Treatment method of sodium oxalate waste residue in Bayer process aluminum oxide production

The Bayer process is used to leach, oxidize and flash evaporate sodium oxalate waste residue in alumina production, which solves the problems of high energy consumption, large carbon emissions and low efficiency in the existing technology, and achieves efficient treatment of sodium oxalate waste residue and sodium carbonate. of recycling.

CN118754160APending Publication Date: 2024-10-11ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410848730.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing treatment process for sodium oxalate waste residue in alumina production has problems such as high energy consumption, large carbon emissions, low efficiency and complex processes.

Method used

Using the Bayer method, the sodium oxalate waste residue is leached and concentrated into a sodium oxalate crystal suspension. Sodium hydroxide is added and oxidized with oxygen under the catalysis of a catalyst to generate a sodium carbonate solution, which is then flashed and causticized. To obtain high concentration caustic lye.

Benefits of technology

It achieves efficient oxidation of sodium oxalate waste residue with low energy consumption, low carbon emissions, simple process, improved treatment efficiency, and can directly recycle sodium carbonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754160A_ABST
    Figure CN118754160A_ABST
Patent Text Reader

Abstract

The invention relates to a treatment method for sodium oxalate waste residues in Bayer process aluminum oxide production, and the treatment method for the sodium oxalate waste residues in Bayer process aluminum oxide production comprises the following steps: carrying out leaching treatment on the sodium oxalate waste residues to obtain a sodium oxalate solution; concentrating the sodium oxalate solution to obtain a sodium oxalate crystal suspension; adding sodium hydroxide into the sodium oxalate crystal suspension to obtain an alkalized suspension; and with oxygen as an oxidizing agent, adding a catalyst at a predetermined total pressure, a predetermined partial pressure of oxygen and a predetermined temperature to carry out an oxidation reaction on the alkalized suspension to obtain a sodium carbonate solution. According to the method, the sodium oxalate in the sodium oxalate waste residues is leached and then treated into the sodium oxalate crystal suspension, the sodium oxalate is directly oxidized in the solution through oxygen under the condition that the sodium hydroxide is added, energy consumption is low, carbon emission is low, efficiency is high, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the aluminum industry, and more particularly to aluminum industry waste treatment. Background Art

[0002] Organic matter in bauxite is a harmful impurity that seriously affects the production of alumina, and sodium oxalate is one of the main organic matter. In order to control the influence of sodium oxalate in alumina production, a variety of sodium oxalate removal technologies have been developed at home and abroad, such as crystallization, ion exchange, solution combustion and oxidation, etc. Among them, the mother liquor crystallization method has been promoted and applied in more and more alumina production enterprises due to its advantages such as simple process control, low energy consumption and low cost.

[0003] Alumina production companies that use the crystallization method to remove organic matter produce a large amount of sodium oxalate waste residue that is harmful to the environment every year. In addition to sodium oxalate and soluble organic matter, the soluble components in the sodium oxalate solid waste residue produced in the alumina production process also contain sodium hydroxide, sodium carbonate, and sodium aluminate; the insoluble components are mainly aluminum hydroxide and a small amount of organic matter. The main technologies for recycling and utilizing sodium oxalate solid waste residue that have been researched and developed include: sintering method, thermal decomposition method, lime causticization method, and preparation of sodium oxalate or oxalic acid products after purification. Among them, the sintering method and thermal decomposition method both have the problems of high energy consumption and large carbon emissions; the lime causticization method cannot be implemented under high caustic concentrations and has low efficiency; the purification of sodium oxalate has the problem of complex process and cumbersome procedures. Summary of the invention

[0004] The embodiment of the present application provides a method for treating sodium oxalate waste residue in Bayer process alumina production to solve the current technical problems of high energy consumption and carbon emissions, low efficiency and complex process in the treatment of sodium oxalate waste residue.

