Method for preparing polyaluminum chloride or polyaluminum ferric chloride from gasified slag
Through the combined technology of mixed acid leaching of hydrochloric acid and sulfuric acid and yellow sodium ferrosite method, the problem of impurity removal in gasification slag is solved, and efficient preparation of polyaluminum chloride or polyaluminum ferric chloride is achieved, which meets national standards, simplifies the process and reduces the cost. cost and improve the utilization efficiency of solid waste resources.
Patent Information
- Application Number
- CN202410769897.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-12
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-11
AI Technical Summary
When the existing technology uses gasification slag to prepare polyaluminum chloride or polyaluminum ferric chloride, there are problems such as difficulty in removing impurity metal ions, high aluminum element loss rate, complex process and high cost, which limits its industrial application.
The mixed acid leaching method of hydrochloric acid and sulfuric acid is used to inhibit the leaching of calcium ions, combined with the yellow sodium ferrosite method to remove iron and chromium ions, and high-quality polyaluminum chloride or polyaluminum ferric chloride is obtained through hydrolysis and polymerization to form an integrated process system.
It effectively reduces the interference of impurity metal ions, improves the utilization rate of aluminum elements, prepares products that meet national standards, simplifies the process, reduces costs, and improves the utilization efficiency of solid waste resources.
Smart Images

Figure CN118754183A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasification slag, and in particular to a method for simultaneously purifying iron and chromium from a chromium-containing, high-calcium, high-iron and low-aluminium gasification slag leaching liquid and preparing polyaluminium chloride or polyaluminium ferric chloride, belonging to the technical field of environmental protection and resource utilization. Background Art
[0002] Polyaluminium chloride Al2Cl n (OH) 6-n and polyaluminium ferric chloride [Al2(OH) n Cl 6-n ] m [Fe2(OH) n Cl 6-n ] m (SO4) x It has the properties of adsorption, coagulation, and precipitation, and is mainly used in the flocculation and precipitation steps in the water and wastewater treatment process. It can promote the aggregation of particles into larger clumps (flocs) by changing the charge characteristics of suspended particles in water, so that they are easier to remove. With the gradual reduction of domestic high-quality bauxite resources and the enhancement of environmental protection requirements, the research on the preparation of polyaluminum chloride using industrial aluminum-containing waste (such as fly ash, coal gangue, gasification slag, etc.) has received increasing attention. For example ("Research on the Preparation of Polyaluminum Chloride (PAC) from Fly Ash", Jiao Hongjun, Master's Thesis, Lanzhou University of Technology, 20080515) publicly uses fly ash as raw material, and successfully prepares qualified polyaluminum chloride products through acid dissolution and polymerization regulation. However, this method still faces difficulties and challenges such as high process difficulty, high equipment technology requirements, and high impurity removal process costs in practice, which limits the industrial application of these processes.
[0003] Coal-based solid waste is solid waste generated during coal mining and utilization, mainly including coal gangue, fly ash, carbide slag, gasification slag, etc. With the rapid development of coal chemical technology, the annual discharge of coal gasification ash slag is huge. Coal-based solid waste contains a large amount of inorganic and organic matter, and its resource utilization has practical application value and economic benefits, and has become an important development direction at present. However, there are still many problems in the disposal and resource utilization of coal-based solid waste, such as low technical maturity, small profit margin, and environmental protection problems that have not been completely solved. At present, Chinese patent CN108314071A discloses a method for preparing polyaluminum chloride using gasification slag, which is to use hydrochloric acid to circulate and leach gasification slag to obtain aluminum-containing liquid and leached slag, and post-treat the aluminum-containing liquid to obtain a polyaluminum chloride product. The aluminum oxide content (mass percentage) of the obtained polyaluminum chloride product reaches more than 7.8%, the basicity is 54% to 82%, and the density reaches 1.15g / cm 3The above is in line with the national standard requirements (GB15892-2009). The operation process of this method is relatively simple, but it needs to be leached for many times (for example, 9 times in the embodiment), the operation process is relatively large, and the quality requirements of aluminum slag are relatively high, the aluminum content is not less than 20%, and it cannot contain a large amount of heavy metals. In fact, for gasification slag, it often contains a large amount of impurities such as calcium ions and heavy metal ions. The removal of these impurities is the key to preparing high-quality polyaluminum chloride products. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for preparing polyaluminium chloride or polyaluminium ferric chloride using gasification slag. The method uses typical coal-based solid waste gasification slag as raw material, suppresses calcium ion leaching through special mixed acid leaching, and simultaneously removes iron ions and chromium ions by sodium ferrocyanide method, which well solves the technical problem of difficult liquid phase impurity removal and separation in the process of coal-based solid waste recycling, and the impurity removal process effectively reduces the loss rate of target aluminum element, and prepares polyaluminium chloride meeting the GB / T 22627-2022 standard or polyaluminium ferric chloride water purifier product meeting the HG / T-5359-2018 standard, realizes efficient secondary utilization of gasification slag solid waste resources, greatly improves the economic efficiency of solid waste utilization, meets the requirements of the country for the development of circular economy, green industry, and low-carbon technology, and is of great significance to the construction of ecological civilization and sustainable development.
