, two or more of quinaldine red, bromothymol blue, phenolphthalein, thymol blue, bromophenol blue, methyl red, methyl orange, dimethyl yellow, catechol violet, Nile blue, ethoxy yellow chigin, naphthol, and meta-cresol violet. Preferably, the pH indicator liquid is selected from methyl red, quinaldine red, bromothymol blue, catechol violet, and phenolphthalein.

[0018] The pH indicator liquid adopts a combination of one or more indicators, and its color change point is consistent with the silicate hydrolysis condensation point and other two-step skeleton synthesis key nodes, and the color change of the indicator facilitates the operator to accurately grasp the operation nodes of each step. Optionally, the pH indicator liquid is a mixed indicator of methyl red and bromothymol blue, a mixed indicator of methyl red and phenolphthalein, or a mixed indicator of quinaldine red and catechol violet.

[0019] Preferably, in the method for preparing the carrier macroporous silica gel, the acid is selected from one of hydrochloric acid, sulfuric acid, nitric acid, citric acid, acetic acid and oxalic acid; preferably, the acid is hydrochloric acid or sulfuric acid.

[0020] Preferably, in the method for preparing the carrier macroporous silica gel, the template is selected from one or two of ammonium bicarbonate, ammonium carbonate, ammonia water, ammonium bisulfate, ammonium chloride, and ammonium acetate; preferably, the template is ammonia water or ammonium bisulfate.

[0021] Preferably, in the method for preparing the carrier macroporous silica gel, the silicate is selected from one or more of sodium silicate, potassium silicate and lithium silicate. Further preferably, the silicate is sodium silicate.

[0022] Further preferably, step S1 is to add a pH indicator solution (final concentration is 0.5-2‰) to 200-1000 mL of an inorganic acid with a mass percentage concentration of 5-20%, add a template agent (final concentration is 5-15%) at 15-60°C, and treat at a constant temperature for 1-2 hours.

[0023] Preferably, step S2 is to maintain the temperature at 45-60° C., then add a silicate solution with a mass percentage concentration of 8-25% in terms of silicon dioxide content, and when the color of the system changes, the primary micronuclei are formed, and add 3-8 times of water to quickly disperse the primary micronuclei;

[0024] Preferably, step S3 is to continue adding a silicate solution with a mass percentage concentration of 8-25% in terms of silicon dioxide content, stop adding after the color of the system changes again, stir at a constant temperature for 1 to 3 hours, then add an inorganic acid with a mass percentage concentration of 5 to 10%, and keep warm for 5 to 10 hours, thereby stabilizing the particle skeleton.

[0025] Preferably, step S4 is to add acid (mass percentage concentration of 1-5%) to the system until the color of the system changes again for acid washing; then wash with water at 50-70°C, add a binder with a mass percentage concentration of 0.5%-10% for pulping and spray drying at 200-300°C, and then calcine at 750-850°C for 0.5-1.5h.

[0026] The binder can be one or more of silica sol, potassium silicate or sodium silicate. Preferably, the amount of silica sol added is 4%-10%, the amount of potassium silicate added is 0.5-6%, and the amount of sodium silicate added is 0.3-5% (all are mass percentage concentrations). The role of adding the binder is to form a film on the surface of the particles, increase the strength of the particle surface, and make the particle skeleton strength after spray molding stronger.

[0027] Preferably, the calcination condition is calcination at 800° C. for 1 hour. Compared with the gradient temperature increase at this stage in the prior art, the treatment under this condition combined with the above treatment is more conducive to improving the overall skeleton strength of the macroporous silica gel after the catalyst is loaded.

[0028] The preparation method of the carrier macroporous silica gel of the present invention has the following beneficial effects:

[0029] 1. The preparation method of macroporous silica gel provided by the present invention can timely judge the formation of primary micronuclei and other important nodes through the gel micronucleus indicating effect of pH indicator liquid and the pore expanding effect of template agent, and has the advantages of sensitive and fast detection and high accuracy. The prepared silica gel has a large pore volume and a large specific surface area, and can be used as a carrier of polyolefin catalysts, and has good application prospects as a catalyst carrier.

