Component gradient gradient perovskite microwire and preparation method thereof
By gradient distribution of Cl and Br ions on perovskite microwires, the problems of poor stability of perovskite materials and difficulty in laser wavelength tuning in the existing technology are solved, and high-quality, wide-band range fluorescence emission and laser miniaturization are achieved. .
Patent Information
- Application Number
- CN202410980012.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
AI Technical Summary
Existing all-inorganic perovskite materials have problems such as poor stability, complex preparation processes, low yields, difficulty in tuning the laser wavelength, high cost, and bulky equipment during the preparation process.
Using the composition gradient structure of CsPbClxBr3-x micron wires, Cl and Br ions are gradiently distributed along the length direction of the perovskite micron wires, and the soft lattice characteristics are used to precisely control the Cl/Br ratio to achieve high-quality, wide Band-wide, continuously tunable fluorescence emission. The method includes selecting CsPbBr3 micron wires with a diameter of 3 to 10 μm and good crystallization quality, transferring them to a PMMA substrate, covering them with thermal release tape, and performing a Cl ion substitution reaction in an anhydrous calcium chloride environment to form CsPbClxBr3-x micron wires. .
It achieves high-quality, wide-band range, and continuously tunable fluorescence emission on a single micron line, promotes the miniaturization and ultra-compact design of lasers, and provides a strategy for broadband tunable lasers and high-precision micro spectrometers.
Smart Images

Figure CN118754192A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to micrometer wires and a preparation method thereof, and in particular to a perovskite micrometer wire with a gradient component change and a preparation method thereof. Background Art
[0002] Lead halide perovskite materials have the advantages of high fluorescence quantum efficiency, wide wavelength tunable range, high light absorption coefficient, long carrier lifetime, and long diffusion length, and have received extensive attention in the field of optoelectronic devices such as light-emitting diodes, photodetectors, and solar cells. The preparation methods of perovskite micro-nano crystals are flexible and diverse, which provides convenient conditions for designing different resonant cavities to meet the needs of different application scenarios. In general, perovskite nanowires and microsheets can serve as natural microcavities of Fabry-Pérot (FP) and whispering gallery mode (WGM) oscillation types and provide sufficient gain for light amplification. In particular, the all-inorganic perovskite material CsPbX3 (X=Cl, Br, I) has excellent stability, and a large number of milestone research works have been reported in the realization of high-quality, low-threshold lasers pumped by single photons.
[0003] In addition, wavelength control of semiconductor lasers is an important requirement in practical applications, and can provide new multifunctional coherent light sources for all-optical integrated chips and optical interconnection systems. In the past decade, research on tunable lasers has been widely reported, and many control methods have been developed, such as self-absorption effect, BM effect, physical field, band engineering, etc. Among them, the most representative method in terms of wide-band wavelength control capability is band engineering, which has been achieved in some II-VI and III-V semiconductor materials by controlling the elemental composition. However, the preparation of these semiconductor micro-nano structures usually requires harsh high temperature and low pressure conditions.
[0004] Although existing all-inorganic perovskite materials can produce lead halide perovskites with concentration gradients, they have the disadvantages of poor stability, complex preparation process, and low yield. In addition, existing lasers generally have the disadvantages of difficult wavelength tuning, high cost, and large size. Summary of the invention
[0005] Purpose of the invention: In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a high-quality, wide-band, continuously tunable component gradient perovskite microwire. Another purpose of the present invention is to provide a simple and convenient method for preparing component gradient perovskite microwire.
[0006] Technical solution: The present invention discloses a perovskite microwire with a gradient composition, the molecular formula of which is: CsPbCl x Br 3-x, 1≤x≤3, Cl and Br are distributed in a gradient along the length direction of the perovskite microwire, the diameter of the perovskite microwire is 3-10 μm, and the length is 100-200 μm.