[0005] In order to achieve the above technical purpose, the present invention provides a method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag, the method comprising the following steps:
[0006] 1) Leaching the gasified slag with a binary mixed acid of hydrochloric acid and sulfuric acid to obtain a leachate;
[0007] 2) removing iron and chromium from the leaching solution by a sodium ferroaluminate method to obtain an aluminum-containing purified solution;
[0008] 3) The aluminum-containing purified liquid is subjected to hydrolysis and polymerization reaction to obtain polyaluminum chloride, or the aluminum-containing purified liquid is subjected to iron-aluminum ratio adjustment and then subjected to hydrolysis and polymerization reaction to obtain polyaluminum chloride iron.
[0009] The key to the process of preparing polyaluminium chloride or polyaluminium chloride iron from gasified slag in the present invention is to reduce the interference of impurity metal ions, inhibit calcium ion leaching by leaching with hydrochloric acid and sulfuric acid mixed acid, and remove iron and chromium by combining the yellow sodium iron alum method, and obtain an aluminium-containing purified liquid, and the aluminium-containing purified liquid is subjected to hydrolysis polymerization to obtain a qualified product. The process flow is coherent and gradually optimized in depth, forming a highly integrated complete process system, which provides a new idea for the resource utilization of gasified slag. First, the present invention uses hydrochloric acid and sulfuric acid binary mixed acid to leach gasified slag, which can not only efficiently leach aluminium and iron, but also effectively inhibit the leaching of calcium ions, and can also greatly reduce the amount of acid. Secondly, the yellow sodium iron alum method is used to remove iron and chromium, which can ensure that on the basis of a low aluminium loss rate, the yellow sodium iron alum generated according to the final demand can be adjusted to remove heavy metal ions such as iron and chromium, thereby obtaining an aluminium-containing purified liquid with a relatively high purity. Thereby, high-quality polyaluminium chloride and polyaluminium chloride iron products can be further obtained.
[0010] As a preferred solution, the chromium content in the gasified slag is 0.2-1%, the calcium content is 15-25%, the iron content is 5-15%, and the aluminum content is 10-20%. The gasified slag has the characteristics of high calcium, high iron, low aluminum, and chromium. Based on the composition characteristics of the gasified slag, it is necessary to remove calcium, iron, and chromium from its leachate, which is also a technical difficulty in realizing the resource utilization of gasified slag to prepare polyaluminum chloride or polyaluminum ferric chloride. The method provided by the present invention can well inhibit the leaching of calcium, and at the same time realize the simultaneous removal of heavy metal ions such as iron and chromium in the leachate, so that the gasified slag can be used to prepare polyaluminum chloride that meets the GB / T22627-2022 standard or polyaluminum ferric chloride products that meet the HG / T-5359-2018 standard.
[0011] As a preferred solution, the leaching adopts a two-stage countercurrent leaching method, comprising the following steps:
[0012] a) mixing the gasified slag with binary mixed acid and adding water to adjust the liquid-to-solid ratio to perform leaching I, thereby obtaining a circulating leaching solution and leaching slag;
[0013] b) mixing the new gasified slag with the circulating leaching solution and adding water to adjust the liquid-to-solid ratio to perform leaching II, to obtain a countercurrent leaching solution and a circulating leaching slag; the countercurrent leaching solution is used in step 2);
[0014] c) the circulating leaching residue is mixed with new binary mixed acid and water is added to adjust the liquid-solid ratio to perform leaching III, thereby obtaining a circulating leaching solution and silicon slag; the circulating leaching solution is returned to step b).
[0015] The present invention adopts a two-stage countercurrent leaching method. On the one hand, the acid is fully utilized and the acid consumption is reduced. On the other hand, the aluminum in the leached residue is efficiently leached to improve the utilization rate of the aluminum. On the third hand, the aluminum ion concentration in the leachate can be increased by circulating the acid leaching.