[0005] The present application embodiment provides a method for treating sodium oxalate waste residue in Bayer process alumina production, and the method for treating sodium oxalate waste residue in Bayer process alumina production comprises the following steps:

[0006] Leaching the sodium oxalate waste residue to obtain a sodium oxalate solution;

[0007] Concentrating the sodium oxalate solution to obtain a sodium oxalate crystal suspension;

[0008] adding sodium hydroxide to the sodium oxalate crystal suspension to obtain an alkaline suspension;

[0009] With oxygen as an oxidant, the alkalized suspension is subjected to an oxidation reaction under the catalysis of a catalyst at a predetermined total gas pressure, a predetermined oxygen partial pressure and a predetermined temperature to obtain a sodium carbonate solution.

[0010] In some embodiments of the present application, the leaching treatment is performed using hot water at 90-98°C.

[0011] In some embodiments of the present application, the concentration of the sodium oxalate solution is 30-60 g / L.

[0012] In some embodiments of the present application, the solid content of the sodium oxalate crystal suspension is 20-60 g / L.

[0013] In some embodiments of the present application, the catalyst is MnO 2 -CeO 2 Composite oxide catalysts.

[0014] In some embodiments of the present application, in the catalyst, MnO 2 and CeO 2 The molar ratio is 1 to 24:1; and / or,

[0015] The amount of the catalyst added is: 5 to 30 g of the catalyst per liter of the alkalized suspension.

[0016] In some embodiments of the present application, the predetermined total gas pressure is 4-6.5 MPa; and / or,

[0017] The predetermined oxygen partial pressure is not less than 1 MPa; and / or,

[0018] The predetermined temperature is 180-260°C.

[0019] In some embodiments of the present application, the method for treating sodium oxalate waste residue in the Bayer process alumina production further comprises the following steps:

[0020] Flash evaporating the sodium carbonate solution to obtain a high-concentration sodium carbonate solution;

[0021] After diluting and filtering the high-concentration sodium carbonate solution, the filtrate is subjected to causticizing treatment to obtain caustic alkali solution.

[0022] In some embodiments of the present application, the concentration of the high concentration sodium carbonate solution is 150-210 g / L.

[0023] In some embodiments of the present application, sodium hydroxide is added to the sodium oxalate crystal suspension, and the molar amount of the sodium hydroxide is not less than twice the molar amount of sodium oxalate in the sodium oxalate crystal suspension.

[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0025] The method for treating sodium oxalate waste residue in Bayer process alumina production provided in the embodiment of the present application is to leach the sodium oxalate in the sodium oxalate waste residue and then process it into a sodium oxalate crystal suspension, and then directly oxidize the sodium oxalate into sodium carbonate in the solution by oxygen in the presence of sodium hydroxide, with low energy consumption, low carbon emissions, high efficiency and simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0028] Figure 1 A schematic flow chart of a method for treating sodium oxalate waste residue in Bayer process alumina production provided in an embodiment of the present application. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0030] Unless otherwise specified, the terms used herein should be understood as commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. In the event of a conflict, this specification takes precedence.

[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0032] The existing sodium oxalate waste residue treatment process has technical problems such as high energy consumption and carbon emissions, low efficiency, and complex process.

[0033] The technical solution provided by the embodiments of the present application is to solve the above technical problems, and the overall idea is as follows:

[0034] The present application embodiment provides a method for treating sodium oxalate waste residue in Bayer process alumina production, and the method for treating sodium oxalate waste residue in Bayer process alumina production comprises the following steps:

[0035] S1: Leaching the sodium oxalate waste residue to obtain a sodium oxalate solution;

[0036] S2: concentrating the sodium oxalate solution to obtain a sodium oxalate crystal suspension;

[0037] S3: adding sodium hydroxide to the sodium oxalate crystal suspension to obtain an alkaline suspension;

[0038] S4: using oxygen as an oxidant, at a predetermined total gas pressure, a predetermined oxygen partial pressure and a predetermined temperature, the alkalized suspension is subjected to an oxidation reaction under the catalysis of a catalyst to obtain a sodium carbonate solution.