[0007] The method for preparing a perovskite microwire with a gradient composition of the present invention comprises the following steps:
[0008] Step 1: Select CsPbBr3 micron wires with a diameter of 3 to 10 μm, good crystal quality, and perfect whispering gallery cavity structure;
[0009] Step 2: Transfer the CsPbBr3 micrometer wires to a clean glass substrate spin-coated with PMMA;
[0010] Step 3, covering one end of the CsPbBr3 micron wire with a thermal release tape, leaving the other end bare;
[0011] Step 4: Take concentrated hydrochloric acid and put it into a glass culture dish with anhydrous calcium chloride together with the product obtained in step 3;
[0012] Step 5, seal the mouth of the glass culture dish with a film and react at 60-80°C;
[0013] Step six, heating the product obtained in step five at 115-125° C., removing the thermal release tape, and further diffusing to obtain perovskite microwires with a gradient composition.
[0014] Furthermore, in step 1, the preparation method of CsPbBr3 micrometer wire is:
[0015] (1) Weighing equal moles of CsBr and PbBr2, dissolving them in a DMSO solvent at 45-55° C., and stirring until completely dissolved to obtain a mixed solution of CsBr and PbBr2;
[0016] (2) While the mixed solution of CsBr and PbBr2 is being vigorously stirred, acetonitrile is added dropwise;
[0017] (3) heating the solution obtained in step (2) to 45-55° C. again and stirring, then cooling to room temperature, filtering the supernatant to obtain a precursor solution;
[0018] (4) The precursor solution is dropped onto the cleaned glass substrate surface, sealed, and reacted at 45-55° C. to obtain randomly distributed CsPbBr 3 perovskite microwires.
[0019] Furthermore, in step 1, the CsPbBr3 micron wire with good crystallization quality is a CsPbBr3 micron wire with complete structure, smooth surface, no degradation, and no impurities. Under a stereo microscope, a probe is used to cause a slight peeling between the micron wire and the substrate to facilitate subsequent transfer. The perfect whispering gallery cavity structure means that the cavity of the material itself is the whispering gallery structure.
[0020] Furthermore, in step 2, the transfer is to dip the probe into PMMA to make the needle tip have adhesion, and then contact the needle tip with PMMA under a microscope to the selected CsPbBr3 micron wire to make it stick to the needle tip.
[0021] Furthermore, in step three, the thermal release tape is made of hot melt adhesive material. The hot melt adhesive becomes soft and fluid after being heated, and solidifies rapidly after being cooled, and has excellent bonding properties.
[0022] Furthermore, in step 4, the mass percentage of concentrated hydrochloric acid is 37wt%. The mass of anhydrous calcium chloride is 25-35g, which is used to absorb the water in the volatilized hydrochloric acid to keep the reaction environment dry. 20μL of 37% concentrated hydrochloric acid is drawn with a pipette, and the purpose of removing the pipette and sealing its thick end is that the thick end will cause the hydrochloric acid to evaporate too quickly, and the high chloride ion in the reaction environment will cause the micron wire to break or degrade the micron wire.
[0023] Furthermore, in step 5, the reaction time is 6 to 8 hours. The opening of the culture dish containing the sample is sealed with a film to isolate the reaction environment from the influence of external impurities and interfere with the reaction.
[0024] Furthermore, in step 6, the heating time is 25 to 35 seconds. The thermal release tape in the covered area is removed to expose the unreacted area, allowing the reacted chloride ions to further diffuse.
[0025] Preparation principle: Under appropriate temperature conditions, the pre-synthesized CsPbBr3 micron wires are exposed to an environment containing HCl gas, and the Cl ions in the gas phase are exchanged with the Br ions in the micron wires by utilizing the unique soft lattice characteristics of the perovskite material. In this process, the Cl ions gradually replace the Br ions to form a CsPbCl with uniform distribution. x Br 3-x Alloy microwires. This method can precisely control the Cl / Br ratio, ensuring high quality and excellent optoelectronic properties of the microwires while avoiding impurities that may be introduced in the solution method.