[0016] As a preferred solution, the conditions of leaching I, leaching II or leaching III are: leaching temperature is 70-90°C, leaching time is 3-4 hours, leaching liquid-solid ratio is 3.5-4mL:1g, the initial concentration of sulfuric acid in the leaching system is 0.4-0.8mol / L, and the initial concentration of hydrochloric acid is 1.5-3mol / L. Sulfuric acid in the leaching system can provide sulfate radicals, which can well inhibit the leaching of calcium ions in gasified slag, and can achieve sufficient leaching of aluminum ions. In addition, sulfate radicals are important anions for subsequent yellow sodium iron alum method to remove iron and chromium, which is beneficial to the coprecipitation of iron and chromium. The higher the leaching liquid-solid ratio, the more conducive to leaching, but when the liquid-solid ratio exceeds 4mL:1g, gel is easily produced and separation cannot be achieved.
[0017] As a preferred solution, the endpoint pH of the countercurrent leaching solution is controlled to be 0.3 to 1. By controlling the pH at the leaching endpoint, the alkali consumption required for subsequent pH adjustment and the introduction of impurity ions can be reduced while ensuring efficient leaching of aluminum ions.
[0018] As a preferred solution, the process of removing iron and chromium by the yellow sodium iron alum method is as follows: adjusting the initial pH of the leachate to 1-1.5, heating to 90-100°C, and slowly dripping hydrogen peroxide while gradually adjusting the pH of the leachate to 1.5-2.2 for reaction, reacting for 1.5-2.5 hours, filtering, and obtaining an aluminum-containing purified liquid. The yellow sodium iron alum method for removing iron is not uncommon in the domestic non-ferrous metallurgy industry, but the present invention realizes the co-precipitation of iron and chromium, which is not obvious. The key to the present invention is to control the reaction conditions so that in the process of yellow sodium iron alum precipitation of iron, the trivalent chromium ions replace the iron ions in the yellow sodium iron alum lattice to form isomorphous crystals, thereby realizing the removal of chromium in the yellow sodium iron alum doping in the form of precipitation. To realize the doping of chromium in the yellow sodium iron alum crystal to form an isomorphous crystal, it is necessary to strictly control its pH change and temperature within a preferred range, such as the temperature needs to reach 90-100°C, which is conducive to the doping process of trivalent chromium ions at this temperature. For example, if the initial pH is 1-1.5, and the pH is strictly controlled in the range of 1.5-2.2 during the oxidation process, although the iron ions can be removed when the pH is too low, the removal efficiency of chromium ions is low. If the pH is too high, the hydrolysis and precipitation loss of aluminum ions will be caused.
[0019] As a more preferred solution, the dripping rate of the hydrogen peroxide is 0.2-0.4 mL / min, and the amount of the hydrogen peroxide is 1.5-2 times the molar amount of the ferrous iron in the leachate. The rate of hydrogen peroxide needs to be strictly controlled so that the ferrous iron is preferably oxidized to ferric iron. If the rate of hydrogen peroxide addition is too fast, rapid oxidation may cause the ferrous iron to be incompletely oxidized, thereby affecting the purity of the final product, or causing local overoxidation, and the trivalent chromium is oxidized to hexavalent chromium ions, thereby affecting the removal of chromium. Slowly dripping hydrogen peroxide can better control the rate of the oxidation reaction, avoiding local overheating or side reactions caused by too fast a reaction. Similarly, the amount of hydrogen peroxide is too low, and some ferrous iron ions are not oxidized, while the amount of hydrogen peroxide is too high, and some trivalent chromium is oxidized to hexavalent chromium.
[0020] As a preferred solution, the aluminum-containing purified liquid is adjusted to pH 3-3.5, firstly subjected to a hydrolysis reaction at 50-70°C for 0.5-1.5h, then heated to 80-90°C for a polymerization reaction for 1-2h, and after the reaction is completed, aged for 12-36h and dried to obtain polyaluminum chloride.
[0021] As a preferred solution, the pH is adjusted by using aluminum hydroxide and sodium hydroxide as pH adjusters. Introducing aluminum hydroxide into the pH adjuster can minimize the introduction of impurity metal ions.
[0022] As a preferred scheme, the aluminum-containing purification liquid uses aluminum chloride and ferric chloride to adjust the aluminum-iron mass ratio to 3-4:1, and adjusts the pH to 3-3.5, firstly performs a hydrolysis reaction at 50-70°C for 0.5-1.5h, then heats up to 80-90°C for a polymerization reaction for 1-2h, and after the reaction is completed, ages for 12-36h and dries to obtain polyaluminum ferric chloride.
[0023] As a preferred solution, the pH is adjusted by using aluminum hydroxide and sodium hydroxide as pH adjusters. Introducing aluminum hydroxide into the pH adjuster can minimize the introduction of impurity metal ions.
