Method for preparing battery-grade lithium carbonate by one-step method

The one-step method of preparing battery-grade lithium carbonate simplifies the process flow, improves production efficiency and purity, solves the problems of high cost and low efficiency in traditional processes, and achieves efficient lithium carbonate production.

CN118754165APending Publication Date: 2024-10-11JIANGXI JINSHANG LI NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410920461.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The traditional production process of battery-grade lithium carbonate is complex, high-cost, low-efficiency, and requires secondary processing, resulting in large equipment footprint and high labor costs.

Method used

A one-step method is used to prepare battery-grade lithium carbonate. By performing a lithium precipitation reaction between lithium sulfate solution and sodium carbonate solution at high temperature, combined with precision filtration, washing and airflow crushing, the process is simplified, production costs are reduced, and production efficiency is improved.

Benefits of technology

Efficient preparation of battery-grade lithium carbonate is achieved, with a purity of more than 99.6%, and a comprehensive recovery rate of lithium of more than 93%, simplifying the process and reducing equipment footprint and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754165A_ABST
    Figure CN118754165A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing battery-grade lithium carbonate by a one-step method, and belongs to the technical field of preparation of battery-grade lithium carbonate. The method comprises the following steps: by taking a lithium sulfate solution as a raw material, carrying out impurity removal and purification through ion exchange to obtain a refined lithium sulfate solution, and mixing the refined lithium sulfate solution with a sodium carbonate solution to carry out lithium precipitation reaction; the method comprises the following steps: preparing lithium carbonate, lithium sulfate, sodium carbonate and sodium sulfate into a mixed slurry, introducing the mixed slurry into equipment for preparing battery-grade lithium carbonate by a one-step method, washing, filtering, drying, and carrying out air jet pulverization to obtain battery-grade lithium carbonate, thereby solving the problems that industrial-grade lithium carbonate is firstly produced and then secondary processing is carried out through carbonization in the traditional lithium carbonate process; according to the method, the technical process is effectively simplified, the occupied area of equipment is reduced, the production cost is reduced, the production efficiency is improved, the comprehensive recovery rate of lithium can reach 93% or above, and the purity of the battery-grade lithium carbonate produced through the method reaches 99.6% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of battery-grade lithium carbonate, and specifically relates to a method for preparing battery-grade lithium carbonate in one step. Background Art

[0002] Lithium carbonate is an inorganic compound with the chemical formula Li2CO3 and a molecular weight of 73.89. It is a colorless monoclinic crystal that is slightly soluble in water and dilute acid, but insoluble in ethanol and acetone. Its thermal stability is lower than that of carbonates of other elements in the same group in the periodic table. It does not deliquesce in the air and can be obtained by adding sodium carbonate to lithium sulfate or lithium oxide solution. Its aqueous solution can be converted into an acid salt by passing carbon dioxide into it, and hydrolysis occurs when it is boiled. Lithium carbonate can be used in the manufacture of lithium compounds, enamel, and glass. It is a raw material for the preparation of lithium compounds and metallic lithium, and can be used as an electrolytic bath additive for aluminum smelting. It is widely used in industries such as glass, ceramics, medicine, and food. It can also be used in synthetic rubber, dyes, semiconductors, military defense industry, televisions, atomic energy, medicine, catalysts, etc. It has a wide range of uses. However, the traditional production process of battery-grade lithium carbonate is to first produce industrial-grade lithium carbonate and then perform secondary processing through carbonization, which leads to high production costs, low production efficiency, complicated preparation processes, large equipment footprint, and frequent manual transportation of materials, resulting in high labor costs. Summary of the invention

[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a one-step method for preparing battery-grade lithium carbonate, which effectively simplifies the process flow, reduces the equipment footprint, reduces production costs, and improves production efficiency.

