Method for treating lithium carbonate mother liquor through membrane concentration

Through chemical precipitation purification and pretreatment of lithium carbonate mother liquor and reverse osmosis membrane filtration and concentration technology under alkaline conditions, the problems of low lithium recovery and high energy consumption in the recycling of existing lithium carbonate mother liquor are solved, and efficient lithium recovery is achieved and comprehensive utilization of resources.

CN118929709APending Publication Date: 2024-11-12ZHUHAI WANLI NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411133904.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing methods for recycling and utilization of lithium carbonate mother liquor have problems such as low lithium recovery rate, waste of resources and energy and high energy consumption. Especially after alkaline lithium precipitation mother liquor is neutralized by sulfuric acid, it is filtered and concentrated by nanofiltration membrane and reverse osmosis membrane, resulting in resources Ineffective utilization and energy consumption increase.

Method used

After pretreatment of lithium carbonate mother liquor through chemical precipitation, it was filtration and concentrated under alkaline conditions. Through three-stage purification methods of caustic precipitation, oxalate precipitation and cooling precipitation, combined with the first-stage four-stage alkali-resistant reverse osmosis Membrane filtration produces lithium-rich concentrated alkali liquid and realizes comprehensive utilization of resources.

Benefits of technology

The lithium recovery rate is improved to more than 99.0%, reducing consumption and energy consumption, and achieving efficient resource utilization and significant savings in energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929709A_ABST
    Figure CN118929709A_ABST
Patent Text Reader

Abstract

The invention discloses a method for treating lithium carbonate mother liquor through membrane concentration, which comprises a lithium carbonate mother liquor pretreatment step and a reverse osmosis membrane filtration and concentration step, the lithium carbonate mother liquor is subjected to chemical precipitation purification pretreatment and then is subjected to reverse osmosis membrane filtration and concentration under an alkaline condition to obtain lithium-rich concentrated alkali liquor; the lithium carbonate mother liquor treatment step comprises three-stage purification of causticization precipitation, oxalate precipitation and cooling precipitation, the reverse osmosis membrane filtration and concentration step comprises first-stage four-stage alkali-resistant reverse osmosis membrane filtration and concentration and second-stage reverse osmosis membrane filtration, and lithium-rich concentrated alkali liquor replaces or partially replaces liquid alkali for neutralizing and purifying an acidic lithium sulfate solution. The calcium carbonate slag, the calcium oxalate slag and the pure water can be regenerated and recycled. The method is applied to lithium carbonate lithium precipitation mother liquor treatment, the lithium recovery rate reaches up to 99.0% or above, consumption and emission are low, energy consumption is low, and comprehensive utilization of resources is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for recycling lithium carbonate precipitation mother liquor, in particular to a method for treating mother liquor by reverse osmosis membrane filtration and concentration under alkaline conditions after chemical precipitation purification pretreatment, belonging to the technical field of lithium carbonate. Background Art

[0002] As the lightest metal element in nature with the lowest standard electrode potential and the largest electrochemical equivalent, lithium is an ideal "battery metal". Therefore, it will have long-term demand rigidity in power and energy storage application scenarios requiring high specific energy, and is known as the "white oil of the future."

[0003] Lithium carbonate is the foundation and core of lithium extraction and application. Typically, lithium resources are pretreated, refined, and concentrated to produce a high-lithium solution, which then reacts with sodium carbonate (soda ash) to produce lithium carbonate products. However, the inherent solubility of lithium carbonate causes some lithium to enter the mother liquor after the reaction. Later, solid-liquid separation is performed to produce a lithium-precipitated mother liquor, also known as lithium carbonate mother liquor.