[0024] The gasified slag of the present invention is pre-ground to -200 mesh.
[0025] The present invention provides a method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag, comprising the following steps:
[0026] (1) Mixed acid secondary countercurrent leaching: (a) Primary leaching process: Take the -200 mesh gasification slag that has been pretreated by grinding and put it in a beaker. Use a binary mixed acid with a sulfuric acid concentration of 0.4-0.8 mol / L and a hydrochloric acid concentration of 1.5-3 mol / L to leach. The amount of sulfuric acid is calculated based on the calcium sulfate required to remove calcium ions in the gasification slag to generate calcium sulfate, which is 0.8-1.2 times the theoretical amount. The liquid-to-solid ratio is 3.5-4 mL:1 g. Then record the liquid level. The leaching temperature is 70-90 ° C. The leaching time is 3-4 hours. After the reaction is completed, filter and wash to obtain a circulating leachate and a primary leaching slag; (b) Secondary leaching process: Take The -200 mesh new gasification slag pretreated by grinding is added with circulating leaching solution and water is added to the liquid level, the leaching temperature is 70-90°C, and the leaching time is 3-4 hours to obtain countercurrent leaching solution (the pH of the countercurrent leaching solution is controlled to be 0.3-1 for subsequent experiments) and circulating leaching slag; (c) after the circulating leaching wet slag is filtered, it is not necessary to dry it, and a binary mixed acid with a sulfuric acid concentration of 0.4-0.8 mol / L and a hydrochloric acid concentration of 1.5-3 mol / L is added for leaching, and water is added to the recorded liquid level, the leaching temperature is 70-90°C, and the leaching time is 3-4 hours. After the reaction is completed, the filter cake is filtered and washed to obtain circulating leaching solution and silicon slag.
[0027] (2) Sodium iron alum method for removing iron and chromium: Based on the fact that some sulfate ions still remain in the solution after mixed acid leaching and the initial pH has met the conditions required for the formation of sodium iron alum, 2-4 mol / L sodium hydroxide is used to adjust the initial pH to 1-1.5, the temperature is raised to 90-100°C, and hydrogen peroxide is added dropwise at a rate of 0.2-0.4 ml / min to oxidize the ferrous ions. 2-4 mol / L sodium hydroxide solution is used to gradually adjust the reaction pH to 1.5-2.2. The reaction time is 1.5-2.5 hours. After the reaction is completed, the purified solution is filtered to obtain.
[0028] (3) Preparation of polyaluminium chloride from purified liquid: The purified liquid is treated with aluminium hydroxide and sodium hydroxide to adjust the pH to 3-3.5 while reducing the introduction of sodium ions. The liquid is first subjected to a hydrolysis reaction at 50-70°C for 0.5-1.5 hours, and then the temperature is raised to 80-90°C for a polymerization reaction for 1-2 hours. After the reaction is completed, the liquid is aged for 12-36 hours to obtain liquid PAC. The liquid PAC is dried to obtain solid polyaluminium chloride.
[0029] (4) Preparation of polyaluminium ferric chloride from purified liquid: Aluminium chloride and ferric chloride are used to adjust the initial aluminium-iron mass ratio of the purified liquid to 3-4:1, and then aluminium hydroxide and sodium hydroxide are used to adjust the pH to 3-3.5 while reducing the introduction of sodium ions. The liquid is first subjected to a hydrolysis reaction at 50-70°C for 0.5-1.5 hours, and then the temperature is raised to 80-90°C for a polymerization reaction for 1-2 hours. After the reaction is completed, the liquid PAFC is aged for 12-36 hours to obtain liquid PAFC, and the liquid PAFC is dried to obtain solid polyaluminium ferric chloride.
[0030] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0031] In the process of preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag, the technical solution of the present invention adopts mixed acid composed of sulfuric acid and hydrochloric acid to leach the gasified slag, thereby reducing the acid dosage and enriching aluminium and iron ions, and preventing calcium ions from entering the solution. The impurity removal process realizes the comprehensive removal of heavy metal ions mainly by co-precipitation of iron and chromium, thereby obtaining an aluminium-containing purified liquid with higher purity, and can prepare polyaluminium chloride meeting the GB / T 22627-2022 standard or polyaluminium ferric chloride water purifier product meeting the HG / T-5359-2018 standard.
[0032] The technical solution of the present invention has a simple operation process, a short flow, and low cost, and is conducive to large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the experimental phenomenon of the secondary countercurrent leaching using a binary mixed acid of hydrochloric acid and sulfuric acid in Example 1.
[0034] Figure 2 This is the experimental phenomenon of removing iron and chromium using the sodium ferroaluminate method in Example 1.