[0004] The above technical purpose of the present invention is achieved by the following technical scheme: a one-step method for preparing battery-grade lithium carbonate comprises the following steps:

[0005] 1) passing the crude lithium sulfate solution into a de-impurity kettle, adding sodium hydroxide to adjust the pH to 11-13, filtering, and sampling to detect the calcium and magnesium content in the solution;

[0006] 2) adding sodium carbonate according to the calcium and magnesium content, and after the heating reaction is completed, obtaining a refined lithium sulfate solution by precise filtration;

[0007] 3) Add sodium carbonate solution to the lithium precipitation kettle, add sodium hydroxide to adjust the pH to 12-14, heat to 90-100° C., slowly drop the refined lithium sulfate solution into the lithium precipitation kettle, stir and mix with the high-temperature sodium carbonate solution to carry out lithium precipitation reaction, keep the temperature at 90-100° C. throughout the process, stir and keep the temperature after all the lithium sulfate solution has been added, and then pass it into the equipment for preparing battery-grade lithium carbonate by one-step method;

[0008] 4) Filtering in the equipment, washing after filtering, drying the material after each washing, controlling the moisture content at 7-10%, and completely drying after washing, with the moisture content below 0.2%, passing through the air flow mill for crushing, and the mother liquor after filtration is concentrated by MVR and passed through the impurity removal kettle as raw material for circulation;

[0009] 5) The dried material is crushed and demagnetized in a jet mill to a particle size of D10 ≥ 1 μm, 3 μm ≤ D50 ≤ 8 μm, 9 μm ≤ D90 ≤ 15 μm; after the crushing is completed, the material is packed in bags, and the obtained product is battery-grade lithium carbonate.

[0010] Preferably, the reaction time in step 1) is 30-60 min, and the lithium content in the lithium sulfate solution after the reaction is ≥10 g / L.

[0011] Preferably, in step 2), the molar ratio of the total amount of calcium and magnesium to sodium carbonate is 1:1.2-1.5.

[0012] Preferably, the heating reaction conditions in step 2) are a temperature of 80-90° C. and a reaction time of 30-60 min.

[0013] Preferably, the dropping speed of the high temperature sodium carbonate in step 3) is 2-3m 3 / h, reaction time 30-60min.

[0014] Preferably, in step 3), the concentration of the sodium carbonate solution is 2.5-3.5 mol / L, and the molar ratio of sodium carbonate to lithium sulfate is 1:1-1.5.

[0015] Preferably, the concentration of sodium hydroxide in step 3) is 0.001-0.01 mol / L.

[0016] Preferably, in step 4), the washing temperature is 95-105°C, the washing solid-liquid ratio is 1:5-8, the washing times are 3-5 times, the water from the first washing is used to prepare the alkali solution, and the water from the remaining washing stages is used for backwashing to reduce the amount of pure water used and discharge, and the last washing is done with pure water.

[0017] Preferably, after the pulverization in step 5), the particle size of the battery-grade lithium carbonate is D10 ≥ 1 μm, 3 μm ≤ D50 ≤ 8 μm, and 9 μm ≤ D90 ≤ 15 μm.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] The method of the present invention uses lithium sulfate solution as a raw material, removes impurities and purifies it through ion exchange to obtain a refined lithium sulfate solution, and then mixes it with a sodium carbonate solution to perform lithium precipitation reaction to obtain a mixed slurry of lithium carbonate, lithium sulfate, sodium carbonate and sodium sulfate, and then passes it into a one-step method for preparing battery-grade lithium carbonate, washes, filters and dries it, and then pulverizes it through air flow to obtain battery-grade lithium carbonate. This solves the problem that the traditional lithium carbonate process first produces industrial-grade lithium carbonate and then performs secondary processing through carbonization, resulting in high production costs, low production efficiency and the like. The method effectively simplifies the process flow, reduces the equipment footprint, reduces production costs, and improves production efficiency. The comprehensive recovery rate of lithium by the method of the present invention can reach more than 93%, and the purity of the battery-grade lithium carbonate produced by the method of the present invention reaches more than 99.6%. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is the overall structure diagram of the device of the present invention;

[0021] Figure 2 It is a cross-sectional structural diagram of the tank body of the present invention;

[0022] Figure 3 for Figure 2 A magnified view of point A;