[0004] Lithium precipitation mother liquor is an important secondary lithium resource, and its recycling has always received great attention from the industry. Common methods for recycling lithium precipitation mother liquor include: 1) neutralizing the lithium precipitation mother liquor with sulfuric acid, concentrating and crystallizing most of the anhydrous sodium sulfate, and adding sodium carbonate solution to the lithium-enriched evaporated crystallization mother liquor to precipitate industrial lithium carbonate; 2) neutralizing the lithium precipitation mother liquor with sulfuric acid, concentrating and crystallizing most of the anhydrous sodium sulfate, and then freezing and crystallizing sodium sulfate decahydrate, and adding sodium carbonate solution to the lithium-enriched frozen crystallization mother liquor to precipitate battery-grade lithium carbonate; 3) neutralizing the lithium precipitation mother liquor with sulfuric acid, adding sodium hydroxide to convert lithium ions into lithium hydroxide, and then evaporating and crystallizing anhydrous sodium sulfate, and then freezing and crystallizing sodium sulfate decahydrate, and then introducing carbon dioxide into the lithium-enriched frozen crystallization mother liquor to precipitate battery-grade lithium carbonate. Obviously, these methods neutralize the alkaline lithium precipitation mother liquor with sulfuric acid, and the carbonate ions in the lithium precipitation mother liquor are discharged in an unorganized manner in the form of low-concentration carbon dioxide, which is not in line with the current development concept of the dual-carbon economy. In addition, the synthesis of low-value sodium sulfate with high-value sulfuric acid and sodium hydroxide or sodium carbonate results in ineffective waste of resources. On the other hand, these methods use or use heating and freezing processes multiple times, resulting in huge energy consumption. On the other hand, whether anhydrous sodium sulfate or sodium sulfate decahydrate crystals are precipitated from the high-lithium solution, entraining lithium sulfate or lithium hydroxide loss, resulting in a lithium recovery rate of approximately 85%, which is difficult to improve.

[0005] In recent years, the recycling and utilization methods of lithium carbonate mother liquor have also made great progress, such as extraction, adsorption and membrane separation. Membrane separation is an innovative technology for recovering liquid lithium resources. This technology covers different types of membrane separation methods, including microfiltration, ultrafiltration, nanofiltration, reverse osmosis and electrodialysis. These methods use different membrane permeability and selectivity to achieve different separation and filtration goals, making them suitable for various liquid lithium resource recovery applications. Wan Lingyun (Experimental study on membrane filtration and concentration of lithium-containing mother liquor [J]. Xinjiang Nonferrous Metals, 2020, 43(03): 15-16.) proposed a membrane filtration and concentration technology to treat lithium carbonate mother liquor. The pressure difference on both sides of the membrane is used. Under pressure, the raw liquid flows through the membrane surface. Only water and small molecular substances can pass through the tiny micropores on the membrane surface to become permeate, and other substances larger than the pore size are intercepted and become concentrated liquid. Experiments have found that under acidic conditions, the concentration effect is optimal and the concentration time is short. Under optimal conditions, the lithium recovery rate can reach 99%.

[0006] Chinese patent CN104338441B also discloses a lithium precipitation mother liquor treatment process, which includes the following steps in sequence: (1) adding 98% concentrated sulfuric acid to the lithium precipitation mother liquor until the pH of the mixed solution is 3-7, then continuously monitoring the pH of the solution and maintaining the pH of the mixed solution at 3-7 by controlling the amount of sulfuric acid added; (2) passing the mixed liquor treated in step (1) through the NF membrane and the RO membrane in sequence, collecting the retained solution at the front end of each membrane, and re-mixing the retained solution into the lithium precipitation mother liquor of step (1); (3) repeating steps (1) and (2), and collecting the solution at the front end of the NF membrane and the RO membrane to obtain a high-concentration lithium ion solution; the lithium precipitation mother liquor refers to the lithium precipitation mother liquor produced by extracting lithium salt from lithium ore through the evaporation crystallization process. The NF membrane mentioned here refers to the nanofiltration membrane, and the RO membrane refers to the reverse osmosis membrane. Obviously, the invention also first neutralizes the lithium carbonate lithium precipitation mother liquor with sulfuric acid, and then filters and concentrates it through the nanofiltration membrane and the reverse osmosis membrane, and the concentrated solution is returned to the lithium precipitation mother liquor, which also causes waste of resources and energy.

[0007] In summary, efficient treatment of lithium carbonate mother liquor is a requirement for the sustainable development of the industry and is also a hot topic in current research and application. Summary of the Invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for recycling lithium carbonate mother liquor with high lithium recovery rate, low consumption and low energy consumption.

