Method for enhancing removal of structural alkali in red mud, obtained dealkalized red mud and application of dealkalized red mud
By ball milling the red mud with deionized water, pyrite-containing waste residue and oxidant, the problem of high red mud dealkalization cost and the introduction of impurities in the existing technology has been successfully solved, and efficient red mud dealkalization and resource utilization have been achieved. use.
Patent Information
- Application Number
- CN202410786431.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
Existing red mud dealkalization technology has problems such as high cost or the introduction of impurities, which limits the widespread use of red mud in industrial applications such as cement.
The red mud is mixed with deionized water, pyrite waste residue and oxidant, and ball milling reaction is carried out. The removal of structural alkali in the red mud is strengthened through refrigerated centrifugation and drying, and acidic substances are used to neutralize free alkali and structural alkali. , to achieve dealkalization of red mud.
It improves the dealkalization rate of red mud, reduces treatment costs, and reduces the dissolution of effective metals. It is suitable for industrial applications and meets the needs of solid waste recycling.
Smart Images

Figure CN118754472A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of red mud dealkalization, and in particular to a method for strengthening the removal of structural alkali in red mud, the obtained dealkalized red mud and applications thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Red mud, also known as red mud, is an industrial solid waste discharged after aluminum oxide is extracted from bauxite. It generally contains a large amount of iron oxide and looks similar to red soil, hence the name, but some are brown or even gray because they contain less iron oxide. If the aluminum content in bauxite is high, the Bayer process is used to smelt aluminum, and the red mud produced is called Bayer process red mud. If the aluminum content in bauxite is low, the sintering process or the sintering process and the Bayer process are used to smelt aluminum, and the red mud produced is called sintering process red mud or combined process red mud. Generally, for every ton of aluminum oxide produced, 1 to 2 tons of red mud are produced.
[0004] Due to the large output and strong alkalinity of red mud, it is difficult to be comprehensively utilized. Open-air stacking is its main disposal method, which not only wastes land resources, but also causes the pollution components in the red mud to seep in during the stacking process due to the red mud's own moisture and the leaching effect of rainfall, thus causing soil, surface water and groundwater pollution. The main components of Bayer red mud are Al2O3, SiO2, and Fe2O3. The chemical composition shows that it has large-scale application potential in the cement industry, but due to the strong alkalinity of red mud, the output cement has problems such as cracking, bulging, and frosting. Therefore, in order to realize the comprehensive application of red mud in industries such as cement and road construction materials, it is urgent to solve the problem of red mud dealkalization.
[0005] According to the existing form, the various alkaline substances in red mud can be divided into free alkali and structured alkali. Free alkali includes NaOH, NaAlO2, Na2CO3, Na2SiO3, etc. Free alkali is attached to the surface of red mud and can be removed by washing; structured alkali includes sodalite ([Na6Al6Si6O 24 ][2NaX]), cancrystal ([Na6Al6Si6O 24 ]·2CaCO3) and hydrogarnet (Ca3Al2(SiO4) x (OH) 12-4x ), etc. Structural alkali exists stably in red mud and needs to be removed through certain reactions. At present, the common methods for removing structural alkali mainly include lime de-alkali, salt replacement de-alkali, acid de-alkali and microbial de-alkali.