[0023] In the figure: 1, tank body; 101, electromagnet; 2, motor; 3, stirring rod; 4, lifting mechanism; 5, feed port; 6, dust collector; 7, liquid inlet; 8, air inlet; 9, discharge port; 10, sampling port; 11, waste outlet; 12, support foot; 13, stirring blade; 14, supporting mesh plate; 15, filter cloth; 16, spray infusion tube; 17, spray head; 18, installation slot; 19, pressure regulating tube; 20, liner; 2001, fixed heat conduction ring; 2002, connector; 2003, heat conduction pipe; 2004, electric heating iron sheet; 2005, heat dissipation fin; 2006, elastic ring. DETAILED DESCRIPTION

[0024] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies realized based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0025] Example 1

[0026] The one-step method for preparing battery-grade lithium carbonate comprises the following steps:

[0027] 1) Passing the crude lithium sulfate solution into a de-impurity kettle, adding sodium hydroxide to adjust the pH to 12, the reaction time is 45 min, after the reaction, the lithium content in the lithium sulfate solution is ≥10 g / L, filtering, sampling and detecting the calcium and magnesium content in the solution;

[0028] 2) Sodium carbonate is added according to the calcium and magnesium content, the molar ratio of the total amount of calcium and magnesium to sodium carbonate is 1:1.5, the heating temperature is increased to 80°C, the reaction time is 40 minutes, and after the heating reaction is completed, a refined lithium sulfate solution is obtained by precision filtration;

[0029] 3) adding sodium carbonate solution with a concentration of 2.5 mol / L into the lithium precipitation kettle, heating to 90° C., adding sodium hydroxide with a concentration of 0.005 mol / L to adjust the pH of the alkali solution to 13, slowly dropping the refined lithium sulfate solution into the lithium precipitation kettle, with a molar ratio of sodium carbonate to lithium sulfate of 1:1.5, stirring and mixing with the high-temperature sodium carbonate solution to carry out lithium precipitation reaction, keeping the temperature at 90° C. throughout the process, stirring and keeping the temperature after all the lithium sulfate solution has been dropped, and then passing into the equipment for preparing battery-grade lithium carbonate by one-step method;

[0030] 4) Filtering in a one-step method for preparing battery-grade lithium carbonate, washing after filtering, the washing temperature is 95° C., the washing solid-liquid ratio is 1:8, the washing number is 5 times, and the material is dried after each washing, the moisture content is controlled at 10%, and the material is completely dried after washing, the moisture content is below 0.2%, and the material is passed into a jet mill for crushing. The mother liquor filtered from the lithium precipitation end is concentrated by MVR and then passed into the front impurity removal kettle as a raw material for circulation. The first washing water can be used to prepare alkali solution, and the remaining washing water is used for backwashing to reduce the amount of pure water and discharge. The last washing needs to be washed with pure water;

[0031] 5) The dried material is crushed and demagnetized in a jet mill to a particle size of D10 ≥ 1 μm, 3 μm ≤ D50 ≤ 8 μm, 9 μm ≤ D90 ≤ 15 μm; after the crushing is completed, the material is packed in bags, and the obtained product is battery-grade lithium carbonate.

[0032] Example 2

[0033] The one-step method for preparing battery-grade lithium carbonate comprises the following steps:

[0034] 1) Passing the crude lithium sulfate solution into a de-impurity kettle, adding sodium hydroxide to adjust the pH to 12, the reaction time is 45 min, after the reaction, the lithium content in the lithium sulfate solution is ≥10 g / L, filtering, sampling and detecting the calcium and magnesium content in the solution;

[0035] 2) Sodium carbonate is added according to the calcium and magnesium content, the molar ratio of the total amount of calcium and magnesium to sodium carbonate is 1:1.4, the heating temperature is increased to 85°C, the reaction time is 40 minutes, and after the heating reaction is completed, a refined lithium sulfate solution is obtained by precision filtration;