[0009] To achieve the above objectives, the technical solutions provided by the present invention are:

[0010] A method for treating lithium carbonate mother liquor through membrane concentration includes a lithium carbonate mother liquor pretreatment step and a reverse osmosis membrane filtration and concentration step. After chemical precipitation purification pretreatment, the lithium carbonate mother liquor is filtered and concentrated under alkaline conditions to obtain a lithium-rich concentrated alkali liquor. The lithium-rich concentrated alkali liquor replaces or partially replaces the liquid alkali used for neutralization, purification, and impurity removal of acidic lithium sulfate leachate, thereby reducing liquid alkali consumption, improving lithium recovery, and reducing the amount of sodium removal processing required for concentration and crystallization of the lithium precipitated mother liquor, thereby reducing energy consumption.

[0011] In a preferred embodiment, the lithium carbonate mother liquor pretreatment step includes a lithium carbonate mother liquor causticizing precipitation purification step, wherein a pre-mixed slaked lime suspension is added to the lithium carbonate mother liquor at a rate of 2.0 g / L to 4.0 g / L, stirred and causticized for 60 to 90 minutes at 85° C. to precipitate at a pH of 12 to 14, and filtered to obtain a causticized solution and calcium carbonate slag. The slaked lime suspension is a pre-mixed solid-liquid mixture of 1 part slaked lime and 2 parts water by mass. The main component of slaked lime is Ca(OH)2, which reacts with the lithium carbonate Li2CO3 and sodium carbonate Na2CO3 in the lithium carbonate mother liquor to precipitate calcium carbonate:

[0012] Li2CO3+Ca(OH)2=2LiOH+CaCO3↓

[0013] Na2CO3+Ca(OH)2=2NaOH+CaCO3↓

[0014] Because the solubility product of calcium carbonate precipitation is smaller than that of calcium sulfate, and lithium carbonate mother liquor is generally an alkaline solution with a pH of 9-11, the slaked lime suspension does not easily undergo a precipitation solid-phase conversion reaction with the sodium sulfate in the lithium carbonate mother liquor to form calcium sulfate precipitate. The carbonate ions in the lithium carbonate mother liquor solidify as calcium carbonate, facilitating carbon dioxide recovery and utilization, avoiding unorganized carbon emissions and enabling the recycling of calcium and carbon dioxide. For example, calcium carbonate can be calcined, and the carbon dioxide collected for edible algae cultivation to achieve carbon neutrality. The calcined product, quicklime, is then collected and hydrated to obtain slaked lime. The regenerated lithium hydroxide and sodium hydroxide from causticization can replace or partially replace liquid caustic soda, achieving comprehensive resource utilization. Clearly, caustic precipitation purification with a slaked lime suspension is significantly superior to sulfuric acid neutralization treatment of lithium carbonate mother liquor.

[0015] In a further preferred embodiment, the lithium carbonate mother liquor pretreatment step further includes a causticized liquor oxalate precipitation purification step, wherein oxalic acid is added to the causticized liquor at a concentration of 30.0 mg / L to 40.0 mg / L, and the mixture is stirred at 80°C to 90°C for 60 to 120 minutes to precipitate an oxalate precipitate. The oxalic acid is filtered to obtain a purified liquid and a clean residue, wherein the oxalic acid is oxalic acid dihydrate crystals. Oxalic acid is a dibasic organic acid that is not only an excellent precipitant but also has strong reducing properties and can react with trace amounts of calcium ions in the lithium carbonate mother liquor to produce calcium oxalate precipitate:

[0016] H2C2O4+2OH - =C2O4 2- +2H2O

[0017] C2O4 2- +Ca 2+ =CaC2O4↓

[0018] It can also reduce trace amounts of high-valent metal ions in lithium carbonate mother liquor, such as ferric ions Fe 3+ .

[0019] Typically, the concentration of the solution on the surface of a reverse osmosis membrane is approximately 50 times that of the bulk solution. Trace amounts of calcium ion precipitation or hydrolyzed particles of high-valent metal ions can clog the membrane, hindering water permeability and increasing reverse osmosis pressure. Oxalate precipitation purification offers high purification efficiency, a simple process, and is safe and reliable. Compared to other filtration media or membrane separation methods like nanofiltration, it offers lower waste and energy consumption, lower facility construction and maintenance costs, and facilitates the expansion of existing process technologies.