[0030] 2. The preparation method of the macroporous silica gel of the present invention can directly use the dyeing waste liquid mixed with polyethylene glycol surfactant as the pH indicator liquid, which can not only greatly reduce the production cost, but also reduce environmental pollution and waste of resources; in addition, the polyethylene glycol mixed in the dyeing waste liquid can not only play the role of dispersing the gel micronuclei, but also play a certain role of expanding the pores as a template, further improving the comprehensive performance of the silica gel product, such as expanding the pore volume and specific surface area. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. In the present invention, unless otherwise specified, the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are conventional methods in the art unless otherwise specified.

[0032] Example 1

[0033] (1) Pour 200 mL of 16% by mass dilute sulfuric acid solution into a reaction kettle, add 30 mL of a mixed indicator of methyl red and bromothymol blue (containing 5% polyethylene glycol), start stirring, add 30 mL of 8% by mass ammonia solution at 35°C, keep the temperature constant for 1.5 hours after the addition is complete, and the solution turns red.

[0034] (2) After heating to 50°C, add a 14% sodium silicate solution; when the solution changes from red to yellow, i.e., gel micronuclei appear, add 800 mL of distilled water to evenly disperse the gel micronuclei;

[0035] (3) Continue to add sodium silicate solution until the solution turns dark blue, stop adding and keep the temperature constant for 1.5 hours; then add 100 ml of 6% dilute sulfuric acid to stabilize the gel skeleton. After keeping the temperature constant for 10 hours, add 500 ml of 3% dilute sulfuric acid solution to acidify until the solution turns yellow-green;

[0036] (4) After washing with water at 50°C, 10 g of 30% silica sol was added for slurrying, spray-dried at 220°C, and calcined at 800°C for 1 hour to obtain a macroporous powdered silica gel product.

[0037] The performance of the product is shown in Table 1.

[0038] Example 2

[0039] (1) Place 400 mL of a 20% by mass dilute hydrochloric acid solution in a reaction kettle, add 0.785‰ of a mixed indicator of methyl red and phenolphthalein (containing 3% polyethylene glycol), start stirring, add 50 mL of a 15% aqueous ammonium bisulfate solution at 60°C, and keep the temperature constant for 1 hour;

[0040] (2) Add 24% sodium silicate solution; when the solution changes from red to orange, i.e. gel micronuclei appear, quickly add 2000 mL of distilled water to evenly disperse the micronuclei;

[0041] (3) Continue to add sodium silicate solution until the solution turns dark red, stop adding and keep the temperature constant for 3 hours; then add 200 ml of 7% dilute hydrochloric acid to stabilize the gel skeleton, continue to keep the temperature constant for 5 hours, then add 200 ml of 5% dilute hydrochloric acid solution to acidify until the solution turns yellow;

[0042] (4) After washing with water at 70°C, 5 g of 30% potassium silicate was added for pulping, spray-dried at 300°C, and calcined at 800°C for 1 hour to obtain a macroporous powdered silica gel product.

[0043] The performance of the product is shown in Table 1.

[0044] Example 3

[0045] (1) Place 1000 mL of 5% by mass dilute sulfuric acid solution in a reaction kettle, add quinaldine red and catechol violet indicator (containing 5% polyethylene glycol), start stirring, slowly add 300 mL of 5% ammonium bisulfate solution at 15° C., and keep the temperature constant for 1.5 hours until the solution becomes colorless;

[0046] (2) Raise the temperature to 50°C and add 8% sodium silicate solution; when the solution changes from colorless to red, i.e., gel micronuclei appear, add 5000 mL of distilled water to disperse the gel micronuclei;

[0047] (3) Continue to add sodium silicate solution until the solution turns purple-red, stop adding and keep the temperature constant for 1.5 hours, then add 200 ml of 6% dilute sulfuric acid to promote continued gelation;

[0048] (4) Finally, the temperature was raised to 60°C, kept at this temperature for 7 hours, and then a dilute sulfuric acid solution was added to acidify the mixture until it turned yellow; after washing with water at 50°C, 13 g of 30% sodium silicate was added to make a pulp, and the mixture was spray-dried at 220°C and then calcined at 800°C for 1 hour to obtain a silica gel product.

[0049] The performance of the product is shown in Table 1.