[0035] Figure 3 Physical pictures of PAC and PAFC prepared in Example 1; (left) polyaluminum chloride, (right) polyaluminum ferric chloride.
[0036] Figure 4 Infrared test results of PAC and PAFC prepared in Example 1; (top) polyaluminium chloride, (bottom) infrared test results of polyaluminium ferric chloride.
[0037] Figure 5 This is a process flow chart of Example 1 using a binary mixed acid of hydrochloric acid and sulfuric acid for secondary countercurrent leaching.
[0038] Figure 6 This is the overall process flow diagram of Example 1.
[0039] Figure 7 This is the solid-liquid separation diagram of Example 3. DETAILED DESCRIPTION
[0040] The following examples are provided to further illustrate the present invention, but are not intended to limit the scope of protection of the claims of the present invention.
[0041] Example 1
[0042] Take the following gasification slag composition as an example:
[0043] Table 1 XRF test results of gasified slag
[0044]
[0045] 1. Mixed acid secondary countercurrent leaching
[0046] (1) Primary leaching process: Take 100g of -200 mesh gasified slag pretreated by grinding and put it in a 1L beaker, and leach it with 0.6mol / L sulfuric acid and 2mol / L hydrochloric acid, with a liquid-to-solid ratio of 4:1. Record the liquid level, put it in an 85℃ water bath, and stir it mechanically for 3.5h. After the reaction is completed, filter and wash the filter cake three times to obtain the circulating leachate and the first leaching residue (the first slag does not participate in the cycle). (2) Secondary leaching process: Take 100g of -200 mesh new gasified slag pretreated by grinding, add the circulating leachate and add water to the liquid level, put it in an 85℃ water bath, and stir it mechanically for 3h to obtain the countercurrent leachate and the circulating leach residue. The pH of the countercurrent leachate is about 0.5. After the wet residue is filtered, it does not need to be dried. 0.6mol / L sulfuric acid and 2mol / L hydrochloric acid are added for leaching. Water is added to the recorded liquid level and then placed in a water bath at 85℃ for mechanical stirring for 3h. After the reaction is completed, filter and wash the filter cake three times to obtain the circulating leachate and silicon slag. The countercurrent leachate is used for subsequent experiments.
[0047] 2. Iron-chromium co-precipitation to remove heavy metal ions
[0048] Since some sulfate ions still remain in the solution after mixed acid leaching, and the initial pH has the conditions required for the formation of yellow sodium iron alum, 3 mol / L sodium hydroxide is used to adjust the initial pH to 1, the temperature is raised to 97°C, and hydrogen peroxide is added at a rate of 0.3 ml / min to oxidize the ferrous ions, and 3 mol / L sodium hydroxide solution is used to gradually adjust the reaction pH to 2. The reaction time is 1.5 hours, and after the reaction is completed, the purified solution is filtered.
[0049] Table 2 Efficiency of removing impurity ions by sodium iron alum method (mg / L)
[0050] Al Fe Ca Cr Ion concentration of leaching solution 16762 6770 1982 26.32 Ion concentration of purification solution 15842 2321 1766 13.59 Metal element purification rate / loss rate 5.48% 65.71% 10.89% 50.49%
[0051] 3. Preparation of polyaluminium ferric chloride from purified liquid
[0052] Add an appropriate amount of aluminum chloride to the purified liquid. This step ensures that the aluminum content in the reaction meets the predetermined requirements. In order to adjust the pH of the solution to 3.5 and minimize the introduction of sodium ions, aluminum hydroxide and sodium hydroxide are used to adjust the pH. This step is to create a suitable environment so that aluminum can be hydrolyzed first, while controlling the introduction of sodium ions to ensure the efficiency of the reaction and the quality of the product. After adjusting the pH, the solution is hydrolyzed at 60°C for 1 hour, at which time the hydrolysis reaction of aluminum is mainly carried out. The hydrolysis reaction provides the necessary material precursor for the subsequent polymerization reaction. During the hydrolysis reaction of aluminum, ferric chloride is added in time to ensure that the addition of iron does not affect the hydrolysis process of aluminum, and at the same time, iron is provided for the subsequent polymerization reaction to meet the initial aluminum-iron mass ratio of 3:1. After the hydrolysis reaction is completed, the reaction temperature is raised to 85°C, and the polymerization reaction is carried out at this temperature for 1.5 hours. This step is the key step in the formation of polyaluminum-ferric chloride (PAFC). Through the polymerization reaction, the hydrolysis products of aluminum and iron form a composite flocculant with good purification effect. After the polymerization reaction is completed, the reactants are aged for 24 hours to ensure that the polymer is fully matured and has good stability. Finally, the obtained liquid PAFC is dried to obtain solid polyaluminium ferric chloride. After analysis, the product has met the requirements of HG / T-5359-2018 standard.
