A two-step calcination method for preferentially extracting lithium from the positive electrode of waste lithium-ion batteries

The two-step roasting method was used to calcinate and precipitate the positive electrode material of the lithium-ion battery with ammonium sulfate, which solved the problems of low lithium extraction rate and pollution in lithium-ion battery recycling, and realized the preparation and environmental protection process of high-purity lithium carbonate.

CN117049575BActive Publication Date: 2024-11-15ANHUI CHAOYUE ENVIRONMENTAL TECH CO LTD +3

Patent Information

Application Number
CN202311097108.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-28
Publication Date
2024-11-15
Estimated Expiration
2043-08-28

AI Technical Summary

Technical Problem

In the existing lithium-ion battery recycling technology, lithium recycling operations are complicated, which will cause gas pollution, low lithium ion extraction rate and low purity.

Method used

Using a two-step roasting method, first mix the positive electrode material with ammonium sulfate for the first stage roasting, then raise the temperature for the second stage roasting, obtain a lithium-rich solution through water immersion and precipitation reaction and filter it, and finally obtain high carbonate ions. Lithium carbonate of purity.

Benefits of technology

High lithium selectivity and extraction rate are achieved, the energy demand for subsequent evaporation and crystallization is reduced, and the release of polluted gas is reduced. The obtained lithium carbonate is highly purified and the process is environmentally friendly and clean.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117049575B_ABST
    Figure CN117049575B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method, and belongs to the technical field of lithium recovery. A method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method comprises the following steps: roasting a positive electrode material and ammonium sulfate after mixing to obtain a first roasting product; roasting at a high temperature to obtain a second roasting product; filtering, evaporating and crystallizing the second roasting product after water leaching to obtain a lithium-rich solution and a slag phase; adding a precipitant to the lithium-rich solution, and filtering to obtain lithium carbonate. The method of the present invention uses ammonium sulfate as a roasting agent to convert part of the positive electrode material into sulfate, and the intermediate product of the temperature rise, the transition metal sulfate, is used as a roasting agent to react with the unreacted positive electrode material to generate water-soluble lithium sulfate and water-insoluble transition metal oxides, and preferential lithium extraction is achieved after water leaching. The preparation method is simple, consumes less ammonium sulfate, and does not generate polluting gases; the lithium extraction rate and selectivity are high, and the obtained lithium carbonate has high purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium recovery, and specifically relates to a method for preferentially extracting lithium from a positive electrode of a waste lithium-ion battery by a two-step roasting method. Background Art

[0002] The positive electrode of a waste lithium-ion battery refers to the positive electrode material in the battery, which is usually a composite material made of lithium compounds (such as oxides, phosphates, etc.) mixed with other metals (such as cobalt, manganese, nickel, etc.). The positive electrode is an important component of a lithium-ion battery, responsible for storing and releasing lithium ions, and participating in the battery's charging and discharging process.

[0003] Discarded lithium-ion battery positive electrodes usually contain valuable metal elements that can be recovered, such as lithium, cobalt, nickel, etc. When recycling and processing discarded batteries, the positive electrodes are usually separated and processed to recover the valuable elements and materials in them. Recycling battery positive electrode materials helps reduce the demand for raw materials, save resources, and also reduce the negative impact on the environment. Through proper recycling and processing, the valuable elements in the discarded lithium-ion battery positive electrodes can be reused to manufacture new batteries or other applications.

[0004] The process of recycling lithium from the cathode involves the following steps:

[0005] 1. Collect discarded lithium-ion batteries: Discarded lithium-ion batteries can be collected from electronic waste recycling stations, recycling centers or specialized waste recycling agencies.

[0006] 2. Separation of positive electrode: After pre-treatment, the discarded batteries can be separated to remove the positive electrode from the battery. Usually mechanical crushing, chemical dissolution or heat treatment methods are used for separation.

[0007] 3. Extraction of lithium: The separated positive electrode can be processed under corresponding process conditions to extract the lithium metal therein. Some common extraction methods include leaching, electrolysis and heat treatment.

[0008] 4. Lithium purification and reuse: The extracted lithium metal needs to go through a purification process to remove other impurities. The purified lithium can be used to prepare new lithium-ion batteries or for other lithium-related applications.