[0036] 3) adding sodium carbonate solution with a concentration of 3 mol / L into the lithium precipitation kettle, heating to 90° C., adding sodium hydroxide with a concentration of 0.005 mol / L to adjust the pH of the alkali solution to 13, slowly dropping the refined lithium sulfate solution into the lithium precipitation kettle, with a molar ratio of sodium carbonate to lithium sulfate of 1:1.4, stirring and mixing with the high-temperature sodium carbonate solution to perform lithium precipitation reaction, and keeping the temperature at 90° C. throughout the process, stirring and keeping the temperature after all the lithium sulfate solution has been dropped, and then passing into the equipment for preparing battery-grade lithium carbonate by one-step method;

[0037] 4) Filtering in a one-step method for preparing battery-grade lithium carbonate, washing after filtering, the washing temperature is 95° C., the washing solid-liquid ratio is 1:8, the washing number is 4 times, and the material is dried after each washing, the moisture content is controlled at 10%, and the material is completely dried after washing, the moisture content is below 0.2%, and the material is passed into a gas flow mill for crushing. The mother liquor filtered at the lithium precipitation end is concentrated by MVR and then passed into the front impurity removal kettle as a raw material for circulation. The first washing water can be used to prepare alkali solution, and the remaining washing water is used for backwashing to reduce the amount of pure water and discharge. The last washing needs to be washed with pure water;

[0038] 5) The dried material is crushed and demagnetized in a jet mill to a particle size of D10 ≥ 1 μm, 3 μm ≤ D50 ≤ 8 μm, 9 μm ≤ D90 ≤ 15 μm; after the crushing is completed, the material is packed in bags, and the obtained product is battery-grade lithium carbonate.

[0039] Example 3

[0040] The one-step method for preparing battery-grade lithium carbonate comprises the following steps:

[0041] 1) Passing the crude lithium sulfate solution into a de-impurity kettle, adding sodium hydroxide to adjust the pH to 12, the reaction time is 45 min, after the reaction, the lithium content in the lithium sulfate solution is ≥10 g / L, filtering, sampling and detecting the calcium and magnesium content in the solution;

[0042] 2) Sodium carbonate is added according to the calcium and magnesium content, the molar ratio of the total amount of calcium and magnesium to sodium carbonate is 1:1.3, the heating temperature is increased to 90°C, the reaction time is 40 minutes, and after the heating reaction is completed, a refined lithium sulfate solution is obtained by precision filtration;

[0043] 3) adding sodium carbonate solution with a concentration of 2.5 mol / L to the lithium precipitation kettle, heating to 90° C., adding sodium hydroxide with a concentration of 0.005 mol / L to adjust the pH of the alkali solution to 13, slowly dropping the refined lithium sulfate solution into the lithium precipitation kettle, with a molar ratio of sodium carbonate to lithium sulfate of 1:1.3, stirring and mixing with the high-temperature sodium carbonate solution to perform lithium precipitation reaction, and keeping the temperature at 90° C. throughout the process, stirring and keeping the temperature to react after all the lithium sulfate solution has been dropped, and then passing into the equipment for preparing battery-grade lithium carbonate by one-step method;

[0044] 4) Filtering in a one-step method for preparing battery-grade lithium carbonate, washing after filtering, the washing temperature is 95° C., the washing solid-liquid ratio is 1:6, the washing number is 5 times, and the material is dried after each washing, the moisture content is controlled at 8%, and the material is completely dried after washing, the moisture content is below 0.2%, and the material is passed into a gas flow mill for crushing. The mother liquor filtered from the lithium precipitation end is concentrated by MVR and then passed into the front impurity removal kettle as a raw material for circulation. The first washing water can be used to prepare alkali solution, and the remaining washing water is used for backwashing to reduce the amount of pure water and discharge. The last washing needs to be washed with pure water;

[0045] 5) The dried material is crushed and demagnetized in a jet mill to a particle size of D10 ≥ 1 μm, 3 μm ≤ D50 ≤ 8 μm, 9 μm ≤ D90 ≤ 15 μm; after the crushing is completed, the material is packed in bags, and the obtained product is battery-grade lithium carbonate.