[0039] It is easy to understand that the purpose of the leaching treatment is to dissolve sodium oxalate into the solution. Those skilled in the art can select appropriate leaching conditions according to the properties of the sodium oxalate waste residue.

[0040] It is easy to understand that the purpose of concentrating the sodium oxalate solution until a large amount of sodium oxalate is precipitated to form a sodium oxalate crystal suspension is to allow the sodium oxalate in step S4 to contact with oxygen as much as possible. Step S4 requires a temperature increase reaction, and a higher temperature will rapidly increase the solubility of sodium oxalate. Step S2 processes the sodium oxalate solution into a sodium oxalate crystal suspension, in which the sodium oxalate crystals will further dissolve in step S4, increasing the concentration of sodium oxalate in the solution, thereby increasing the contact of sodium oxalate with oxygen.

[0041] It is easy to understand that after sodium hydroxide is added in step S3, sodium oxalate is oxidized in the presence of alkali in step S4, and the chemical reaction equation is:

[0042] 2Na 2 C 2 O 4 +O 2 +4NaOH==4Na 2 CO 3 +2H 2 O

[0043] It can be seen that the reaction products in step S4 are all sodium carbonate except water, and no carbon dioxide is emitted. Moreover, the oxidation reaction in step S4 is directly carried out in the solution, and the dissolved sodium carbonate can be directly recycled. In particular, for the Bayer process alumina production process, sodium carbonate can be directly causticized by calcium hydroxide to obtain sodium hydroxide, and the sodium hydroxide is returned to the Bayer process alumina production process.

[0044] The present application processes the sodium oxalate in the sodium oxalate waste residue to be leached and then processed into a sodium oxalate crystal suspension, and then the sodium oxalate is directly oxidized in the solution by oxygen under the condition of adding sodium hydroxide, which has low energy consumption, low carbon emission, high efficiency and simple process.

[0045] In some embodiments of the present application, the leaching treatment is performed using hot water at 90-98°C.

[0046] It is easy to understand that the beneficial effect of the leaching treatment using hot water at 90 to 98° C. is that sodium oxalate can be dissolved as quickly as possible through hot water leaching at this temperature, and the solubility of sodium oxalate is greater at high temperatures. The obtained sodium oxalate solution has a higher concentration. When concentrating the sodium oxalate solution in step S2, only a small amount of water needs to be removed to obtain a sodium oxalate crystal suspension, which is beneficial to increase work efficiency and reduce process energy consumption.

[0047] In some embodiments of the present application, the concentration of the sodium oxalate solution is 30-60 g / L.

[0048] It is easy to understand that the beneficial effect of the sodium oxalate solution having a concentration of 30 to 60 g / L is to ensure that the sodium oxalate concentration in the leachate does not exceed its saturation concentration, while improving the efficiency of the leaching process.

[0049] In some embodiments of the present application, the solid content of the sodium oxalate crystal suspension is 20-60 g / L.

[0050] It is easy to understand that the beneficial effect of the solid content of the sodium oxalate crystal suspension being 20 to 60 g / L is to maximize the efficiency of the sodium oxalate oxidation treatment process, while controlling the sodium carbonate concentration after the oxidation reaction not to exceed its saturation concentration, avoiding crystallization during the flash evaporation process of the solution, and ensuring stable operation of the production process.

[0051] In some embodiments of the present application, the oxidation reaction is carried out under the catalysis of a catalyst, and the catalyst is MnO 2 -CeO 2 catalyst.

[0052] Easy to understand, choose MnO 2 -CeO 2 The beneficial effect of the catalyst as a catalyst for the oxidation reaction is to accelerate the reaction rate of oxygen oxidation of sodium oxalate and improve the conversion rate of sodium oxalate.

[0053] In some embodiments of the present application, in the catalyst, MnO 2 and CeO 2 The molar ratio is 1 to 24:1; and / or,

[0054] The amount of the catalyst added is: 5 to 30 g of the catalyst per liter of the alkalized suspension.