[0053] Example 2
[0054] Take the following gasification slag composition as an example:
[0055] Table 3 Gasification slag XRF test results
[0056]
[0057] 1. Mixed acid secondary countercurrent leaching
[0058] (1) Primary leaching process: Take 100g of -200 mesh gasified slag pretreated by grinding in a 1L beaker, add 0.4mol / L sulfuric acid and 2.5mol / L hydrochloric acid, liquid-to-solid ratio 4:1, record the liquid level, put it in an 85℃ water bath, and mechanically stir for 3.5h. After the reaction is completed, filter and wash the filter cake three times to obtain circulating leaching liquid and primary leaching slag (the first slag does not participate in the cycle). (2) Secondary leaching process: Take 100g of -200 mesh new gasified slag pretreated by grinding, add circulating leaching liquid and add water to the liquid level, put it in an 85℃ water bath, and mechanically stir for 3h to obtain countercurrent leaching liquid and circulating leaching slag. The pH of the countercurrent leaching liquid is about 0.5. After the wet residue is filtered, it does not need to be dried. It is continued to be leached with sulfuric acid of 0.4 mol / L and hydrochloric acid of 2.5 mol / L, and water is added to the recorded liquid level. Then it is placed in a water bath at 85°C and mechanically stirred for 3 hours. After the reaction is completed, it should be filtered and the filter cake washed three times to obtain the circulating leachate and silicon slag. The countercurrent leachate is used for subsequent experiments.
[0059] 2. Iron-chromium co-precipitation to remove heavy metal ions
[0060] Since some sulfate ions still remain in the solution after mixed acid leaching, and the initial pH has the conditions required for the generation of yellow sodium iron alum, 2 mol / L sodium hydroxide is used to adjust the initial pH to 1.3, the temperature is raised to 95°C, and hydrogen peroxide is added at a rate of 0.4 ml / min to oxidize the ferrous ions, and 2 mol / L sodium hydroxide solution is continued to be used to gradually adjust the reaction pH to 2.2. The reaction time is 2 hours, and after the reaction is completed, the purified solution is filtered.
[0061] Table 4 Efficiency of removing impurity ions by sodium iron alum method (mg / L)
[0062]
[0063]
[0064] 3. Preparation of polyaluminium chloride from purified liquid
[0065] Add an appropriate amount of aluminum chloride to the purified liquid. This step ensures that the aluminum content in the reaction meets the predetermined requirements. In order to adjust the pH of the solution to 3.5 and minimize the introduction of sodium ions, aluminum hydroxide and sodium hydroxide are used to adjust the pH. This step is to create a suitable environment so that aluminum can be hydrolyzed first, while controlling the introduction of sodium ions to ensure the efficiency of the reaction and the quality of the product. After adjusting the pH, the solution is hydrolyzed at 60°C for 1 hour, at which time the main reaction is the hydrolysis of aluminum. The hydrolysis reaction provides the necessary material precursor for the subsequent polymerization reaction. After the hydrolysis reaction is completed, the reaction temperature is raised to 85°C, and the polymerization reaction is carried out at this temperature for 1.5 hours. This step is a key step in the formation of polyaluminum chloride (PAC). Through the polymerization reaction, the hydrolysis product of aluminum forms a flocculant with good purification effect. After the polymerization reaction is completed, the reactants are aged for 24 hours to ensure the full maturity and stability of the polymer. Finally, the obtained liquid PAC is dried to obtain solid polyaluminum chloride. After analysis, the product has met the requirements of GB / T22627-2022 standard.
[0066] Example 3 (Comparative Example)
[0067] Take the following gasification slag composition as an example:
[0068] Table 5 XRF test results of gasified slag
[0069]
[0070] Leaching process: Take 100g of -200 mesh gasified slag pretreated by grinding into a 1L beaker, and leach it with 0.6mol / L sulfuric acid and 3mol / L hydrochloric acid, with a liquid-solid ratio of 5:1, and record the liquid level. Put it into an 85℃ water bath and stir it mechanically for 5h. Because the liquid-solid ratio is too high and the reaction time is too long, it is speculated that colloid is generated, making it difficult to filter, so subsequent experiments cannot be carried out. Figure 7 Therefore, a reasonable liquid-to-solid ratio, leaching time and other reasonable experimental parameters are required to avoid such a situation.