[0050] Comparative Example 1

[0051] Macroporous silica gel was prepared by referring to the scheme of Example 1 of the existing patent CN102745698 B:

[0052] Place 200 ml of 1.1 mol / L dilute sulfuric acid solution in a reactor, start stirring, slowly add 30 ml of 5.0 mol / L ammonia solution at 30°C, and keep the temperature constant for 1 hour after the addition is completed; raise the temperature to 50°C, and add 1.3 mol / L sodium silicate solution at 3.0 ml / min; when the solution is initially gelled, quickly add 400 ml of distilled water, and stir the silica gel to disperse it thoroughly; continue to add sodium silicate solution until the pH value of the solution is 11 (detected by a pH meter), Stop adding and keep the temperature constant for 1 hour; add a dilute sulfuric acid solution with a concentration of 1.1 mol / L at 4.0 ml / min to promote the continued gelation of the silica gel. When the pH value of the solution reaches 9 (detected by a pH meter), stop adding dilute sulfuric acid and keep the temperature constant for 1 hour; finally, heat to 70°C, keep the temperature constant for 5 hours, then quickly add dilute sulfuric acid solution for acidification, wash and pulp with distilled water, spray dry at 220°C, and activate with gradient heating (200°C (1 hour) - 400°C (1 hour) - 600°C (2 hours)) to obtain a silica gel product. The performance of the product is shown in Table 1.

[0053] Comparative Example 2

[0054] Except that polyethylene glycol was not added during the preparation process, the other preparation processes were the same as those in Example 1. The properties of the product are shown in Table 1.

[0055] Comparative Example 3

[0056] Except that the pH indicator solution containing polyethylene glycol is not added during the preparation process, the other preparation processes are the same as those of Example 1. The properties of the product are shown in Table 1.

[0057] Silicone performance test example

[0058] The silica gel products prepared in the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to various performance tests according to the following methods.

[0059] 1. Determination of silica gel pore volume - water titration method

[0060] Weigh 10g of the sample dried at (150±5)℃, accurate to 0.01g. Place it in a dry 250mL conical flask with a ground stopper, accurately add about 5mL of water at a time with a 25mL burette, cover the stopper, and then shake the conical flask for 5min until the sample is loose. Open the stopper again, add water drop by drop, and shake the conical flask after each addition of water. If the sample is still loose after shaking, continue to add water drop by drop; if the sample particles stick to each other and adhere to the bottle wall and do not disappear after shaking for 1min, it is the titration end point. Record the volume of water consumed.

[0061] The pore volume w8, expressed in mL / g, is calculated according to formula (1):

[0062]

[0063] Where:

[0064] V——The volume of water consumed, in milliliters (mL)

[0065] m – the numerical value of the sample mass, in grams (g).

[0066] The arithmetic mean of the parallel determination results was taken as the determination result, and the absolute difference between the two parallel determination results was not greater than 0.02 mL / g.

[0067] 2. Determination method of specific surface area of ​​silica gel - BET method

[0068] Weigh 0.2g~0.3g of the sample dried to constant mass, accurate to 0.0002g. Put it into the measuring tube, vacuum degas for 2h at 150℃~200℃, make the vacuum degree reach below 1Pa, and start measuring the adsorption isotherm. Dead volume correction needs to be started for the first measurement. BET equation:

[0069] P / V(Po-P)=1 / VmC+[(C-1) / VmC](P / Po)

[0070] Analysis shows that when (P / Po) is in the range of 0.05-0.35, the BET equation is a linear equation, and the reciprocal of the sum of the slope and the intercept of the straight line is exactly the saturated adsorption capacity of the single layer. Therefore, in this range, 3-5 pressure points are selected, the adsorption capacity of each pressure point is measured, and then a graph is drawn according to the BET equation to obtain the saturated adsorption capacity of the single layer, and then the specific surface area is calculated.

[0071] 3. Average pore size of silica gel Measurement method

[0072] The calculation of silica gel pore size is pore size = 40000*pore volume / specific surface area

[0073] 4. Determination method of silica gel skeleton strength (load crushing rate)

[0074] The skeleton strength test method is to add silica gel into an organic solvent, stir it at high temperature for 8 hours, and then observe and compare the crushing conditions under a microscope after drying.