[0055] As an example, MnO 2 and CeO 2 The molar ratio can be 1:1, 2:1, 4:1, 8:1, 16:1, 24:1.

[0056] As an example, the amount of catalyst added per liter of the alkalized suspension may be 5 g, 10 g, 15 g, 20 g, 25 g, or 30 g.

[0057] In some embodiments of the present application, the predetermined total gas pressure is 4-6.5 MPa; and / or,

[0058] The predetermined oxygen partial pressure is not less than 1 MPa; and / or,

[0059] The predetermined temperature is 180-260°C.

[0060] It is easy to understand that the beneficial effect of the predetermined total gas pressure of 4 to 6.5 MPa is to avoid boiling of the sodium oxalate suspension as much as possible by applying external pressure, and at the same time, there is no high requirement for the reaction equipment.

[0061] It is easy to understand that the predetermined oxygen partial pressure is not less than 1 MPa so as to dissolve as much oxygen as possible in the sodium oxalate suspension to accelerate the reaction rate.

[0062] It is easy to understand that the beneficial effect of the predetermined temperature of 180-260° C. is that it can ensure that the sodium oxalate oxidation reaction proceeds at a higher rate without placing high requirements on the reaction equipment.

[0063] As an example, the predetermined total air pressure may be 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa, 6 MPa, or 6.5 MPa.

[0064] As an example, the predetermined temperature may be 180°C, 200°C, 220°C, 240°C, or 260°C.

[0065] In some embodiments of the present application, the method for treating sodium oxalate waste residue in the Bayer process alumina production further comprises the following steps:

[0066] S5: flash evaporating the sodium carbonate solution to obtain a high-concentration sodium carbonate solution;

[0067] S6: After diluting and filtering the high-concentration sodium carbonate solution, the filtrate is subjected to causticizing treatment to obtain a caustic alkali solution.

[0068] It is easy to understand that the purpose of flash evaporation of the sodium carbonate solution is to remove volatile impurities in the sodium carbonate solution.

[0069] It is easy to understand that the purpose of diluting the high concentration sodium carbonate solution is to reduce the solution viscosity, increase the catalyst filtration rate, reduce the content of attached liquid in the filter cake, and meet the requirements of the subsequent causticizing process.

[0070] It is easy to understand that the caustic soda solution can be directly returned to the Bayer process for producing alumina.

[0071] In some embodiments of the present application, the concentration of the high concentration sodium carbonate solution is 150-210 g / L.

[0072] As an example, the concentration of the high concentration sodium carbonate solution can be 150 g / L, 170 g / L, 190 g / L, or 210 g / L.

[0073] In some embodiments of the present application, sodium hydroxide is added to the sodium oxalate crystal suspension, and the molar amount of the sodium hydroxide is not less than twice the molar amount of sodium oxalate in the sodium oxalate crystal suspension.

[0074] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0075] Example 1

[0076] Using hot water at 91°C to leach sodium oxalate solid waste residue produced by crystallization of Bayer process mother liquor to obtain a sodium oxalate solution with a sodium oxalate concentration of 40 g / L;

[0077] The sodium oxalate solution is evaporated and concentrated to obtain a sodium oxalate crystal suspension with a solid content of 20 g / L;

[0078] Adding a 32% sodium hydroxide solution to the sodium oxalate crystal suspension at a molar ratio of sodium oxalate: sodium hydroxide = 1:2, stirring evenly, and obtaining an alkaline suspension;

[0079] The alkaline suspension was transported into the high-pressure reactor by a high-pressure diaphragm pump, and oxygen with a purity of ≥99% was introduced into the high-pressure reactor. At the same time, 5 g / L of MnO 2 -CeO 2 The composite oxide catalyst, wherein in the catalyst, MnO 2 and CeO 2 The molar ratio of is 1:1, and an oxidation reaction is carried out for 3 hours under the conditions of controlling the total pressure of the high-pressure reactor to be 4.0 MPa, the oxygen partial pressure to be not less than 1.0 MPa and the temperature to be 180° C. to obtain a sodium carbonate solution;