[0020] In order to ensure the long-term stable operation of the reverse osmosis membrane, in a further preferred scheme, the lithium carbonate mother liquor pretreatment step also includes a purified liquid cooling precipitation purification step, taking the purified liquid, stirring and cooling, cooling to 25°C to 35°C to precipitate, and filter pressing to obtain a feed liquid and a second clean slag. Both causticizing precipitation purification and oxalate precipitation purification belong to purification precipitation at a relatively high temperature (above 80°C). For precipitates whose solubility decreases with increasing temperature, they have the advantages of high precipitation efficiency and complete crystallinity, while for precipitates whose solubility increases with increasing temperature, the precipitation efficiency may decrease. Cooling precipitation can supplement the above two purification methods and further ensure the long-term stable operation of reverse osmosis membrane filtration.

[0021] To ensure a high recovery rate of lithium from the lithium carbonate mother liquor, a further optimized solution also includes a slurry washing step. The purified slag is slurried with fresh or recycled water at a liquid-to-solid ratio of 3:1 by mass. The slurry is then stirred and washed at room temperature for 1.0 to 1.5 hours. The slag is then filtered to produce calcium oxalate slag and wash water. The purified slag is the second clean slag from the purification liquid cooling and precipitation purification step and / or the first clean slag from the causticized liquid oxalate precipitation purification step. The produced wash water is partially returned to the causticized liquid oxalate precipitation purification step and partially returned to the slurry washing step. The calcium oxalate slag can also be decomposed with sulfuric acid to produce oxalic acid for reuse, achieving comprehensive resource utilization.

[0022] The lithium carbonate mother liquor is pre-treated by chemical precipitation purification and then filtered and concentrated by a first-stage four-stage alkali-resistant reverse osmosis membrane to obtain a lithium-rich concentrated alkali solution. First, the lithium carbonate mother liquor is taken and the solution is pre-treated by chemical precipitation purification, filtered through a security filter, and then enters a first-stage reverse osmosis membrane for reverse osmosis filtration and concentration. The produced concentrated water then enters the second-stage reverse osmosis membrane, the third-stage reverse osmosis membrane and the fourth-stage reverse osmosis membrane for reverse osmosis filtration and concentration in sequence to obtain a lithium-rich concentrated alkali solution with a lithium ion concentration enriched by 3.0 to 3.5 times. The recycled water produced by the reverse osmosis membrane filtration of each stage is collected and combined.

[0023] In the preferred embodiment, a secondary reverse osmosis membrane filtration step is also included, in which the collected and combined primary reverse osmosis filtered regenerated water is filtered through a secondary reverse osmosis membrane to obtain pure water and concentrated water, and the concentrated water is returned to the primary reverse osmosis membrane for filtration. The operation of each stage is regulated, and the pure water is used for cleaning and regeneration of the reverse osmosis membrane, etc., to further improve the control performance of the reverse osmosis membrane filtration.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1) High lithium recovery rate The present invention adopts a three-stage chemical precipitation purification method of causticizing precipitation, oxalate precipitation and cooling precipitation to pre-treat the lithium carbonate mother liquor, and then adopts a two-stage reverse osmosis membrane concentration to produce lithium-rich concentrated alkali solution and pure water. The amount of precipitated residue is small, and it is produced from a low-lithium solution with little entrainment; the pure water contains trace amounts of lithium, and the loss is negligible; the lithium-rich concentrated alkali solution replaces or partially replaces the liquid caustic soda, and the lithium is fully recovered, with a lithium recovery rate of more than 99.0%. The existing lithium carbonate mother liquor treatment includes concentrated crystallization and frozen crystallization processes, which produce a large amount of sodium sulfate, all of which precipitate from the lithium-rich solution. The entrained lithium usually reaches 1% to 2% of the crystal mass percentage, and the lithium recovery rate is about 85.0%, which is difficult to improve.

[0026] 2) Low Consumption and Emissions: The present invention uses 2.0g / L to 4.0g / L of slaked lime suspension for causticizing precipitation and 30.0mg / L to 40.0mg / L of oxalic acid for oxalate precipitation. No auxiliary materials are consumed in other steps. Simultaneously with causticizing precipitation, an equal amount of hydroxide is regenerated, resulting in extremely low consumption, a small precipitated slag rate, and low emissions. Existing technologies often use sulfuric acid to neutralize the alkali in the lithium carbonate mother liquor, which not only consumes high-value sulfuric acid and sodium hydroxide or sodium carbonate in the lithium carbonate mother liquor, but also results in unorganized carbon emissions.