[0009] Sulfate roasting is a commonly used method for recovering lithium from lithium-ion batteries. In the prior art, lithium, cobalt, nickel, and manganese are often converted into lithium sulfate, cobalt sulfate, nickel sulfate, and manganese sulfate at the same time by adding an excessive amount of roasting agent. Subsequently, lithium, cobalt, nickel, and manganese are leached into the solution by water immersion, and then calcium hydroxide or calcium oxide is added to precipitate the cobalt, nickel, and manganese ions in the solution, and finally sodium carbonate is added to the solution to synthesize lithium carbonate. First, the above method consumes a lot of roasting agents, and polluting gases such as ammonia and sulfur dioxide are generated during the roasting process; secondly, lithium ions will inevitably be taken away during the first precipitation of cobalt, nickel, and manganese ions, resulting in a low extraction rate of lithium ions, and the obtained lithium carbonate is easily mixed with impurity cations, resulting in a low purity of lithium carbonate. Summary of the invention

[0010] The present invention provides a method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method, so as to solve the technical problems in the prior art that the lithium recovery operation is complicated, gas pollution is generated, the lithium ion extraction rate is low, and the purity is low.

[0011] In order to solve the above-mentioned invention object, the technical solution provided by the present invention is as follows:

[0012] A method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method comprises the following steps:

[0013] S1, mixing the positive electrode material with ammonium sulfate and performing a first stage roasting, so that the positive electrode material is partially converted into sulfate, to obtain a first roasting product;

[0014] S2, raising the temperature so that the first calcined product is subjected to a second stage of calcination to obtain a second calcined product;

[0015] S3, filtering, evaporating and crystallizing the second calcined product after soaking in water to obtain a lithium-rich solution and a slag phase;

[0016] S4. Add a precipitant to the lithium-rich solution to obtain a precipitation reaction solution, and obtain lithium carbonate after filtering.

[0017] Preferably, the mass ratio of the positive electrode material to ammonium sulfate is 1:1.25-1.5. If the ratio is too low, too much unreacted positive electrode material in the first stage of calcination will reduce the lithium extraction rate. If it is too high, all cations in the positive electrode material will be converted into sulfate, and the relevant reactions of the second stage of calcination cannot be carried out. Since the decomposition temperature of (NH4)2SO4 is relatively low, as the temperature rises, the excess (NH4)2SO4 will decompose and release SO x Gas. Therefore, the mass ratio of positive electrode material to ammonium sulfate cannot be too high.

[0018] Preferably, the second stage calcination in S2 is carried out at a temperature of 800-840° C. and for a time of 100-120 min.

[0019] Preferably, the temperature of the first stage calcination in S1 is 250-400°C and the time is 90-150 min.

[0020] Preferably, the positive electrode material in S1 is one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and nickel-cobalt-manganese ternary lithium-ion battery.

[0021] Preferably, the positive electrode material in S1 is lithium cobalt oxide, and the first calcined product contains lithium sulfate, cobalt sulfate and unreacted lithium cobalt oxide.

[0022] Preferably, the second calcined product in S2 contains lithium sulfate and cobalt tetroxide.

[0023] Preferably, the solid-to-liquid ratio during the water immersion in S3 is 200 to 800 g·L -1 The water immersion temperature is 30-90℃ and the time is 10-90min.

[0024] Preferably, the precipitant in S4 is one or both of Na2CO3 and carbon dioxide.

[0025] As a preferred embodiment, n(CO3 2- ) / n(Li + ) is 1.2-1.5.

[0026] In the first step of the calcination process of the present invention, (NH4)2SO4 is used as a calcining agent, and in the second step of the calcination process, transition metal sulfate is used as a calcining agent to preferentially extract lithium from waste positive electrode materials and recover transition metal oxides at the same time. The specific reaction process of the present invention is to first use ammonium sulfate as a calcining agent to carry out the first stage of calcination. In this process, the ratio of positive electrode material to ammonium sulfate must be strictly controlled. The purpose is to ensure that only part of the positive electrode material participates in the reaction during the first stage of the calcination process, and the ammonium sulfate has been completely consumed. In the second stage of the calcination process, ammonium sulfate is used as a calcining agent to recover lithium from waste positive electrode materials. x (SO4) y (M is cobalt, manganese, or nickel), which acts as a calcining agent to react with unreacted positive electrode materials to generate water-soluble lithium sulfate and water-insoluble M oxide; subsequent water immersion directly separates the M ions from the lithium ions, and then battery-grade lithium carbonate is obtained by adding carbonate ions.