[0046] The equipment for preparing battery-grade lithium carbonate in one step in Examples 1-3 of the present invention is as follows Figure 1-3 As shown, the tank body (1) comprises a tank body (1), a motor (2) arranged on the tank body (1), a stirring rod (3) arranged on the power output end of the motor (2) and extending into the tank body (1), a stirring blade (13) arranged on the stirring rod (3), and a feed inlet (5), a liquid inlet (7), a discharge port (9) and a waste outlet (11) opened on the tank body (1), the tank body (1) is provided with a lifting mechanism (4), the motor (2) is arranged on the lifting mechanism (4), and under the driving action of the lifting mechanism (4), the stirring rod (3) can be axially moved up and down inside the tank body (1). The tank body (1) is movable, a spray infusion pipe (16) connected to the liquid inlet (7) is provided at the top of the tank body (1), and a plurality of spray heads (17) are installed on the spray infusion pipe (16). A filtering mechanism is provided at the bottom of the tank body (1), and the filtering mechanism comprises a supporting mesh plate (14) and a filter cloth (15) detachably arranged on the supporting mesh plate (14). A lifting mechanism (4) is provided on the tank body (1), and the motor (2) is arranged on the lifting mechanism (4). Under the driving action of the lifting mechanism (4), the stirring rod (3) can move up and down along the axial direction inside the tank body (1).

[0047] An annular mounting groove (18) is provided on the inner wall of the tank body (1), a plurality of electromagnets (101) are embedded in the side wall of the mounting groove (18), an inner liner (20) having a cylindrical structure with openings at both ends is sealedly embedded in the mounting groove (18), the inner wall of the inner liner (20) is flush with the inner wall of the tank body (1), and an annular closed cavity is formed between the two;

[0048] The inner container (20) comprises a plurality of fixed heat-conducting rings (2001) and a plurality of elastic rings (2006) connected in alternating layers, the fixed heat-conducting rings (2001) being fixedly mounted on the tank body (1) via a connecting piece (2002), a plurality of heat-conducting tubes (2003) being arranged around and in close contact with the outer wall of the fixed heat-conducting ring (2001), a plurality of electric heating iron sheets (2004) being embedded in a circular array on the elastic ring (2006), the positions of the plurality of electric heating iron sheets (2004) corresponding to the positions of the plurality of electromagnets (101) one by one, and a heat dissipation fin (2005) being arranged on one side of the electric heating iron sheet (2004) facing the axis of the elastic ring (2006);

[0049] A pressure regulating tube (19) is provided on one side of the tank body (1), one end of the pressure regulating tube (19) is connected to the air pressure regulating mechanism, and the other end is branched into a plurality of output ends extending into the installation groove (18), and the output ends of the pressure regulating tube (19) are distributed at the upper and lower ends of each electromagnet (101).

[0050] The method of using the equipment for preparing battery-grade lithium carbonate in one step is as follows:

[0051] S1, injecting a solid-liquid mixture containing lithium carbonate solid and impurities into the tank body 1 through the feed port 5, and allowing it to stand to separate the solid and liquid;

[0052] S2, opening the waste outlet 11, filtering out the waste liquid in the solid-liquid mixture in step S1 under the filtering action of the filtering mechanism, and obtaining the impure and moist lithium carbonate solid. At this time, the impure and moist lithium carbonate solid is retained on the filtering mechanism, and the filtering operation is completed;

[0053] S3, injecting the impurity solvent into the spraying liquid infusion pipe 16 through the liquid inlet 7, and then spraying it outward from the spray head 17;

[0054] S4, start the motor 2, drive the stirring rod 3 and the stirring blade 13 to stir the material through the motor 2, and continue stirring until the impurities are completely dissolved, and then open the waste outlet 11 to discharge the waste liquid to obtain wet lithium carbonate solid. At this time, the wet lithium carbonate solid is retained on the filtering mechanism, and the washing operation is completed;

[0055] S5, a heat medium is introduced into the heat pipe 2003, and the heat medium can be hot steam or steam condensed water generated by the evaporator in the workshop, and the waste heat of the condensed water is used to generate heat, and the electric heating iron sheet 2004 is powered on to generate heat, and at the same time, the motor 2 is kept turned on, and the material is continuously stirred by the stirring blade 13 until the lithium carbonate is completely dried, and the drying operation is completed;

[0056] S6, open the discharge port 9 to discharge the material.