[0075] Table 1 Comparison of the performance of macroporous silica gel in various embodiments

[0076]

[0077]

[0078] According to the experimental results in Table 1 above, compared with the existing scheme of Comparative Example 1, the average pore size of the macroporous silica gel prepared in Examples 1 to 3 of the present application is improved, and the skeleton strength is significantly improved, especially the pore volume and specific surface area of ​​the macroporous silica gel in Example 1 are significantly better than those in Comparative Document 1.

[0079] Compared with Comparative Example 3, the pore volume, specific surface area, average pore size, etc. of Example 1 are greatly reduced, which shows that the use of a pH indicator solution containing polyethylene glycol is helpful to accurately determine the formation of primary micronuclei and other important nodes, and greatly improves the quality of macroporous silica gel.

[0080] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.

Claims

1. A method for preparing a catalyst carrier macroporous silica gel, It is characterized in that The following steps are involved: S1. Add pH indicator solution and template agent to inorganic acid, stir evenly, and the solution presents the first color; S2, add silicate solution, when the color of the system changes, the primary micronucleus is formed, add 3 times more water to make the primary micronucleus disperse quickly; S3, continue to add silicate solution, stop adding after the color of the system changes again, stir evenly at constant temperature, and then add acid to stabilize the particle skeleton; S4. Then the system is sequentially subjected to acid washing, water washing, pulping, spray drying and high-temperature calcination to obtain a carrier macroporous silica gel.

2. The method for preparing the macroporous silica gel carrier according to claim 1, It is characterized in that The pH indicator solution is mixed with polyethylene glycol at a weight percentage concentration of 5-15%.

3. The method for preparing the catalyst carrier macroporous silica gel according to claim 1, It is characterized in that The acid is selected from one of hydrochloric acid, sulfuric acid, nitric acid, citric acid, acetic acid and oxalic acid; preferably, the acid is hydrochloric acid or sulfuric acid; The silicate is selected from one or more of sodium silicate, potassium silicate and lithium silicate; preferably, the silicate is sodium silicate.

4. The method for preparing the catalyst carrier macroporous silica gel according to claim 1, It is characterized in that The template is selected from one or two of ammonium bicarbonate, ammonium carbonate, ammonia water, ammonium bisulfate, ammonium chloride, and ammonium acetate; preferably, the template is ammonia water or ammonium bisulfate.

5. The method for preparing the catalyst carrier macroporous silica gel according to claim 1, It is characterized in that The pH indicator liquid is selected from one, two or more of quinaldine red, bromothymol blue, phenolphthalein, thymol blue, bromophenol blue, methyl red, methyl orange, dimethyl yellow, catechol violet, Nile blue, ethoxylated yellow chitin, naphthol and m-cresol violet.

6. The method for preparing the catalyst carrier macroporous silica gel according to claim 5, It is characterized in that The silicate is sodium silicate.

7. The method for preparing the macroporous silica gel carrier according to claim 1, It is characterized in that Step S1 is to add a pH indicator solution to 200 to 1000 mL of an inorganic acid with a mass percentage concentration of 5 to 20%, add a template agent at 15 to 60° C., and treat at a constant temperature for 1 to 2 hours.

8. The method for preparing the catalyst carrier macroporous silica gel according to claim 1, It is characterized in that Step S2 is to maintain the temperature at 45-60°C, and then add a silicate solution with a mass percentage concentration of 8-25% in terms of silicon dioxide content. When the color of the system changes, the primary micronuclei are formed, and 3-8 times of water is added to quickly disperse the primary micronuclei.

9. The method for preparing the catalyst carrier macroporous silica gel according to claim 1, It is characterized in that Step S4 is to add acid to the system until the color of the system changes again for acid washing; then wash with water at 50-70°C, add a binder for pulping and spray drying at 200-300°C, and then calcine at 750-850°C for 0.5-1.5h.

10. A catalyst carrier macroporous silica gel, It is characterized in that The catalyst carrier is prepared by the method for preparing macroporous silica gel as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of carrier silica gel

    CN102745698A

  • Preparation method of silica gel carrier for olefin catalysis

    CN109836517A

  • Production method of spherical silica gel for catalyst carrier and obtained spherical silica gel

    CN116947055A

  • Nano-silicon dioxide used for nanometer standard granule

    CN1594079A

  • Method for preparing Nano silicon dioxide

    CN1626440A