[0027] 3) Low energy consumption The present invention adopts a first-stage four-stage alkali-resistant reverse osmosis membrane to filter and concentrate lithium carbonate mother liquor, and the lithium ion concentration is enriched by 3.0 to 3.5 times, which is equivalent to 65% to 70% of evaporated water. The energy consumption of reverse osmosis membrane filtration and concentration is calculated as 50% of the evaporation energy consumption. For every 1.0m 3 The processing capacity of lithium carbonate mother liquor is equivalent to evaporating 650kg to 700kg of water, the heat of water evaporation is 2260kJ / kg, and the energy consumption saved is 734500kJ to 791000kJ, which is equivalent to 25.0kg to 27kg of standard coal.

[0028] 4) High resource utilization rate: After the lithium carbonate mother liquor of the present invention is pre-treated by chemical precipitation purification, it is filtered and concentrated by reverse osmosis membrane under alkaline conditions to obtain lithium-rich concentrated alkali solution and pure water, as well as calcium carbonate slag and calcium oxalate slag generated in the process, which can all be reasonably applied or recycled. The lithium-rich concentrated alkali solution replaces or partially replaces the liquid alkali used for neutralization and purification of acidic lithium sulfate. The calcium carbonate slag solidifies carbon dioxide and can be recycled to achieve carbon neutralization and calcium circulation. The calcium oxalate slag can be recycled for oxalic acid circulation, and the comprehensive resource utilization rate is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a process flow chart for treating lithium carbonate mother liquor by membrane concentration according to the present invention. DETAILED DESCRIPTION

[0030] To make the objectives, technical solutions, and advantages of the present invention more clearly understood, the present invention will be further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are merely exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present invention.

[0031] Lithium extraction from ore is the primary source for battery-grade lithium carbonate production. Lithium carbonate mother liquor, also known as lithium carbonate mother liquor, is an important secondary lithium resource, and its recovery has long been of great interest within the industry. Existing techniques often neutralize the lithium carbonate mother liquor with sulfuric acid and then concentrate it to obtain a lithium-rich solution, from which lithium is subsequently extracted. This results in low lithium recovery rates, wasteful resources, high costs, and high emissions.

[0032] The present invention provides a method for treating lithium carbonate mother liquor by chemical precipitation purification pretreatment and then filtering and concentrating it through reverse osmosis membrane under alkaline conditions. The preferred process flow chart is as follows: Figure 1 Show.

[0033] Depend on Figure 1 It can be seen that the present invention adopts the preferred causticizing precipitation, oxalate precipitation and cooling precipitation three-stage chemical precipitation purification method to pretreat the lithium carbonate mother liquor, and then adopts the preferred two-stage reverse osmosis membrane concentration to produce lithium-rich concentrated alkali solution and pure water, and also includes a slurry washing step for purifying the slag, and the output lithium-rich concentrated alkali solution replaces or partially replaces the acidic lithium sulfate solution and the liquid alkali for purification. The calcium carbonate slag solidifies the carbonate in the lithium carbonate mother liquor, avoids unorganized carbon emissions, and can be regenerated to achieve calcium circulation and carbon neutralization utilization. The calcium oxalate slag can also be regenerated to achieve oxalic acid recycling. The present invention has high lithium recovery rate, low consumption and emission, low energy consumption, and high comprehensive resource utilization rate.

[0034] Some embodiments are listed below to further illustrate the present invention.

[0035]

Example 1

[0036] Weigh 100.0g slaked lime, add 200mL water to prepare slaked lime suspension. 2 .12g / L lithium carbonate mother liquor was heated to 85°C with stirring, and the pre-mixed slaked lime suspension was injected to a pH of 12.0. The causticizing reaction was continued with stirring for 60 minutes. After the reaction was completed, vacuum filtration was performed to obtain a causticized solution and 186.7g of calcium carbonate slag.

[0037] The causticized solution obtained above was heated to 80°C with stirring, 1.5 g of oxalic acid dihydrate was added, and the reaction was continued with stirring for 60 min. After the reaction was completed, vacuum filtration was performed to obtain a purified solution and 2.8 g of a clean residue.