[0057] Through testing, the technical indicators of battery-grade lithium carbonate prepared by the method embodiment 1 of the present invention are as follows in Table 1:

[0058] Table 1

[0059]

[0060] Each metal element in the above table exists in the form of ions.

[0061] It can be seen from Table 1 that the comprehensive recovery rate of lithium using the method of the present invention can reach more than 93%, and the purity of battery-grade lithium carbonate produced by the method can reach more than 99.6%.

[0062] The above descriptions are merely embodiments of the present invention. It should be pointed out that, for those skilled in the art, various changes, modifications, substitutions and variations can be made to these embodiments without departing from the technical principles of the present invention. These changes, modifications, substitutions and variations should also be regarded as the scope of protection of the present invention.

Claims

1. A one-step method for preparing battery-grade lithium carbonate, It is characterized in that The following steps are involved: 1) Pass the crude lithium sulfate solution into the impurity removal kettle, add sodium hydroxide to adjust the pH to 11-13, filter, and take samples to detect the calcium and magnesium content in the solution; 2) Sodium carbonate is added according to the calcium and magnesium content. After the heating reaction is completed, refined lithium sulfate solution is obtained by precise filtration; 3) Add sodium carbonate solution to the lithium precipitation kettle, add sodium hydroxide to adjust the pH to 12-14, heat to 90-100°C, slowly drop the refined lithium sulfate solution into the lithium precipitation kettle, stir and mix with the high-temperature sodium carbonate solution to react with lithium precipitation, keep the temperature at 90-100°C throughout the process, stir and keep the temperature after all the lithium sulfate solution has been added, and then pass it into the equipment for preparing battery-grade lithium carbonate in one step; 4) Filter in a one-step process for preparing battery-grade lithium carbonate, wash after filtration, dry the material after each washing, control the moisture content at 7-10%, and completely dry after washing, with the moisture content below 0.2%, pass through a jet mill for crushing, and the mother liquor after filtration is concentrated by MVR and passed through a decontamination kettle as a raw material for circulation; 5) The dried material is crushed and demagnetized in a jet mill. After the crushing is completed, it is packaged in bags. The obtained product is battery-grade lithium carbonate.

2. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that The reaction time in step 1) is 30-60 minutes, and the lithium content in the lithium sulfate solution after the reaction is ≥10 g / L.

3. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that In the step 2), the molar ratio of the total amount of calcium and magnesium to sodium carbonate is 1:1.2-1.

5.

4. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that The heating reaction conditions in step 2) are a temperature of 80-90° C. and a reaction time of 30-60 min.

5. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that In step 3), the dropping speed of high-temperature sodium carbonate is 2-3 m³ / h, and the reaction time is 30-60 min.

6. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that In step 3), the concentration of the sodium carbonate solution is 2.5-3.5 mol / L, and the molar ratio of sodium carbonate to lithium sulfate is 1:1-1.

5.

7. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that In the step 3), the concentration of sodium hydroxide is 0.001-0.01 mol / L.

8. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that In step 4), the washing temperature is 95-105°C, the washing solid-liquid ratio is 1:5-8, the washing times are 3-5 times, the first washing water is used to prepare the alkali solution, and the remaining washing water is used for backwashing to reduce the amount of pure water and discharge, and the last washing is washed with pure water.

9. The method for preparing battery-grade lithium carbonate in one step according to claim 1, It is characterized in that After the pulverization in step 5), the particle size of the battery-grade lithium carbonate is D10 ≥ 1 μm, 3 μm ≤ D50 ≤ 8 μm, and 9 μm ≤ D90 ≤ 15 μm.

Citation Information

Cited By

  • Metal ion leaching process optimization process

    CN122791178A