[0080] After flash evaporation of the sodium carbonate solution, the temperature is reduced to below 100° C. to obtain a high-concentration sodium carbonate solution with a concentration of 150 g / L;

[0081] The high concentration sodium carbonate solution is diluted with water and filtered to obtain a catalyst filter cake and a filtrate. The catalyst filter cake is diluted with water to a slurry with a solid content of 250 g / L and then sent to a catalyst storage tank. The filtrate is sent to the causticizing process of alumina production for causticizing treatment.

[0082] Example 2

[0083] Using hot water at 96°C to leach sodium oxalate solid waste residue produced by crystallization of Bayer process mother liquor to obtain a sodium oxalate solution with a sodium oxalate concentration of 40 g / L;

[0084] The sodium oxalate solution is evaporated and concentrated to obtain a sodium oxalate crystal suspension with a solid content of 55 g / L;

[0085] Adding a 32% sodium hydroxide solution to the sodium oxalate crystal suspension at a molar ratio of sodium oxalate: sodium hydroxide = 1:2, stirring evenly, and obtaining an alkaline suspension;

[0086] The alkalized suspension was transported into a high-pressure reactor by a high-pressure diaphragm pump, oxygen with a purity of ≥99% was introduced into the high-pressure reactor, and 25 g / L of MnO was added by a high-pressure metering pump. 2 -CeO 2 The composite oxide catalyst, wherein in the catalyst, MnO 2 and CeO 2 The molar ratio of is 5:1, and an oxidation reaction is carried out for 3 hours under the conditions of controlling the total pressure of the high-pressure reactor to 4.5 MPa and the temperature to 180° C. to obtain a sodium carbonate solution;

[0087] After flash evaporation of the sodium carbonate solution, the temperature is reduced to below 100° C. to obtain a high-concentration sodium carbonate solution with a concentration of 185 g / L;

[0088] The high concentration sodium carbonate solution is diluted with water and filtered to obtain a catalyst filter cake and a filtrate. The catalyst filter cake is diluted with water to a solid content of 600 g / L slurry and then sent to a catalyst storage tank. The filtrate is sent to the causticizing process of alumina production for causticizing treatment.

[0089] Example 3

[0090] Using hot water at 90°C to leach sodium oxalate solid waste residue produced by crystallization of Bayer process mother liquor to obtain a sodium oxalate solution with a sodium oxalate concentration of 60 g / L;

[0091] The sodium oxalate solution is evaporated and concentrated to obtain a sodium oxalate crystal suspension with a solid content of 40 g / L;

[0092] Adding a 32% sodium hydroxide solution to the sodium oxalate crystal suspension at a molar ratio of sodium oxalate: sodium hydroxide = 1:2, stirring evenly, and obtaining an alkaline suspension;

[0093] The alkalized suspension was transported into the high-pressure reactor by a high-pressure diaphragm pump, oxygen with a purity of ≥99% was introduced into the high-pressure reactor, and 10 g / L of MnO was added by a high-pressure metering pump. 2 -CeO 2 The composite oxide catalyst, wherein in the catalyst, MnO 2 and CeO 2 The molar ratio of is 3:1, and the oxidation reaction is carried out for 3 hours under the conditions of controlling the total pressure of the high-pressure reactor to 5.5 MPa and the temperature to 230° C. to obtain a sodium carbonate solution;

[0094] After flash evaporation of the sodium carbonate solution, the temperature is reduced to below 100° C. to obtain a high-concentration sodium carbonate solution with a concentration of 192 g / L;

[0095] The high concentration sodium carbonate solution is diluted with water and filtered to obtain a catalyst filter cake and a filtrate. The catalyst filter cake is diluted with water to a solid content of 400 g / L slurry and then sent to a catalyst storage tank. The filtrate is sent to the causticizing process of alumina production for causticizing treatment.