[0038] The purified liquid obtained above was cooled down to 25° C. under stirring, and vacuum filtered to obtain a feed liquid and 1.0 g of a second clean residue.

[0039] The above-obtained feed liquid is put into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter and inlet and outlet liquid pipes, etc. During operation, the concentrated water and the permeated water can be separated by themselves, and the reverse osmosis membrane is an alkali-resistant reverse osmosis membrane.), the system is started, and reverse osmosis filtration is performed to obtain 30.0L of concentrated water and 20.0L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for two-stage reverse osmosis filtration to obtain 21.0L of concentrated water and 9.0L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for three-stage reverse osmosis filtration to obtain 16.7L of concentrated water and 4.3L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for four-stage reverse osmosis filtration to obtain 14.1L of concentrated water and 2.6L of recycled water. The concentrated water filtered by the four-stage reverse osmosis membrane is a lithium-rich concentrated alkali solution containing Li + 7.48g / L, lithium ion concentration enriched 3.5 times, lithium recovery rate 99.50%, 35.9L recycled water produced by reverse osmosis filtration of each section was collected and combined, containing Li + 0.012g / L.

[0040]

Example 2

[0041] Weigh 200.0g slaked lime, add 400mL water to prepare slaked lime suspension. + The 2.32 g / L lithium carbonate mother liquor was heated to 95°C with stirring, and the pre-mixed slaked lime suspension was injected to a pH of 14.0. The causticizing reaction was continued with stirring for 90 minutes. After the reaction was completed, vacuum filtration was performed to obtain the causticized solution and 375.2 g of calcium carbonate slag.

[0042] The causticized solution obtained above was heated to 90°C with stirring, 2.0 g of oxalic acid dihydrate was added, and the reaction was continued with stirring for 120 min. After the reaction was completed, vacuum filtration was performed to obtain a purified solution and 3.7 g of a clean residue.

[0043] The purified liquid obtained above was cooled to 35° C. under stirring and vacuum filtered to obtain a feed liquid and 1.5 g of a second clean residue.

[0044] The above-obtained feed liquid is put into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter and inlet and outlet liquid pipes, etc. During operation, the concentrated water and the permeated water can be separated by themselves, and the reverse osmosis membrane is an alkali-resistant reverse osmosis membrane.), the system is started, and reverse osmosis filtration is performed to obtain 32.0L of concentrated water and 18.0L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for two-stage reverse osmosis filtration to obtain 23.5L of concentrated water and 8.5L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for three-stage reverse osmosis filtration to obtain 18.8L of concentrated water and 4.7L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for four-stage reverse osmosis filtration to obtain 16.6L of concentrated water and 2.2L of recycled water. The concentrated water filtered by the four-stage reverse osmosis membrane is a lithium-rich concentrated alkali solution containing Li + 6.96g / L, lithium ion concentration enriched 3.0 times, lithium recovery rate 99.60%, 33.4L recycled water produced by reverse osmosis filtration of each section was collected and combined, containing Li + 0.013g / L.

[0045]

Example 3

[0046] Weigh 150.0g slaked lime, add 300mL water to prepare slaked lime suspension. + The 2.54 g / L lithium carbonate mother liquor was heated to 90°C with stirring, and the pre-mixed slaked lime suspension was injected to a pH of 13.0. The causticizing reaction was continued with stirring for 80 minutes. After the reaction was completed, vacuum filtration was performed to obtain a causticized solution and 274.5 g of calcium carbonate slag.

[0047] The causticized solution obtained above was heated to 85°C with stirring, 2.0 g of oxalic acid dihydrate was added, and the reaction was continued with stirring for 90 minutes. After the reaction was completed, vacuum filtration was performed to obtain a purified liquid and 3.5 g of a clean residue.

[0048] The purified liquid obtained above was cooled down to 30° C. under stirring, and vacuum filtered to obtain a feed liquid and 1.2 g of a second clean residue.