[0027] Compared with the prior art, the above technical solution has at least the following beneficial effects:

[0028] In the above scheme, no impure cations are introduced during the entire roasting process, which reduces the energy demand for subsequent evaporation and crystallization; high lithium selectivity and extraction rate, 98.75% of Li can be selectively extracted through water immersion at room temperature of 30°C, and then battery-grade Li2CO3 is successfully prepared; strict control of the use of (NH4)2SO4 can effectively reduce the release of pollutant gases, and it is a relatively environmentally friendly and clean process. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A reaction process diagram of a method for preferentially extracting lithium from a positive electrode of a waste lithium-ion battery by a two-step roasting method provided in a specific embodiment of the present invention.

[0030] Figure 2 XRD analysis diagram of the second calcined product in Examples 1 and 2 and Comparative Examples 1 and 2 in the specific implementation manner of the present invention;

[0031] Figure 3 The XRD analysis diagram of the second calcined product in Example 1 and Comparative Examples 3 and 4 in the specific implementation manner of the present invention is shown. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] A method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method comprises the following steps:

[0035] S1, mixing lithium cobalt oxide and ammonium sulfate and then performing a first stage calcination at a temperature of 350° C. for 120 min, so that the positive electrode material is partially converted into sulfate to obtain a first calcination product, wherein the mass ratio of the positive electrode material to ammonium sulfate is 1:1.25, and the first calcination product contains lithium sulfate, cobalt sulfate and unreacted lithium cobalt oxide;

[0036] In this step, (NH4)2SO4 can decompose at a relatively low calcination temperature during the heating process, and the products NH4HSO4 and (NH4)2SO4 have high thermodynamic spontaneity in an air atmosphere. The specific reaction process is as follows;

[0037] (NH4)2SO4=NH4HSO4+NH3(g)

[0038] NH4HSO4=1 / 3NH3(g)+SO2(g)+2H2O(g)+1 / 3N2(g)

[0039] (NH4)2SO4+O2(g)=N2(g)+4H2O(g)+SO2(g)

[0040] NH4HSO4+1 / 4O2(g)=1 / 2N2(g)+5 / 2H2O(g)+SO2(g)

[0041] Under the promotion of NH4HSO4 and (NH4)2SO4, the thermodynamic driving force for the decomposition of LiCoO2 cathode material is greatly improved. The temperature is further increased. At this stage of reaction temperature, the ΔG of Li and Co oxides with NH4HSO4 and (NH4)2SO4 is negative, which indicates that Li2O and Co3O4 can be spontaneously converted into CoSO4 and Li2SO4 in this step of calcination. The specific reaction formula is as follows:

[0042] Li2O+NH4HSO4=Li2SO4+NH3(g)+H2O(g)

[0043] Co3O4+3NH4HSO4=3CoSO4+7 / 3NH3(g)+4H2O(g)+1 / 3N2(g)

[0044] Li2O+(NH4)2SO4=Li2SO)4+2NH3(g)+H2O(g)

[0045] Co3O4+3(NH4)2SO4=3CoSO4+16 / 3NH3(g)+4H2O(g)+1 / 3N2(g)

[0046] S2. Raise the temperature to carry out a second stage of calcination on the first calcined product. The temperature of the second stage of calcination is 800° C. and the time is 110 min to obtain a second calcined product. The second calcined product contains lithium sulfate and cobalt tetroxide. The calcination atmosphere is nitrogen, argon, or air.

[0047] When entering this step, the ammonium sulfate has been consumed. Raising the temperature will promote the following reactions:

[0048] LiCoO2(R)+1 / 2CoSO4=1 / 2Li2SO4+1 / 2Co3O4

[0049] The CoSO4 produced in the previous stage reacts with the remaining LiCoO2 (R-LCO) to form Li2SO4, while CoSO4 is converted into Co3O4 which is insoluble in water.

[0050] S3, the second roasted product is filtered after being soaked in water, and the solid-liquid ratio during the soaking process is 600g·L -1 , the water immersion temperature is 60°C, the time is 50min, and a lithium-containing solution and a slag phase are obtained;

[0051] S4, adding Na2CO3 and carbon dioxide to the lithium-containing solution to obtain a precipitation reaction solution, wherein n(CO3 2- ) / n(Li + ) is 1.3. After complete precipitation, lithium carbonate is obtained by filtration.