[0026] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0027] 1. Able to produce perovskite CsPbCl with a gradient of single halogen composition x Br3-x Micrometer wires, using the interdiffusion mechanism of halogen anions at the atomic scale and the exciton recombination process, successfully achieve high-quality, wide-band, and continuously tunable fluorescence emission on a single wire;
[0028] 2. The present invention utilizes the soft lattice characteristics of perovskite materials to provide a new strategy for constructing a new broadband tunable laser and a high-precision micro-spectrometer, so as to achieve the laser emitting at different wavelengths on a micron line and realize the miniaturization and ultra-compactness of the laser. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a preparation flow chart of the present invention;
[0030] Figure 2 The single CsPbCl obtained in Example 1 of the present invention x Br 3-x Fluorescence emission spectra of micrometer wires;
[0031] Figure 3 The single CsPbCl obtained in Example 1 of the present invention x Br 3-x The dependence diagram between the emission peak position of the micrometer line and different collection points;
[0032] Figure 4 The single CsPbCl obtained in Example 1 of the present invention x Br 3-x Band gap gradient variation diagram at different points along the axis of the microwire;
[0033] Figure 5 This is a microscope image of the micrometer wire obtained in Comparative Example 5. DETAILED DESCRIPTION
[0034] Unless otherwise specified, the materials, reagents, instruments, etc. used in the following examples can be obtained from commercial sources. Experimental methods without specific conditions in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0035] Example 1
[0036] like Figure 1 , a method for preparing a perovskite microwire with a gradient composition, comprising the following steps:
[0037] (1) Weigh equimolar amounts of CsBr and PbBr2, dissolve them in DMSO solvent at 50°C, and stir for 2 h until the two salts are completely dissolved to prepare a 0.3 mol / L mixed solution of CsBr and PbBr2.
[0038] (2) The solution is cooled to room temperature, and acetonitrile is added dropwise to the mixed solution under vigorous stirring with a magnetic stirrer. As the acetonitrile solvent is titrated, a yellow substance is produced, but then it immediately dissolves. When the solution is close to saturation, a white precipitate that does not dissolve with stirring is produced. As the acetonitrile solvent is continued to be added dropwise, the yellow-orange substance no longer disappears, and the solution has reached a supersaturated state.
[0039] (3) The supersaturated solution is heated to 50° C. again and stirred for 24 h, then cooled to room temperature. The supernatant is filtered to obtain the precursor solution required for growing CsPbBr3 micrometer wires.
[0040] (4) The size is about 2×2cm 2 The glass substrate was first ultrasonically cleaned with acetone and anhydrous ethanol for 5 min each, then ultrasonically cleaned with deionized water for 15 min, and then dried with a nitrogen gun.
[0041] (5) The treated glass substrate is transferred to a polytetrafluoroethylene container containing 10 mL of acetonitrile solvent. A certain amount of precursor solution is dripped onto the surface of the glass substrate, and the container is sealed.
[0042] (6) The sealed container is placed in a 50°C forced air drying oven for 12 hours to obtain randomly distributed CsPbBr3 micrometer wires.
[0043] (7) Using an optical microscope, CsPbBr3 microwires with perfect whispering gallery cavity structure were selected from randomly distributed CsPbBr3 microwires with a diameter and length of 5 μm and 100 μm, respectively, and transferred to a clean glass substrate spin-coated with PMMA.
[0044] (8) Under a stereo microscope, a CsPbBr3 micron wire with good crystal quality and perfect whispering gallery cavity structure was selected and covered with a thermal release tape, leaving the other end exposed.
[0045] (9) Use a pipette to draw up 20 μL of 37% concentrated hydrochloric acid, remove the pipette and seal its thick end, and place it together with the transferred microwires in a 13 cm × 3 cm (diameter × height) glass culture dish (with 30 g of anhydrous calcium chloride pre-placed at the bottom).
[0046] (10) Seal the mouth of the culture dish containing the sample with a film and place it in a 65°C forced air drying oven for 7 h.
[0047] (11) After the reaction was completed, the sample was placed on a heating table at 120 °C and heated for 30 s. After the thermal release tape was removed, it was further diffused to obtain a single CsPbCl with a gradient composition. x Br 3-x Perovskite microwires.