[0049] The above-obtained feed liquid is put into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter and inlet and outlet liquid pipes, etc. During operation, the concentrated water and the permeated water can be separated by themselves, and the reverse osmosis membrane is an alkali-resistant reverse osmosis membrane.), the system is started, and reverse osmosis filtration is performed to obtain 31.0L of concentrated water and 19.0L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for two-stage reverse osmosis filtration to obtain 22.5L of concentrated water and 8.5L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for three-stage reverse osmosis filtration to obtain 18.5L of concentrated water and 4.0L of recycled water. The produced concentrated water is put into the small reverse osmosis membrane filtration system again for four-stage reverse osmosis filtration to obtain 15.8L of concentrated water and 2.7L of recycled water. The concentrated water filtered by the four-stage reverse osmosis membrane is a lithium-rich concentrated alkali solution containing Li + 8.01g / L, lithium ion concentration enriched 3.15 times, lithium recovery rate 99.65%, 34.2L recycled water produced by reverse osmosis filtration of each section was collected and combined, containing Li + 0.012g / L.

[0050]

Example 4

[0051] Collect the first and second clean residues obtained in Examples 1 to 3, totaling 13.7 g, add 65 mL of water, slurry, wash with magnetic stirring at room temperature for 80 min, and vacuum filter to obtain 11.5 g of calcium oxalate residue and 60 mL of washing water. The washing water contains Li + 0.09g / L.

[0052]

Example 5

[0053] Collect the recycled water obtained from Examples 1 to 3, containing Li + 0.012g / L, take 100.0L and put it into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter and inlet and outlet pipes, etc. During operation, the concentrated water and the permeate can be separated by themselves, and the reverse osmosis membrane is an acid and alkali resistant reverse osmosis membrane.), start the system, and perform reverse osmosis filtration to obtain 32.0L of concentrated water containing Li + 0.038g / L and 68.0L of pure water containing Li + Not detected.

[0054] [Comparative Example 1]

[0055] Take 50.0L of Li +2.44g / L lithium carbonate mother liquor, pH=10.5, was put into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter and inlet and outlet liquid pipes. During operation, the concentrated water and the permeated water can be separated automatically. The reverse osmosis membrane is an alkali-resistant reverse osmosis membrane.), the system was started, and reverse osmosis filtration was performed to obtain 42.5L of concentrated water and 7.5L of recycled water.

[0056] [Comparative Example 2]

[0057] Weigh 150.0g slaked lime, add 300mL water to prepare slaked lime suspension. + The 2.54 g / L lithium carbonate mother liquor was heated to 90°C with stirring, and the pre-mixed slaked lime suspension was injected to a pH of 13.0. The causticizing reaction was continued with stirring for 80 minutes. After the reaction was completed, vacuum filtration was performed to obtain a causticized solution and 274.5 g of calcium carbonate slag.

[0058] The causticized liquid obtained above was put into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter, and inlet and outlet liquid pipes. During operation, the concentrate and permeate can be separated automatically. The reverse osmosis membrane is an alkali-resistant reverse osmosis membrane.). The system was started and reverse osmosis filtration was performed to obtain 37.5 L of concentrate and 12.5 L of recycled water.

[0059] [Comparative Example 3]

[0060] Weigh 150.0g slaked lime, add 300mL water to prepare slaked lime suspension. + The 2.54 g / L lithium carbonate mother liquor was heated to 90°C with stirring, and the pre-mixed slaked lime suspension was injected to a pH of 13.0. The causticizing reaction was continued with stirring for 80 minutes. After the reaction was completed, vacuum filtration was performed to obtain a causticized solution and 274.5 g of calcium carbonate slag.

[0061] The causticized solution obtained above was heated to 85°C with stirring, 2.0 g of oxalic acid dihydrate was added, and the reaction was continued with stirring for 90 minutes. After the reaction was completed, vacuum filtration was performed to obtain a purified liquid and 3.5 g of a clean residue.

[0062] The purified liquid obtained above was put into a small reverse osmosis membrane filtration system (the system consists of a storage tank, a safety filter, a pressurized plunger pump, a single tubular reverse osmosis membrane filter and inlet and outlet liquid pipes. During operation, the concentrated water and the permeated water can be separated automatically, and the reverse osmosis membrane is an alkali-resistant reverse osmosis membrane.), the system was started, and reverse osmosis filtration was performed to obtain 34.5L of concentrated water and 15.5L of recycled water.