[0052] In this embodiment, the extraction rate of lithium is 98.89%, and the purity of the obtained lithium carbonate is 99.67%.

[0053] like Figure 1 As shown, the reaction mechanism of the preparation method in this embodiment is as follows: ammonium sulfate gradually decomposes and releases NH3 and SO2 gases. Under the promotion of NH3 and SO2, part of the positive electrode material LCO decomposes into Li2O and Co3O4, and is converted into sulfates Li2SO4 and CoSO4. The main calcination products in the first stage are Li2SO4, CoSO4 and R-LCO. At this time, sulfur is in the form of SO4 2- is stored in the form of Li2SO4 without emitting SO2. When the roasting temperature rises to above 800°C, CoSO4 reacts with the remaining LCO (R-LCO) to produce water-soluble Li2SO4 and water-insoluble Co3O4. Li exists in the form of water-soluble Li2SO4, while CoSO4 is converted into water-insoluble Co3O4. The selective extraction of Li element is achieved through a subsequent simple water leaching process. It is worth mentioning that at 800°C, CoSO4 is in a metastable state, so it will not decompose and release SO2 gas. At the same time, the introduction of cations is avoided, reducing the energy demand for subsequent evaporation and crystallization, as well as complex unit operations.

[0054] The results obtained by replacing lithium cobalt oxide with lithium nickel oxide, lithium manganese oxide, and nickel-cobalt-manganese ternary lithium-ion batteries are similar to those in Example 1.

[0055] Example 2

[0056] A method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method comprises the following steps:

[0057] S1, mixing the positive electrode material with ammonium sulfate and performing a first stage calcination at a temperature of 250° C. for 90 min, so that the positive electrode material is partially converted into sulfate to obtain a first calcination product, wherein the mass ratio of the positive electrode material to ammonium sulfate is 1:1.5;

[0058] S2, raising the temperature so that the first calcined product is subjected to a second stage of calcination, the temperature of the second stage of calcination is 810° C., the time is 100 min, and a second calcined product is obtained;

[0059] S3, the second roasted product is filtered after being soaked in water, and the solid-liquid ratio during the soaking process is 200g·L -1 , the water immersion temperature is 30°C, the time is 10 min, and a lithium-containing solution and a slag phase are obtained;

[0060] S4, adding Na2CO3 and carbon dioxide to the lithium-containing solution to obtain a precipitation reaction solution, wherein n(CO3 2- ) / n(Li + ) is 1.2. After precipitation is complete, lithium carbonate is obtained by filtration.

[0061] In this embodiment, the extraction rate of lithium is 99.12%, and the purity of the obtained lithium carbonate is 99.71%.

[0062] Example 3

[0063] A method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery by a two-step roasting method comprises the following steps:

[0064] S1, mixing the positive electrode material with ammonium sulfate and performing a first stage of calcination at a temperature of 400° C. for 150 min, so that the positive electrode material is partially converted into sulfate to obtain a first calcination product, wherein the mass ratio of the positive electrode material to ammonium sulfate is 1:1.3;

[0065] S2, raising the temperature so that the first calcined product is subjected to a second stage of calcination, the temperature of the second stage of calcination is 840° C., the time is 120 min, and a second calcined product is obtained;

[0066] S3, the second roasted product is filtered after being soaked in water, and the solid-liquid ratio during the soaking process is 800g·L -1 , the water immersion temperature is 90°C, the time is 90 minutes, and a lithium-containing solution and a slag phase are obtained;

[0067] S4, adding Na2CO3 to the lithium-containing solution to obtain a precipitation reaction solution, wherein n(CO3 2- ) / n(Li + ) is 1.5. After precipitation is complete, lithium carbonate is obtained by filtration.

[0068] In this embodiment, the extraction rate of lithium is 98.32%, and the purity of the obtained lithium carbonate is 99.73%.

[0069] Comparative Example 1

[0070] This comparative example is similar to Example 1, except that the mass ratio of the positive electrode material to ammonium sulfate in this comparative example is 1:1.

[0071] The extraction rate of Li in this comparative example is 87.46 wt % and the amount of (NH 4 ) 2 SO 4 used is relatively small, so that the Li in LCO is insufficient to be completely extracted.