[0048] The single CsPbCl obtained in this example was measured by a micro-fluorescence spectroscopy system. x Br 3-x Optical performance test of micrometer wire composite microcavity structure: Figures 2 to 4 The research results show that the fluorescence emission spectrum of the sample in Example 1 shows that the emission peak position changes continuously toward the short-wave direction as the collection point moves from the Br-rich end to the Cl-rich end, and the wavelength change range is about 430nm to 520nm. Taking the Br-rich end face as the test origin, it can be obtained that the entire diffusion range can reach up to nearly 60μm.
[0049] Example 2
[0050] A method for preparing a perovskite micron wire with a gradient composition comprises the following steps:
[0051] (1) Weigh equimolar amounts of CsBr and PbBr2, dissolve them in DMSO solvent at 50°C, and stir for 2 h until the two salts are completely dissolved to prepare a 0.3 mol / L mixed solution of CsBr and PbBr2.
[0052] (2) The solution is cooled to room temperature, and acetonitrile is added dropwise to the mixed solution under vigorous stirring with a magnetic stirrer. As the acetonitrile solvent is titrated, a yellow substance is produced, but then it immediately dissolves. When the solution is close to saturation, a white precipitate that does not dissolve with stirring is produced. As the acetonitrile solvent is continued to be added dropwise, the yellow-orange substance no longer disappears, and the solution has reached a supersaturated state.
[0053] (3) The supersaturated solution is heated to 50° C. again and stirred for 24 h, then cooled to room temperature. The supernatant is filtered to obtain the precursor solution required for growing CsPbBr3 micrometer wires.
[0054] (4) The size is about 2×2cm 2 The glass substrate was first ultrasonically cleaned with acetone and anhydrous ethanol for 5 min each, then ultrasonically cleaned with deionized water for 15 min, and then dried with a nitrogen gun.
[0055] (5) The treated glass substrate is transferred to a polytetrafluoroethylene container containing 10 mL of acetonitrile solvent. A certain amount of precursor solution is dripped onto the surface of the glass substrate, and the container is sealed.
[0056] (6) The sealed container is placed in a 50°C forced air drying oven for 12 hours to obtain randomly distributed CsPbBr3 micrometer wires.
[0057] (7) Using an optical microscope, CsPbBr3 microwires with perfect whispering gallery cavity structure were selected from randomly distributed CsPbBr3 microwires with a diameter and length of 5 μm and 150 μm, respectively, and transferred to a clean glass substrate spin-coated with PMMA.
[0058] (8) Under a stereo microscope, a CsPbBr3 micron wire with good crystal quality and perfect whispering gallery cavity structure was selected and covered with a thermal release tape, leaving the other end exposed.
[0059] (9) Use a pipette to draw up 20 μL of 37% concentrated hydrochloric acid, remove the pipette and seal its thick end, and place it together with the transferred microwires in a 13 cm × 3 cm (diameter × height) glass culture dish (with 30 g of anhydrous calcium chloride pre-placed at the bottom).
[0060] (10) Seal the mouth of the culture dish containing the sample with a film and place it in a 65°C forced air drying oven for 6 h.
[0061] (11) After the reaction was completed, the sample was placed on a heating table at 120 °C and heated for 30 s. After the thermal release tape was removed, it was further diffused to obtain a single CsPbCl with a gradient composition. x Br 3-x Perovskite microwires.
[0062] Example 3
[0063] A method for preparing a perovskite micron wire with a gradient composition comprises the following steps:
[0064] (1) Weigh equimolar amounts of CsBr and PbBr2, dissolve them in DMSO solvent at 50°C, and stir for 2 h until the two salts are completely dissolved to prepare a 0.3 mol / L mixed solution of CsBr and PbBr2.
[0065] (2) The solution is cooled to room temperature, and acetonitrile is added dropwise to the mixed solution under vigorous stirring with a magnetic stirrer. As the acetonitrile solvent is titrated, a yellow substance is produced, but then it immediately dissolves. When the solution is close to saturation, a white precipitate that does not dissolve with stirring is produced. As the acetonitrile solvent is continued to be added dropwise, the yellow-orange substance no longer disappears, and the solution has reached a supersaturated state.
[0066] (3) The supersaturated solution is heated to 50° C. again and stirred for 24 h, then cooled to room temperature. The supernatant is filtered to obtain the precursor solution required for growing CsPbBr3 micrometer wires.