[0096] Example 4

[0097] Using hot water at 94°C to leach sodium oxalate solid waste residue produced by crystallization of Bayer process mother liquor to obtain a sodium oxalate solution with a sodium oxalate concentration of 50 g / L;

[0098] The sodium oxalate solution is evaporated and concentrated to obtain a sodium oxalate crystal suspension with a solid content of 30 g / L;

[0099] Adding a 32% sodium hydroxide solution to the sodium oxalate crystal suspension at a molar ratio of sodium oxalate: sodium hydroxide = 1:2, stirring evenly, and obtaining an alkaline suspension;

[0100] The alkaline suspension was transported into the high-pressure reactor by a high-pressure diaphragm pump, oxygen with a purity of ≥99% was introduced into the high-pressure reactor, and 30 g / L of MnO was added by a high-pressure metering pump. 2 -CeO 2 The composite oxide catalyst, wherein in the catalyst, MnO 2 and CeO 2 The molar ratio of is 9:1, and the oxidation reaction is carried out for 2 hours under the conditions of controlling the total pressure of the high-pressure reactor to 6.0 MPa and the temperature to 250° C. to obtain a sodium carbonate solution;

[0101] After flash evaporation of the sodium carbonate solution, the temperature is reduced to below 100° C. to obtain a high-concentration sodium carbonate solution with a concentration of 190 g / L;

[0102] The high concentration sodium carbonate solution is diluted with water and filtered to obtain a catalyst filter cake and a filtrate. The catalyst filter cake is diluted with water to a slurry with a solid content of 500 g / L and then sent to a catalyst storage tank. The filtrate is sent to the causticizing process of alumina production for causticizing treatment.

[0103] Example 5

[0104] Using hot water at 93°C to leach sodium oxalate solid waste residue produced by crystallization of Bayer process mother liquor to obtain a sodium oxalate solution with a sodium oxalate concentration of 40 g / L;

[0105] The sodium oxalate solution is evaporated and concentrated to obtain a sodium oxalate crystal suspension with a solid content of 30 g / L;

[0106] Adding a 32% sodium hydroxide solution to the sodium oxalate crystal suspension at a molar ratio of sodium oxalate: sodium hydroxide = 1:2, stirring evenly, and obtaining an alkaline suspension;

[0107] The alkaline suspension was transported into the high-pressure reactor by a high-pressure diaphragm pump, and oxygen with a purity of ≥99% was introduced into the high-pressure reactor. At the same time, 5 g / L of MnO 2 -CeO 2 The composite oxide catalyst, wherein in the catalyst, MnO 2 and CeO 2 The molar ratio of is 14:1, and the oxidation reaction is carried out for 3 hours under the conditions of controlling the total pressure of the high-pressure reactor to 5.9 MPa and the temperature to 240° C. to obtain a sodium carbonate solution;

[0108] After flash evaporation of the sodium carbonate solution, the temperature is reduced to below 100° C. to obtain a high-concentration sodium carbonate solution with a concentration of 180 g / L;

[0109] The high concentration sodium carbonate solution is diluted with water and filtered to obtain a catalyst filter cake and a filtrate. The catalyst filter cake is diluted with water to a slurry with a solid content of 500 g / L and then sent to a catalyst storage tank. The filtrate is sent to the causticizing process of alumina production for causticizing treatment.

