A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting.

By combining ultrasonic conditioning with low-temperature roasting, the agglomeration structure of red mud is destroyed and the mineral phase is reconstructed, which solves the problems of incomplete dehydration and insufficient dealkalization in red mud treatment, realizes the efficient resource utilization of red mud, and reduces energy consumption and pollution.

CN123105690APending Publication Date: 2026-11-17SHANDONG HI SPEED GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611305979.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing red mud treatment technologies suffer from problems such as incomplete dehydration, insufficient dealkalization depth, strong mineral phase inertness, cumbersome processes, high energy consumption, serious secondary pollution, and low resource utilization rate, making it impossible to achieve simultaneous and efficient completion of dehydration, dealkalization, and mineral phase reconstruction.

Method used

By employing a combined approach of ultrasonic conditioning and low-temperature roasting, the ultrasonic cavitation effect disrupts the agglomeration structure of red mud. Combined with the low-temperature roasting process, this achieves deep dehydration, deep dealkalization, and mineral phase reconstruction of red mud, thus constructing an integrated synergistic system.

Benefits of technology

It achieves low-temperature, energy-saving, simultaneous, efficient, and environmentally friendly resource utilization of red mud. The deep treatment of red mud reduces the pH to 6.5-8.0, the total dealkali rate is ≥ 95%, the water content is ≤ 8%, the active SiO2 content is ≥ 10%, and the active Al2O3 content is ≥ 7%, which greatly reduces energy consumption and operating costs, avoids secondary pollution, and improves the resource utilization rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of red mud solid waste resource utilization technology, and particularly to a method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting. This invention utilizes the ultrasonic cavitation effect to pretreat red mud slurry, disrupting its agglomeration structure and enhancing mass transfer efficiency. Combined with a low-temperature roasting process, it achieves simultaneous deep dehydration, deep dealkalization, and active mineral phase reconstruction of red mud, constructing an integrated synergistic system of "ultrasonic conditioning-low-temperature roasting-mineral phase reconstruction." This achieves the goals of "low-temperature energy saving, simultaneous high efficiency, green environmental protection, and resource utilization." The red mud treated by this invention can be directly used to prepare high-value-added products such as cementitious materials, adsorbents, and soil conditioners, significantly improving the resource utilization rate of red mud.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of red mud solid waste resource utilization technology, and in particular to a method for red mud ultrasonic conditioning-low temperature roasting synergistic dehydration, dealkalization and mineral phase reconstruction. Background Technology

[0002] Red mud is characterized by high water content, high alkalinity, and the inertness of sialic acid minerals. The high water content and high alkalinity lead to the accumulation of red mud and the generation of alkaline leachate that pollutes the environment, thus limiting the comprehensive utilization of red mud. The inertness of sialic acid minerals results in low activity of red mud, making it difficult to be effectively utilized. Most of it relies on stockpiling for disposal, causing serious waste of resources and environmental pressure.

[0003] Currently, red mud dewatering, dealkalization, and mineral phase activation mostly employ step-by-step processing or single-process technologies. Although existing technologies have made some improvements, they still have many limitations that are difficult to overcome. They generally suffer from technical dilemmas such as "incomplete dewatering, insufficient dealkalization depth, strong mineral phase inertness, cumbersome processes, high energy consumption, serious secondary pollution, and low resource utilization rate," making it impossible to achieve simultaneous and efficient completion of dewatering, dealkalization, and mineral phase reconstruction. Summary of the Invention

[0004] In view of this, the present invention provides a method for the synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting. This invention utilizes the ultrasonic cavitation effect to pretreat red mud slurry, disrupting the agglomerate structure and enhancing mass transfer efficiency. Combined with a low-temperature roasting process, it achieves simultaneous deep dehydration, deep dealkalization, and active mineral phase reconstruction of red mud, constructing an integrated synergistic system of "ultrasonic conditioning-low-temperature roasting-mineral phase reconstruction," achieving the goals of "low-temperature energy saving, simultaneous high efficiency, green environmental protection, and resource utilization."

[0005] To achieve the above objectives, the present invention is implemented through the following technical solution: This invention provides a method for the synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting, comprising the following steps: The red mud was stirred to obtain a homogenized red mud slurry; The homogenized red mud slurry was ultrasonically treated and dried to obtain dried red mud particles. Dry red mud particles are calcined under an inert atmosphere to obtain deeply treated red mud. The deeply processed red mud is cooled and pulverized to obtain red mud powder.

[0006] Furthermore, the red mud is Bayer process red mud.

[0007] Furthermore, the stirring time is 20-60 minutes.

[0008] Furthermore, the ultrasonic treatment employs dual-frequency ultrasonic synergy, with ultrasonic frequencies of 20-40 kHz (low frequency) and 80-100 kHz (high frequency) working together.

[0009] Furthermore, the ultrasonic power is 300-500 W, the ultrasonic time is 20-40 min, the ultrasonic temperature is controlled at 25-45℃, and continuous stirring is carried out during the ultrasonic process at a stirring speed of 60-100 r / min.

[0010] Furthermore, the drying operation involves drying at 120-150 ℃ until the moisture content is ≤ 15%.

[0011] Furthermore, the calcination process employs a two-stage calcination method, with the inert gas flow rate controlled at 0.5-1.0 L / min; the first stage calcination temperature is 180-220 ℃, and the calcination time is 1.0-2.0 h; the second stage calcination temperature is increased to 250-300 ℃, and the calcination time is 2.0-3.0 h.