[0006] Lime de-alkali is to add lime to red mud to generate Ca2+ Under hydrothermal conditions, it can react with the free alkali in red mud. On the other hand, the Na + Can directly or indirectly interact with Ca 2+ The calcium-sodium replacement reaction occurs, so that the bound alkali in different forms is converted into free alkali and diffuses into the solution or forms a more stable insoluble substance, thereby achieving red mud dealkalization. This method has the advantages of low cost and good dealkalization effect, but there are problems such as large amount of lime and high cost, which limit the industrial application of this method. The salt replacement method is to add inorganic salts (such as CaCl2, MgCl2), precipitate and replace with red mud, convert free alkali into low-solubility hydroxides, carbonates, etc. and release Na + And de-alkali. However, this method has the problems of poor separation effect of red mud and sediment after the reaction, and the waste liquid containing calcium and magnesium ions has complex composition and is easy to introduce impurities. Acid de-alkali is to use acidic gas or acidic solution to react with alkali in red mud for de-alkali. Acid can completely neutralize the free alkali in red mud, and can also react with bound alkali, with a high de-alkali rate, but traditional acid-base neutralization (i.e. directly adding acid to red mud) uses a large amount of acid and is costly. In addition, for the industrial application of red mud in building materials, traditional acid-base neutralization will dissolve metal elements such as calcium and aluminum, resulting in the dissolution of effective metal ions in red mud, which affects the mechanical properties to a certain extent. Microbial de-alkali is also based on the principle of acid-base neutralization, and suitable microorganisms are screened to produce acid to reduce the alkalinity of red mud. However, microbial de-alkali has high cost and long cycle, and its application scenarios are relatively limited.
[0007] The commonly used red mud dealkalization methods currently have problems such as high cost or the introduction of impurities, which are not suitable for industrial treatment, and to some extent limit the industrial application of red mud. Therefore, it is urgent to explore and optimize the red mud dealkalization process, which can not only ensure the dealkalization rate, but also retain the effective metal components in the red mud and reduce the treatment cost. Summary of the invention
[0008] In order to overcome the above problems, the present invention provides a method for strengthening the removal of structural alkali in red mud, the obtained dealkalized red mud and its application.
[0009] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0010] The first aspect of the present invention provides a method for strengthening the removal of structural alkali in red mud, comprising:
[0011] After the red mud and deionized water are evenly mixed, pyrite slag and oxidant are added, and all reactants are transferred to a ball mill, which is sealed and ball milled; the mixed liquid after the reaction is collected, and solids are obtained by freeze centrifugation, and the obtained solids are dried to complete the removal of structural alkali in the red mud.
[0012] The second aspect of the present invention provides dealkalized red mud prepared by the above preparation method.
[0013] The third aspect of the present invention provides the use of the above-mentioned dealkalized red mud in the preparation of cement materials.
[0014] The beneficial effects of the present invention are:
[0015] (1) Pyrite-containing waste residue will be fully oxidized by oxidants in water to generate acidic substances, which will neutralize the free alkali and structural alkali in red mud, thereby achieving the removal of free alkali and structural alkali in red mud. Taking pyrite and hydrogen peroxide as an example, the reaction equations involved in the reaction process include:
[0016]
[0017] 2 2+ +2O2+2H + →2Fe 3+ +2H2O
[0018]
[0019] Fe 3+ +3H2O→Fe(OH)3+3H +
[0020] First, ferrous disulfide will be oxidized by hydrogen peroxide to generate ferrous ions and acid. Ferrous ions will be further oxidized to ferric ions. The ferric ions will react with ferrous disulfide to further generate acid. At the same time, the ferric ions will also hydrolyze to generate acid. Therefore, the introduction of hydrogen peroxide can not only achieve the 2+ The oxidation of 3+ To produce acid, it can also directly oxidize S2 2- Produce acid, accelerate the FeS2 dual-driven acid production rate, and achieve effective dealkalization of red mud.
[0021] (2) The present invention adopts a ball milling method to better crush the red mud, accelerate the release of structural alkali in the red mud, and at the same time make the red mud-sulfur-containing iron ore waste slag-oxidant coupling system react more fully, which is beneficial to the removal of alkali in the red mud.
[0022] (3) Compared with the existing technology, the greatest advantage of the present invention is that it can enhance the removal of structural alkali in red mud, improve the dealkalization rate of red mud, and at the same time improve the iron grade of red mud and reduce the dissolution of effective metals (iron) in red mud, thus providing favorable conditions for the industrial application of red mud after dealkalization.
[0023] (4) The present invention is based on the concept of "treating waste with waste" and uses industrial waste slag pyrite to produce acid through oxidation, which is more in line with the current demand for solid waste resource utilization.