[0063] It should be understood that the above specific embodiments of the present application are merely illustrative or explain the principles of the present invention and do not constitute limitations of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included within the scope of protection of the present invention. In addition, the appended claims are intended to cover all variations and modifications that fall within the scope and limits of the appended claims, or equivalents of such scope and limits.

Claims

1. A method for treating lithium carbonate mother liquor by membrane concentration, comprising a lithium carbonate mother liquor pretreatment step and a reverse osmosis membrane filtration concentration step, It is characterized in that The lithium carbonate mother liquor is pre-treated by chemical precipitation purification and then concentrated by reverse osmosis membrane filtration under alkaline conditions to obtain lithium-rich concentrated alkali liquor.

2. The method for treating lithium carbonate mother liquor by membrane concentration according to claim 1, It is characterized in that The lithium carbonate mother liquor pretreatment step includes a lithium carbonate mother liquor causticizing precipitation purification step, wherein 2.0 g / L to 4.0 g / L of lithium carbonate mother liquor is added with a pre-prepared slaked lime suspension, stirred and causticized for 60 min to 90 min at 85° C. to 95° C. and pH=12 to 14 to precipitate, and filtered to obtain a causticized solution and calcium carbonate slag, wherein the slaked lime suspension is a pre-prepared solid-liquid mixture of 1 part slaked lime and 2 parts water in parts by mass.

3. The method for treating lithium carbonate mother liquor by membrane concentration according to claim 2, It is characterized in that The lithium carbonate mother liquor pretreatment step also includes a causticized liquid oxalate precipitation purification step, wherein 30.0 mg / L to 40.0 mg / L of oxalic acid is added to the causticized liquid, stirred at 80° C. to 90° C. for 60 min to 120 min to precipitate oxalate, and filtered to obtain a purified liquid and a clean residue, wherein the oxalic acid is dihydrate oxalic acid crystals.

4. The method for treating lithium carbonate mother liquor by membrane concentration according to claim 3, It is characterized in that The lithium carbonate mother liquor pretreatment step also includes a purification step of cooling and precipitating the purified liquid, wherein the purified liquid is stirred and cooled to 25° C. to 35° C. to precipitate, and is filtered to obtain a feed liquid and a second clean slag.

5. The method for treating lithium carbonate mother liquor by membrane concentration according to claim 4, It is characterized in that The method further comprises a slurry washing step, wherein the purified slag is added with new water or recycled water, slurried at a liquid-to-solid ratio of 3 to 5:1 by mass, washed with stirring at room temperature for 1.0 to 1.5 hours, and filtered to obtain calcium oxalate slag and washing water, wherein the purified slag is the second clean slag in the purified liquid cooling precipitation purification step and / or the first clean slag in the causticized liquid oxalate precipitation purification step, and part of the washing water is returned to the causticized liquid oxalate precipitation purification step, and part is returned to the slurry washing step.

6. The method for treating lithium carbonate mother liquor by membrane concentration according to any one of claims 1 to 5, It is characterized in that The lithium carbonate mother liquor is pre-treated by chemical precipitation purification and then filtered and concentrated by a first-stage four-stage alkali-resistant reverse osmosis membrane to obtain a lithium-rich concentrated alkali solution. First, the lithium carbonate mother liquor is taken after chemical precipitation purification and pre-treatment, and the solution is filtered through a security filter and then enters a first-stage reverse osmosis membrane for reverse osmosis filtration and concentration. The produced concentrated water then enters the second-stage reverse osmosis membrane, the third-stage reverse osmosis membrane and the fourth-stage reverse osmosis membrane for reverse osmosis filtration and concentration in turn to obtain a lithium-rich concentrated alkali solution with a lithium ion concentration enriched by 3.0 to 3.5 times. The recycled water produced by the reverse osmosis membrane filtration of each stage is collected and combined.

7. The method for treating lithium carbonate mother liquor by membrane concentration according to claim 6, It is characterized in that The method also includes a secondary reverse osmosis membrane filtration step, in which the collected and combined primary reverse osmosis membrane filtered regenerated water is filtered through a secondary reverse osmosis membrane to obtain pure water and concentrated water, and the concentrated water is returned to the primary reverse osmosis membrane for filtration.

Citation Information

Cited By

  • Method for recovering iron phosphate and lithium carbonate from lithium iron phosphate waste