[0110] Example 6

[0111] Using hot water at 98°C to leach sodium oxalate solid waste residue produced by crystallization of Bayer process mother liquor to obtain a sodium oxalate solution with a sodium oxalate concentration of 45 g / L;

[0112] The sodium oxalate solution is evaporated and concentrated to obtain a sodium oxalate crystal suspension with a solid content of 55 g / L;

[0113] Adding a 32% sodium hydroxide solution to the sodium oxalate crystal suspension at a molar ratio of sodium oxalate: sodium hydroxide = 1:2, stirring evenly, and obtaining an alkaline suspension;

[0114] The alkaline suspension was transported into the high-pressure reactor by a high-pressure diaphragm pump, oxygen with a purity of ≥99% was introduced into the high-pressure reactor, and 15 g / L of MnO was added by a high-pressure metering pump. 2 -CeO 2 The composite oxide catalyst, wherein in the catalyst, MnO 2 and CeO 2 The molar ratio of is 22:1, and the oxidation reaction is carried out for 1 hour under the conditions of controlling the total pressure of the high-pressure reactor to 6.5 MPa and the temperature to 260° C. to obtain a sodium carbonate solution;

[0115] After flash evaporation of the sodium carbonate solution, the temperature is reduced to below 100° C. to obtain a high-concentration sodium carbonate solution with a concentration of 208 g / L;

[0116] The high concentration sodium carbonate solution is diluted with water and filtered to obtain a catalyst filter cake and a filtrate. The catalyst filter cake is diluted with water to a slurry with a solid content of 500 g / L and then sent to a catalyst storage tank. The filtrate is sent to the causticizing process of alumina production for causticizing treatment.

[0117] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0118] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present application specification, the terms "including", "comprising", etc. refer to "including but not limited to". Moreover, the terms "including", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "including..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. For the association relationship of more than three associated objects described by "and / or", it means that any one of these three associated objects can exist alone, or any at least two of them exist at the same time. For example, for A, and / or B, and / or C, it can be represented that any one of A, B, and C exists alone, or any two of them exist at the same time, or three of them exist at the same time. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single (individual) or plural (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, wherein a, b, and c can be single or multiple, respectively.

[0119] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for treating sodium oxalate waste residue in Bayer process alumina production, characterized in that: The method for treating sodium oxalate waste residue in the Bayer process alumina production comprises the following steps: Leaching the sodium oxalate waste residue to obtain a sodium oxalate solution; Concentrating the sodium oxalate solution to obtain a sodium oxalate crystal suspension; adding sodium hydroxide to the sodium oxalate crystal suspension to obtain an alkaline suspension; Oxygen is used as an oxidant, and the alkalized suspension is subjected to an oxidation reaction under the catalysis of a catalyst at a predetermined total gas pressure, a predetermined oxygen partial pressure, and a predetermined temperature to obtain a sodium carbonate solution.

2. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, characterized in that: The leaching treatment is performed using hot water at 90 to 98°C.

3. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, characterized in that: The concentration of the sodium oxalate solution is 30-60 g / L.

4. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, characterized in that: The solid content of the sodium oxalate crystal suspension is 20-60 g / L.

5. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, wherein the catalyst is a MnO2-CeO2 composite oxide catalyst.

6. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 5, characterized in that: In the catalyst, the molar ratio of MnO2 to CeO2 is 1 to 24:1; and / or, The amount of the catalyst added is: 5 to 30 g of the catalyst per liter of the alkalized suspension.

7. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, characterized in that: The predetermined total gas pressure is 4-6.5 MPa; and / or, The predetermined oxygen partial pressure is not less than 1 MPa; and / or, The predetermined temperature is 180-260°C.

8. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, characterized in that: The method for treating sodium oxalate waste residue in the Bayer process alumina production also includes the following steps: Flash evaporating the sodium carbonate solution to obtain a high-concentration sodium carbonate solution; After diluting and filtering the high-concentration sodium carbonate solution, the filtrate is subjected to causticizing treatment to obtain caustic alkali solution.

9. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 8, characterized in that: The concentration of the high-concentration sodium carbonate solution is 150-210 g / L.

10. The method for treating sodium oxalate waste residue in Bayer process alumina production according to claim 1, characterized in that: The sodium hydroxide is added to the sodium oxalate crystal suspension, and the molar amount of the sodium hydroxide is not less than twice the molar amount of the sodium oxalate in the sodium oxalate crystal suspension.