[0024] (5) The cost of the present invention is lower than that of the existing dealkalization technology and is more suitable for practical engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0026] Figure 1 is the pH of each group in the aqueous solution homogeneous system in Example 1;
[0027] Figure 2 is the pH of each group under the ball milling system in Example 2 and the Na in the leaching solution + concentration;
[0028] Figure 3 This is a comparison diagram of the dealkalization effects of the stirring system and the ball milling system in Example 3. DETAILED DESCRIPTION
[0029] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0031] A first typical embodiment of the present invention provides a method for enhancing the removal of structural alkali in red mud, comprising:
[0032] After the red mud and deionized water are evenly mixed, pyrite slag and oxidant are added, and all reactants are transferred to a ball mill, which is sealed and ball milled; the mixed liquid after the reaction is collected, and solids are obtained by freeze centrifugation, and the obtained solids are dried to complete the removal of structural alkali in the red mud.
[0033] In one or more embodiments, the mass ratio of the red mud to deionized water is 1:5 to 1:10.
[0034] In one or more embodiments, the pyrite in the pyrite-containing waste slag includes makinoite, pyrite, pyroxene, etc., preferably pyrite.
[0035] In one or more embodiments, the oxidant includes oxidizing substances such as H2O2, CaO2, potassium permanganate, persulfate, oxygen-enriched water, etc., preferably H2O2.
[0036] In one or more embodiments, the molar ratio of the pyrite-containing waste slag to the oxidant is 1:4 to 1:6.
[0037] In one or more embodiments, the ball milling beads include small balls, medium balls or large balls; wherein the particle size of the small balls is 0.5-1 mm, the particle size of the medium balls is 3-5 mm, and the particle size of the large balls is 6-10 mm.
[0038] Preferably, when small balls are used, the mass ratio of small balls to materials is 5:1-10:1; when medium balls are used, the mass ratio of medium balls to materials is 5:1-10:1; when large balls are used, the number of large balls is 4-12.
[0039] In one or more embodiments, the rotation speed of the ball mill is 100-1000 rpm, the rotation time of each circle is 15-30 minutes, the pause time of each circle is 1-5 minutes; the total number of positive and negative rotation circles is 20-40 circles.
[0040] In one or more embodiments, the rotation speed of the refrigerated centrifuge is 8000-10000 rpm, the centrifugation temperature is 4-25° C., and the centrifugation time is 5-15 min.
[0041] A second typical embodiment of the present invention provides dealkalized red mud prepared by the above method.
[0042] A third typical embodiment of the present invention provides the use of the above-mentioned dealkalized red mud in the preparation of cement materials.
[0043] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0044] Example 1
[0045] This example illustrates the acid-generating capacity of pyrite, and the addition of hydrogen peroxide can enhance the oxidation rate and acid-generating capacity of pyrite.
[0046] Group 1: Take 5g of red mud in a beaker with a solid-liquid ratio of 1:6, add 30mL of deionized water into the beaker, and stir evenly with a glass rod.
[0047] Group 2: Weigh 0.5 g FeS2 into a beaker, add 30 mL deionized water, and stir evenly with a glass rod.
[0048] Group 3: Measure 30 mL of deionized water into a beaker, add 2 mL of H2O2, and stir well.
[0049] Group 4: Weigh 0.5 g FeS2 into a beaker, add 30 mL deionized water, and add 2 mL H2O2, and stir evenly with a glass rod.
[0050] The pH of the solutions in groups 1 to 4 was measured using a pH meter.
[0051] The results are as follows Figure 1 As shown, the pH in group 1 was 10.83, indicating that free alkali was released after red mud dissolved in water, confirming the strong alkalinity of red mud. The pH in group 2 was 2.4, indicating that FeS2 was acidified by oxygen in the air. The pH in group 3 was 5.19, and the pH in group 4 was 2.36, indicating that the introduction of H2O2 can increase the acid production capacity during the oxidation of FeS2.
[0052] Embodiment 2:
[0053] In this embodiment, free alkali and most of the structural alkali in the red mud are removed by ball milling red mud + FeS2 + H2O2, verifying the strong de-alkali ability of the red mud + reducing waste residue + oxidant ball milling system.