[0067] (4) The size is about 2×2cm 2The glass substrate was first ultrasonically cleaned with acetone and anhydrous ethanol for 5 min each, then ultrasonically cleaned with deionized water for 15 min, and then dried with a nitrogen gun.
[0068] (5) The treated glass substrate is transferred to a polytetrafluoroethylene container containing 10 mL of acetonitrile solvent. A certain amount of precursor solution is dripped onto the surface of the glass substrate, and the container is sealed.
[0069] (6) The sealed container is placed in a 50°C forced air drying oven for 12 hours to obtain randomly distributed CsPbBr3 micrometer wires.
[0070] (7) Using an optical microscope, CsPbBr3 microwires with perfect whispering gallery cavity structure were selected from randomly distributed CsPbBr3 microwires with a diameter and length of 5 μm and 100 μm, respectively, and transferred to a clean glass substrate spin-coated with PMMA.
[0071] (8) Under a stereo microscope, a CsPbBr3 micron wire with good crystal quality and perfect whispering gallery cavity structure was selected and covered with a thermal release tape, leaving the other end exposed.
[0072] (9) Use a pipette to draw up 20 μL of 37% concentrated hydrochloric acid, remove the pipette and seal its thick end, and place it together with the transferred microwires in a 13 cm × 3 cm (diameter × height) glass culture dish (with 30 g of anhydrous calcium chloride pre-placed at the bottom).
[0073] (10) Seal the mouth of the culture dish containing the sample with a film and place it in a 65°C forced air drying oven for 7 h.
[0074] (11) After the reaction was completed, the sample was placed on a heating table at 120 °C and heated for 30 s. After the thermal release tape was removed, it was further diffused to obtain a single CsPbCl with a gradient composition. x Br 3-x Perovskite microwires.
[0075] Example 4
[0076] A method for preparing a perovskite micron wire with a gradient composition comprises the following steps:
[0077] (1) Weigh equimolar amounts of CsBr and PbBr2, dissolve them in DMSO solvent at 45°C, and stir for 2 h until the two salts are completely dissolved to prepare a 0.3 mol / L mixed solution of CsBr and PbBr2.
[0078] (2) The solution is cooled to room temperature, and acetonitrile is added dropwise to the mixed solution under vigorous stirring with a magnetic stirrer. As the acetonitrile solvent is titrated, a yellow substance is produced, but then it immediately dissolves. When the solution is close to saturation, a white precipitate that does not dissolve with stirring is produced. As the acetonitrile solvent is continued to be added dropwise, the yellow-orange substance no longer disappears, and the solution has reached a supersaturated state.
[0079] (3) The supersaturated solution is heated to 45° C. again and stirred for 24 h, then cooled to room temperature. The supernatant is filtered to obtain the precursor solution required for growing CsPbBr3 micrometer wires.
[0080] (4) The size is about 2×2cm 2 The glass substrate was first ultrasonically cleaned with acetone and anhydrous ethanol for 5 min each, then ultrasonically cleaned with deionized water for 15 min, and then dried with a nitrogen gun.
[0081] (5) The treated glass substrate is transferred to a polytetrafluoroethylene container containing 10 mL of acetonitrile solvent. A certain amount of precursor solution is dripped onto the surface of the glass substrate, and the container is sealed.
[0082] (6) The sealed container is placed in a 45°C forced air drying oven for 12 hours to obtain randomly distributed CsPbBr3 micrometer wires.
[0083] (7) Using an optical microscope, CsPbBr3 microwires with perfect whispering gallery cavity structure were selected from randomly distributed CsPbBr3 microwires with a diameter and length of 3 μm and 200 μm, respectively, and transferred to a clean glass substrate spin-coated with PMMA.
[0084] (8) Under a stereo microscope, a CsPbBr3 micron wire with good crystal quality and perfect whispering gallery cavity structure was selected and covered with a thermal release tape, leaving the other end exposed.
[0085] (9) Use a pipette to draw up 20 μL of 37% concentrated hydrochloric acid, remove the pipette and seal its thick end, and place it together with the transferred microwires in a 13 cm × 3 cm (diameter × height) glass culture dish (with 25 g of anhydrous calcium chloride pre-placed at the bottom).