[0072] Comparative Example 2

[0073] This comparative example is similar to Example 1, except that the mass ratio of the positive electrode material to ammonium sulfate in this comparative example is 1:0.75.

[0074] The extraction rate of Li in this comparative example is smaller than that in comparative example 1.

[0075] The second calcined products in Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to XRD analysis. Figure 2 It can be seen that when w(LCO) / w((NH4)2SO4) is 1:1, there is a LCO diffraction peak, indicating that the CoSO4 produced in the first stage of calcination is not enough to completely convert R-LCO into lithium sulfate. When w(LCO) / w((NH4)2SO4) is 1:0.75, impurity peaks also appear. In addition, if the amount of (NH4)2SO4) is excessive, the selectivity of Li will be reduced. Only when the value of w(LCO) / w((NH4)2SO4) is within the scope of the present invention can the second calcined product contain only lithium sulfate and cobalt oxide, which can ensure the purity of the final lithium carbonate, and at the same time, cobalt can be recovered, and the recovered cobalt has high purity.

[0076] Comparative Example 3

[0077] This comparative example is similar to Example 1, except that the temperature of the second stage calcination in this comparative example is 850°C.

[0078] Comparative Example 4

[0079] This comparative example is similar to Example 1, except that the temperature of the second stage calcination in this comparative example is 750°C.

[0080] The second calcined products in Example 1 and Comparative Examples 3 and 4 were subjected to XRD analysis. Figure 3 The XRD results show that when the calcination temperature is 750℃, different amounts of water-soluble CoSO4 and Li2Co(SO4)2 exist, and a small amount of LCO remains. This indicates that the low calcination temperature cannot completely react CoSO4 with R-LCO, which will reduce the leaching efficiency of Li. When the temperature continues to rise to 850℃, cobalt oxide appears.

[0081] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. The protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A two-step calcination method for preferentially extracting lithium from the positive electrode of waste lithium-ion batteries. It is characterized in that The following steps are involved: S1, mixing the positive electrode material with ammonium sulfate and performing a first stage roasting, so that the positive electrode material is partially converted into sulfate, to obtain a first roasting product; S2, raising the temperature to perform a second stage of roasting on the first roasted product to obtain a second roasted product; S3, filtering, evaporating and crystallizing the second calcined product after soaking in water to obtain a lithium-rich solution and a slag phase; S4, adding a precipitant to the lithium-rich solution to obtain a precipitation reaction solution, and filtering to obtain lithium carbonate; The positive electrode material in S1 is lithium cobalt oxide, and the mass ratio of the positive electrode material to ammonium sulfate is 1:1.25-1.5; The first stage calcination temperature in S1 is 250-400°C and the time is 90-150min; The second stage calcination in S2 has a temperature of 810-840°C and a time of 100-120 min.

2. The method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery according to claim 1, It is characterized in that The first calcined product in S1 contains lithium sulfate, cobalt sulfate and unreacted lithium cobaltate.

3. The method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery according to claim 2, It is characterized in that The second calcined product in S2 contains lithium sulfate and cobalt tetroxide.

4. The method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery according to claim 1, It is characterized in that The solid-liquid ratio during the water immersion process in S3 is 200-800 g·L -1 The water immersion temperature is 30-90℃ and the time is 10-90min.

5. The method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery according to claim 1, It is characterized in that The precipitant in S4 is Na 2 CO 3 , one or both of carbon dioxide.

6. The method for preferentially extracting lithium from the positive electrode of a waste lithium-ion battery according to claim 5, It is characterized in that In S4, the precipitation reaction liquid n(CO 3 2- ) / n(Li + ) is 1.2-1.5.

Citation Information

Patent Citations

  • Method for selectively recovering lithium in waste lithium iron phosphate anode material by high temperature solid phase method

    CN108456788A

  • Recycling method for positive electrode material of waste lithium cobalt oxide battery

    CN113106247A

  • Method for recycling lithium from positive electrode material of waste lithium ion battery

    CN113278805A

  • Method for recycling waste lithium iron phosphate battery at low temperature regenerating lithium iron phosphate positive electrode material

    CN113562717A

  • Method for selectively separating and recycling lithium and manganese from waste lithium manganate battery

    CN115652077A

Cited By

  • Method and device for rapidly preparing high-purity lithium carbonate based on waste lithium battery positive electrode material

    CN123041585A