[0054] Group 1: Weigh 5 g of red mud, add 30 mL of deionized water and stir well.
[0055] Group 2: Weigh 5 g red mud and 0.5 g FeS2, add 30 mL deionized water and stir well.
[0056] Group 3: Weigh 5 g red mud and 0.5 g FeS2, add 30 mL deionized water and 2 mL H2O2 and stir evenly.
[0057] The mixed solutions of groups 1, 2, and 3 were transferred to ball mills respectively, and a certain mass of ball mill beads (mass ratio of ball to material was 5:1) was added. The speed of the ball mill was set to 1000 rpm, the rotation time of each circle was 20 minutes, the pause time of each circle was 1 minute, and the total number of positive and negative rotations was 40 circles. After the ball milling was completed, the ball and material were separated, and the pH of the obtained mixed solution was measured with a pH meter. The mixed solution was centrifuged, and the speed of the refrigerated centrifuge was set to 10000 rpm, the temperature was 4°C, and the centrifugation time was 5 minutes. The supernatant was retained and the Na in the aqueous phase was measured by ion chromatography. + The solid phase is naturally dried to obtain the dealkalized red mud.
[0058] The results are as follows Figure 2 The pH of the mixture after ball milling of water and red mud was 11.14, which was greater than the pH before ball milling (10.83), indicating that mechanical ball milling can play a role in crushing and accelerate the release of structural alkali in red mud. After adding FeS2 to the red mud and ball milling, it was found that the pH was somewhat lower than that of group 1. Na is the main alkaline element in red mud.+ The concentration of Na in group 2 solution represents the dealkalization effect of red mud to a certain extent. + The concentration (11.95 g / L) was also slightly higher than that of group 1 (10.58 g / L), which was consistent with the pH result. After adding FeS2 and H2O2 to the red mud and milling, it was found that the pH (7.44) was significantly lower than that of group 1 and group 2. + The concentration of (19.83 g / L) also increased accordingly. The better dealkalization effect of group 3 is attributed to the addition of oxidant, i.e., H2O2, in the system. The introduction of hydrogen peroxide can not only achieve the 2+ The oxidation of 3+ To produce acid, it can also directly oxidize S2 2- Acid production can accelerate the FeS2 dual-driven acid production rate and achieve effective dealkalization of red mud. This is also consistent with the experimental results in Example 1.
[0059] Example 3
[0060] This embodiment compares the dealkalization effects of the same group in a stirring system and a ball milling system, highlighting the superiority of mechanical ball milling.
[0061] The same three groups as in Example 2 were set up, namely Group 1, Group 2 and Group 3. Rotors were added to the beakers of the three groups respectively, and placed on a magnetic stirrer for stirring reaction. The speed of the magnetic stirrer was set to 300 rpm, and the stirring time was set to 12 h. The rest of the operations were the same as in Example 2. The main dealkalization index in this example was Na in the solution. + concentration.
[0062] The results are as follows Figure 3 As shown. The same groups were compared and it was found that the dealkalization effect of the ball milling system in the same group was better than that of the stirring system. In particular, for Group 3, the dealkalization rate of the ball milling system was much higher than that of the stirring system, which also shows that compared with the stirring system, mechanical ball milling can better promote the dealkalization of the red mud-pyrite waste slag-oxidant coupling system. The addition of the ball milling system, pyrite waste slag and oxidant is an indispensable factor in accelerating the dealkalization of red mud in the present invention.
[0063] Example 4
[0064] This study focused on the SO4 2- dissolution condition.
[0065] The supernatant of group 3 after centrifugation in Example 2 was taken and SO4 was measured by ion chromatography. 2- The concentration was calculated as follows to explore the risk of sulfur dissolution after red mud dealkalization.