[0086] (10) Seal the mouth of the culture dish containing the sample with a film and place it in an 80°C forced air drying oven for 7 h.
[0087] (11) After the reaction was completed, the sample was placed on a heating table at 115 °C for 35 s. After the thermal release tape was removed, it was further diffused to obtain a single CsPbCl with a gradient composition. x Br 3-x Perovskite microwires.
[0088] Example 5
[0089] A method for preparing a perovskite micron wire with a gradient composition comprises the following steps:
[0090] (1) Weigh equal moles of CsBr and PbBr2, dissolve them in DMSO solvent at 55°C, and stir for 2 h until the two salts are completely dissolved to prepare a 0.3 mol / L mixed solution of CsBr and PbBr2.
[0091] (2) The solution is cooled to room temperature, and acetonitrile is added dropwise to the mixed solution under vigorous stirring with a magnetic stirrer. As the acetonitrile solvent is titrated, a yellow substance is produced, but then it immediately dissolves. When the solution is close to saturation, a white precipitate that does not dissolve with stirring is produced. As the acetonitrile solvent is continued to be added dropwise, the yellow-orange substance no longer disappears, and the solution has reached a supersaturated state.
[0092] (3) The supersaturated solution is heated to 55° C. again and stirred for 24 h, then cooled to room temperature. The supernatant is filtered to obtain the precursor solution required for growing CsPbBr3 micrometer wires.
[0093] (4) The size is about 2×2cm 2 The glass substrate was first ultrasonically cleaned with acetone and anhydrous ethanol for 5 min each, then ultrasonically cleaned with deionized water for 15 min, and then dried with a nitrogen gun.
[0094] (5) The treated glass substrate is transferred to a polytetrafluoroethylene container containing 10 mL of acetonitrile solvent. A certain amount of precursor solution is dripped onto the surface of the glass substrate, and the container is sealed.
[0095] (6) The sealed container is placed in a forced air drying oven at 55° C. for 12 h to obtain randomly distributed CsPbBr3 micrometer wires.
[0096] (7) Using an optical microscope, CsPbBr3 microwires with perfect whispering gallery cavity structure were selected from randomly distributed CsPbBr3 microwires with a diameter and length of 10 μm and 150 μm, respectively, and transferred to a clean glass substrate spin-coated with PMMA.
[0097] (8) Under a stereo microscope, a CsPbBr3 micron wire with good crystal quality and perfect whispering gallery cavity structure was selected and covered with a thermal release tape, leaving the other end exposed.
[0098] (9) Use a pipette to draw up 20 μL of 37% concentrated hydrochloric acid, remove the pipette and seal its thick end, and place it together with the transferred microwires into a 13 cm × 3 cm (diameter × height) glass culture dish (with 35 g of anhydrous calcium chloride pre-placed at the bottom).
[0099] (10) Seal the mouth of the culture dish containing the sample with a film and place it in a 60°C forced air drying oven for 8 h.
[0100] (11) After the reaction was completed, the sample was placed on a heating table at 125 °C and heated for 25 s. After the thermal release tape was removed, it was further diffused to obtain a single CsPbCl with a gradient composition. x Br 3-x Perovskite microwires.
[0101] Comparative Example 1
[0102] The remaining steps of this comparative example are the same as those of Example 1, except that 30 g of anhydrous calcium chloride in step (9) is replaced by 0 g of anhydrous calcium chloride. x Br 3-x The surface of the microwires is degraded by moisture and even cracks appear, making it impossible to achieve a gradient composition of CsPbCl x Br 3-x Fabrication of perovskite microwires.
[0103] Comparative Example 2
[0104] The remaining steps of this comparative example are the same as those of Example 1, except that the reaction temperature in the blast drying oven in step (10) is replaced from 65°C to 60°C. x Br 3-x The diffusion region of the micrometer line is 60 to 70 nanometers, the shortest photoluminescence wavelength is around 470 to 480 nanometers, and the diffusion length is short.