[0071] Example 4 (Comparative Example)
[0072] Take the following gasification slag composition as an example:
[0073] Table 6 Gasification slag XRF test results
[0074]
[0075] 1. Mixed acid secondary countercurrent leaching
[0076] (1) Primary leaching process: Take 100g of -200 mesh gasified slag pretreated by grinding and put it in a 1L beaker, and leach it with 0.3mol / L sulfuric acid and 2.5mol / L hydrochloric acid, with a liquid-to-solid ratio of 4:1. Record the liquid level, put it in an 85℃ water bath, and stir it mechanically for 3.5h. After the reaction is completed, filter and wash the filter cake three times to obtain the circulating leachate and the first leaching residue (the first slag does not participate in the cycle). (2) Secondary leaching process: Take 100g of -200 mesh new gasified slag pretreated by grinding, add the circulating leachate and add water to the liquid level, put it in an 85℃ water bath, and stir it mechanically for 3h to obtain the countercurrent leachate and the circulating leach residue. The pH of the countercurrent leachate is about 0.5. After the wet residue is filtered, it does not need to be dried. 0.3 mol / L sulfuric acid and 2.5 mol / L hydrochloric acid are added for leaching. Water is added to the recorded liquid level and then placed in an 85°C water bath for mechanical stirring for 3 hours. After the reaction is completed, filter and wash the filter cake three times to obtain the circulating leachate and silicon slag. The countercurrent leachate is used for subsequent experiments.
[0077] 2. Iron-chromium co-precipitation to remove heavy metal ions
[0078] In the initial exploration of the amount of mixed acid, although the initial pH has been controlled to an ideal state, the sulfuric acid ratio in the mixed acid is not within the appropriate range, resulting in residual calcium ions in the solution and insufficient sulfate. The impurities are still removed according to the following steps: use 3 mol / L sodium hydroxide to adjust the initial pH to 1, heat to 97 ° C, and add hydrogen peroxide at a rate of 0.3 ml / min to oxidize ferrous ions, and use 3 mol / L sodium hydroxide solution to gradually adjust the reaction pH to 2, the reaction time is 1.5 hours, and filter after the reaction to obtain a purified solution.
[0079] Table 7 Efficiency of removing impurity ions by sodium iron alum method (mg / L)
[0080] Al Fe Ca Cr Ion concentration of leaching solution 16114 6239 4233 25.44 Ion concentration of purification solution 15993 3324 2449 21.33 Metal element purification rate / loss rate 0.75% 46.72% 42.15% 16.15%
[0081] According to the test results, it can be analyzed that the impurity removal effect is poor due to the lack of a suitable mixed acid ratio. The iron and chromium content in the polyaluminium chloride (PAC) prepared with the purification liquid exceeds the standard and fails to meet the national standard.
[0082] Example 5 (Comparative Example)
[0083] Take the following gasification slag composition as an example:
[0084] Table 8 Gasification slag XRF test results
[0085]
[0086] 1. Mixed acid secondary countercurrent leaching
[0087] (1) Primary leaching process: Take 100g of -200 mesh gasified slag pretreated by grinding and put it in a 1L beaker, and leach it with 0.6mol / L sulfuric acid and 2mol / L hydrochloric acid, with a liquid-to-solid ratio of 4:1. Record the liquid level and put it in an 85℃ water bath, and stir it mechanically for 3.5h. After the reaction is completed, filter and wash the filter cake three times to obtain the circulating leachate and primary leaching slag. (2) Secondary leaching process: Take 100g of -200 mesh new gasified slag pretreated by grinding, add the circulating leachate and add water to the liquid level, put it in an 85℃ water bath, and stir it mechanically for 3h to obtain the countercurrent leachate and circulating leach slag. The pH of the countercurrent leachate is about 0.5. After filtering the circulating leaching wet slag, there is no need to dry it. Continue to add 0.6mol / L sulfuric acid and 2mol / L hydrochloric acid for leaching, add water to the recorded liquid level, and put it in an 85℃ water bath, and stir it mechanically for 3h. After the reaction is finished, filter and wash the filter cake three times to obtain the circulating leaching solution and silicon slag. The countercurrent leaching solution is used for subsequent experiments.
[0088] 2. Iron-chromium co-precipitation to remove heavy metal ions
[0089] Under a reasonable acidity ratio, calcium ions are fully removed, and the residual sulfate in the solution can make yellow sodium ferrocite normally generated. The effect of reaction pH on the impurity removal effect is further explored. The impurity removal is carried out according to the following steps: the solution is heated to 97°C, and hydrogen peroxide is added at a rate of 0.3 ml / min to oxidize ferrous ions, and 3 mol / L sodium hydroxide solution is used to gradually adjust the reaction end point pH to 1.3. The reaction time is 1.5 hours. After the reaction is completed, it is filtered to obtain a purified solution.