[0066] FeS2 dosage (10%): 0.5g
[0067] Theoretically, SO4 can be produced 2- : 0.8g, converted to a concentration of 26666.7mg / L
[0068] After measurement, FeS2 and red mud were ball-milled and SO4 was dissolved with the solution. 2- Actual concentration: 15847.19 mg / L;
[0069] SO4 2- Dissolution rate: 15847.19 / 26666.7*100%=60%;
[0070] The maximum residual amount of S in red mud after ball milling: 1.33%;
[0071] The above calculation process shows that the SO4 generated in the system 2- Most of it enters the water phase, while the sulfur remaining in the red mud exists in the form of low-valent sulfur, which can generate H2S under high temperature conditions and be volatilized and removed. Therefore, the sulfur content in the red mud obtained by dealkalization in the present invention meets the sulfur content requirements of raw materials in the cement industry and the requirements of building materials, which is convenient for direct industrial utilization of dealkalized red mud.
[0072] Embodiment 5:
[0073] This embodiment compares the Na content of red mud leachate from ball-milled organic acid system and the system of the present invention. + concentrations, and the raw material costs of the two treatment technologies were compared.
[0074] The amount of red mud was 5 g, citric acid was selected as a typical organic acid, the amount of citric acid was 70 mM, and the volume of deionized water was 30 mL for ball milling. + , the remaining operations are consistent with those in Example 2.
[0075] The results are shown in Table 1. When the dealkalization rates of the two groups are close, the cost of the industrial-grade raw materials used in the two groups is calculated, and it is found that the cost of treating 1 ton of red mud by the present invention is lower than that of the traditional acid-base neutralization process. In addition, the price of FeS2 is the industrial price of high-grade pyrite. In practical applications, sulfur-containing tailings can be used instead of industrial-grade FeS2, which can not only further reduce the treatment cost of red mud dealkalization, but also realize the resource utilization of sulfur-containing tailings.
[0076] Table 1. Comparison of the dealkalization effect and raw material cost of organic acid and the present invention
[0077]
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for strengthening the removal of structural alkali in red mud, characterized in that: include: After the red mud and deionized water are evenly mixed, pyrite slag and oxidant are added, and all reactants are transferred to a ball mill, which is sealed and ball milled; the mixed liquid after the reaction is collected, and solids are obtained by freeze centrifugation, and the obtained solids are dried to complete the removal of structural alkali in the red mud.
2. The method according to claim 1, characterized in that The mass ratio of the red mud to deionized water is 1:5 to 1:
10.
3. The method according to claim 1, characterized in that The pyrite in the pyrite waste slag includes makinoite, pyrite and pyroxene, preferably pyrite.
4. The method according to claim 1, characterized in that The oxidant includes H2O2, CaO2, potassium permanganate, persulfate, oxygen-enriched water, preferably H2O2.
5. The method according to claim 1, characterized in that The molar ratio of the pyrite-containing waste slag to the oxidant is 1:4 to 1:
6.
6. The method according to claim 1, characterized in that The rotation speed of the ball mill is 100-1000 rpm, the rotation time of each circle is 15-30 minutes, the pause time of each circle is 1-5 minutes; the total number of positive and negative rotation circles is 20-40 circles.
7. The method according to claim 1, characterized in that The rotation speed of the refrigerated centrifuge is 8000-10000 rpm, the centrifugal temperature is 4-25°C, and the centrifugal time is 5-15 minutes.
8. The method according to claim 1, characterized in that Ball mill beads include small balls, medium balls or large balls; the particle size of small balls is 0.5-1mm, the particle size of medium balls is 3-5mm, and the particle size of large balls is 6-10mm; Preferably, when small balls are used, the mass ratio of small balls to materials is 5:1-10:1; when medium balls are used, the mass ratio of medium balls to materials is 5:1-10:1; when large balls are used, the number of large balls is 4-12.
9. Dealkalized red mud prepared by the method according to any one of claims 1 to 8.
10. Use of the dealkalized red mud according to claim 9 in preparing cement materials.
Citation Information
Patent Citations
Red mud dealkalization method
CN101423318A
Dealkalizing method of Bayer process red mud
CN108585005A
Circulating water type dealkalization system and method for red mud by sulfur-containing tailings
CN110482821A
Manufacturing process of finished cement added with Bayer process red mud
CN111747665A
Building material containing treated bauxite waste and method for producing the same
JP2004530544A