[0105] Comparative Example 3
[0106] The remaining steps of this comparative example are the same as those of Example 1, except that the reaction temperature in the blast drying oven in step (10) is replaced from 65°C to 80°C. x Br 3-x The micrometer line diffusion region is 70-80 nanometers, the shortest photoluminescence wavelength is 450-470 nanometers, and CsPbCl x Br 3-x Cracks will appear on the micron lines.
[0107] Comparative Example 4
[0108] The remaining steps of this comparative example are the same as those of Example 1, except that the volume of concentrated hydrochloric acid in step (9) is replaced with 10 μL. x Br 3-xThe diffusion region of the micron wire is 50 to 60 nanometers, the shortest photoluminescence wavelength is 470 to 490 nanometers, and there is no break on the surface of the micron wire, but the exchange limit is not reached.
[0109] Comparative Example 5
[0110] The remaining steps of this comparative example are the same as those of Example 1, except that the volume of concentrated hydrochloric acid in step (9) is replaced with 40 μL. x Br 3-x The micron line diffusion region is 80-90 nanometers, and the shortest photoluminescence wavelength is 440-450 nanometers, but CsPbCl x Br 3-x The micrometer wires are broken in many places, destroying the original perfect echo gallery cavity structure. Figure 5 shown.
[0111] Among the above embodiments, embodiment 1 is the best embodiment.
Claims
1. A perovskite microwire with a gradient composition, characterized in that: Its molecular formula is: CsPbCl x Br 3-x , 1≤x≤3, the Cl and Br are both distributed in a gradient along the length direction of the perovskite micron wire, and the diameter of the perovskite micron wire is 3-10 μm and the length is 100-200 μm.
2. A method for preparing a perovskite microwire with a gradient composition, characterized in that: The following steps are involved: Step 1: Select CsPbBr3 micron wires with a diameter of 3 to 10 μm, good crystal quality, and perfect whispering gallery cavity structure; Step 2: Transfer the CsPbBr3 micrometer wires to a clean glass substrate spin-coated with PMMA; Step 3, covering one end of the CsPbBr3 micron wire with a thermal release tape, leaving the other end bare; Step 4: Take concentrated hydrochloric acid and put it into a glass culture dish with anhydrous calcium chloride together with the product obtained in step 3; Step 5, seal the mouth of the glass culture dish with a film and react at 60-80°C; Step six, heating the product obtained in step five at 115-125° C., removing the thermal release tape, and further diffusing to obtain perovskite microwires with a gradient composition.
3. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step 1, the preparation method of CsPbBr3 micrometer wire is: (1) Weighing equal moles of CsBr and PbBr2, dissolving them in a DMSO solvent at 45-55° C., and stirring until completely dissolved to obtain a mixed solution of CsBr and PbBr2; (2) While the mixed solution of CsBr and PbBr2 is being vigorously stirred, acetonitrile is added dropwise; (3) heating the solution obtained in step (2) to 45-55° C. again and stirring, then cooling to room temperature, filtering the supernatant to obtain a precursor solution; (4) The precursor solution is dropped onto the cleaned glass substrate surface, sealed, and reacted at 45-55° C. to obtain randomly distributed CsPbBr3 micrometer wires.
4. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step 1, the CsPbBr3 micron wire with good crystal quality is a CsPbBr3 micron wire with a complete structure, a smooth surface, no degradation, and no impurities.
5. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step 2, the transfer is to dip the probe into PMMA so that the needle tip has adhesion, and then the needle tip with PMMA is brought into contact with the selected CsPbBr3 micron wire under a microscope so that it adheres to the needle tip.
6. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step three, the thermal release tape is a hot melt adhesive material.
7. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step 4, the mass percentage of concentrated hydrochloric acid is 37wt%.
8. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step 4, the mass of anhydrous calcium chloride is 25-35 g.
9. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In the step 5, the reaction time is 6 to 8 hours.
10. The method for preparing a perovskite microwire with a gradient composition according to claim 2, characterized in that: In step six, the heating time is 25 to 35 seconds.
Citation Information
Cited By
Miniature perovskite thin film with components in gradient gradual change distribution and preparation method of miniature perovskite thin film
CN120981134A