[0090] Table 9 Efficiency of removing impurity ions by sodium iron alum method (mg / L)
[0091] Al Fe Ca Cr Ion concentration of leaching solution 13243 8770 1282 28.17 Ion concentration of purification solution 12534 1942 1125 21.33 Metal element purification rate / loss rate 5.35% 77.86% 12.24% 24.28%
[0092] According to the test results, it can be analyzed that because the pH at the reaction end point is too low, although sodium ferroaluminate can be generated normally and a large amount of iron can be removed, only a small amount of chromium is generated in the same phase as the iron and removed together, resulting in poor impurity removal effect. The content of trace element chromium in the polyaluminium chloride (PAC) prepared with this purification liquid exceeds the standard and fails to meet the national standard.
Claims
1. A method for preparing polyaluminium chloride or polyaluminium ferric chloride using gasified slag, characterized in that: The following steps are involved: 1) Leaching the gasified slag with a binary mixed acid of hydrochloric acid and sulfuric acid to obtain a leachate; 2) removing iron and chromium from the leaching solution by a sodium ferroaluminate method to obtain an aluminum-containing purified solution; 3) The aluminum-containing purified liquid is subjected to hydrolysis and polymerization reaction to obtain polyaluminum chloride, or the aluminum-containing purified liquid is subjected to iron-aluminum ratio adjustment and then subjected to hydrolysis and polymerization reaction to obtain polyaluminum chloride iron.
2. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 1, characterized in that: The gasified slag has a chromium content of 0.2-1% by mass, a calcium content of 15-25% by mass, an iron content of 5-15% by mass and an aluminum content of 10-20% by mass.
3. A method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 1 or 2, characterized in that: The leaching adopts a two-stage countercurrent leaching method, comprising the following steps: a) mixing the gasified slag with binary mixed acid and adding water to adjust the liquid-to-solid ratio to perform leaching I, thereby obtaining a circulating leaching solution and leaching slag; b) mixing the new gasified slag with the circulating leaching solution and adding water to adjust the liquid-to-solid ratio to perform leaching II, to obtain a countercurrent leaching solution and a circulating leaching slag; the countercurrent leaching solution is used in step 2); c) the circulating leaching residue is mixed with new binary mixed acid and water is added to adjust the liquid-solid ratio to perform leaching III, thereby obtaining a circulating leaching solution and silicon slag; the circulating leaching solution is returned to step b).
4. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 3, characterized in that: The conditions of leaching I, leaching II or leaching III are: leaching temperature is 70-90° C., leaching time is 3-4 hours, leaching liquid-solid ratio is 3.5-4 mL:1 g, initial concentration of sulfuric acid in the leaching system is 0.4-0.8 mol / L, and initial concentration of hydrochloric acid is 1.5-3 mol / L.
5. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 1, characterized in that: The process of removing iron and chromium by the yellow sodium ferroaluminate method is as follows: adjusting the initial pH of the leaching solution to 1-1.5, heating to 90-100° C., slowly dripping hydrogen peroxide and gradually adjusting the pH of the leaching solution to a range of 1.5-2.2 for reaction, reacting for 1.5-2.5 hours, filtering, and obtaining an aluminum-containing purified solution.
6. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 1, characterized in that: The dripping rate of the hydrogen peroxide is 0.2-0.4 mL / min, and the amount of the hydrogen peroxide is 1.5-2 times the molar amount of the divalent iron in the leaching solution.
7. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 1, characterized in that: The aluminum-containing purified liquid is adjusted to pH 3-3.5, firstly subjected to a hydrolysis reaction at 50-70° C. for 0.5-1.5 h, then heated to 80-90° C. for a polymerization reaction for 1-2 h, and after the reaction is completed, aged for 12-36 h and dried to obtain polyaluminum chloride.
8. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 7, characterized in that: The pH is adjusted by using aluminum hydroxide and sodium hydroxide as pH adjusters.
9. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 1, characterized in that: The aluminum-containing purification liquid uses aluminum chloride and ferric chloride to adjust the aluminum-iron mass ratio to 3-4:1, and adjusts the pH to 3-3.5, firstly performs a hydrolysis reaction at 50-70° C. for 0.5-1.5 hours, then heats up to 80-90° C. for a polymerization reaction for 1-2 hours, and after the reaction is completed, ages for 12-36 hours and is dried to obtain polyaluminum ferric chloride.
10. The method for preparing polyaluminium chloride or polyaluminium ferric chloride by using gasified slag according to claim 9, characterized in that: The pH is adjusted by using aluminum hydroxide and sodium hydroxide as pH adjusters.