[0012] Furthermore, the inert gas is either nitrogen or argon.

[0013] Furthermore, the deep-treated red mud has a pH reduced to 6.5-8.0, a total dealkali removal rate of ≥ 95%, a moisture content of ≤ 8%, an active SiO2 content of ≥ 10%, and an active Al2O3 content of ≥ 7%.

[0014] Further, the deep-processed red mud is cooled to room temperature and pulverized to a particle size ≤ 120 mesh.

[0015] Furthermore, the alkaline volatiles generated during the roasting process are condensed and recovered, neutralized with dilute hydrochloric acid, and a mixed solution of sodium chloride and potassium chloride is obtained. After evaporation, concentration, cooling and crystallization, the solution is recycled as an industrial raw material.

[0016] Furthermore, the concentration of dilute hydrochloric acid was 5%, the neutralization temperature was 40 °C, and the purity of the resulting mixed crystals was ≥ 94%.

[0017] Compared with the prior art, the present invention has achieved the following beneficial effects: This invention achieves deep dehydration, deep dealkalization, and mineral phase reconstruction of red mud simultaneously through the synergistic effect of ultrasonic conditioning and low-temperature roasting. It solves the problems of low efficiency and poor effect of existing step-by-step treatment technologies. The deep-treated red mud achieves a pH reduction to 6.5-8.0, a total dealkalization rate of ≥95%, a moisture content of ≤8%, an active SiO2 content of ≥10%, and an active Al2O3 content of ≥7%. Ultrasonic conditioning has low energy consumption, and its synergistic effect with low-temperature roasting further reduces overall energy consumption; the energy consumption for treating 1 ton of red mud is ≤35 kWh, significantly saving operating costs. This invention requires no chemical reagents, avoiding secondary pollution from chemical conditioning agents; the low-temperature roasting process generates no harmful gases, alkaline volatiles are neutralized and recycled, inert gases are recycled, and there is no wastewater or waste gas emission. The filter residue is disposed of harmlessly, truly achieving "zero pollution" emissions, which aligns with the concept of green and low-carbon development. This invention achieves lattice reconstruction of the inert mineral phase of red mud through low-temperature roasting, generating an active silica-alumina mineral phase. The deeply treated red mud can be directly used to prepare high-value-added products such as cementitious materials, adsorbents, and soil conditioners, significantly improving the resource utilization rate of red mud. Detailed Implementation

[0018] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0019] This invention provides a method for the synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting, comprising the following steps: The red mud was stirred to obtain a homogenized red mud slurry; The homogenized red mud slurry was ultrasonically treated and dried to obtain dried red mud particles. Dry red mud particles are calcined under an inert atmosphere to obtain deeply treated red mud. The deeply processed red mud is cooled and pulverized to obtain red mud powder.

[0020] Existing red mud treatment processes separate dehydration, dealkalization, and mineral phase reconstruction into independent steps. This step-by-step approach is not only cumbersome and complex, but also prone to interference between steps. Incomplete dehydration affects the efficiency of subsequent dealkalization, and the dealkalization process easily damages the red mud mineral phase structure, leading to a decrease in mineral phase activation and ultimately resulting in high red mud treatment costs and low resource utilization rates. Current technologies lack an integrated process of "ultrasonic conditioning-low-temperature roasting synergy," making it impossible to simultaneously complete dehydration, dealkalization, and mineral phase reconstruction. Furthermore, it fails to leverage the ultrasonic cavitation effect to enhance mass transfer and improve the efficiency and effectiveness of low-temperature roasting, thus failing to meet the demands for large-scale, efficient, and green red mud treatment. This invention overcomes the limitations of existing red mud treatment processes that involve "step-by-step dehydration, dealkalization, and mineral phase reconstruction, resulting in high energy consumption, low efficiency, and poor synergy." It constructs an integrated system of "ultrasonic conditioning-low-temperature roasting synergy," utilizing the ultrasonic cavitation effect to enhance mass transfer and achieve simultaneous and efficient completion of dehydration, dealkalization, and mineral phase reconstruction.

[0021] Furthermore, the initial water content of red mud can be as high as 80%, for example, 60-75%; the pH can be 10-14; the total alkali content can be 6-9.5%; and the bound alkali content can be 5-8%.

[0022] Furthermore, the red mud is Bayer process red mud.

[0023] Furthermore, the stirring time is 20-60 minutes. The stirring time can be any value between 20-60 minutes, such as 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, etc. The homogenized red mud slurry obtained through stirring lays the foundation for the full utilization of the ultrasonic cavitation effect during subsequent ultrasonic conditioning, ensuring that ultrasonic energy is uniformly transferred to the interior of the red mud particles.

[0024] Furthermore, the ultrasonic treatment employs a dual-frequency ultrasonic synergy, with specific parameters controlled as follows: a dual-frequency synergy of 20-40 kHz (low frequency) and 80-100 kHz (high frequency). The ultrasonic frequency can be any value between 20-40 kHz and 80-100 kHz, such as 25 kHz, 30 kHz, 35 kHz; 85 kHz, 90 kHz, 95 kHz, etc.

[0025] Furthermore, the ultrasonic power is 300-500 W, the ultrasonic time is 20-40 min, the ultrasonic temperature is controlled at 25-45℃, and continuous stirring is performed during the ultrasonic process at a stirring speed of 60-100 r / min. The ultrasonic power can be any value between 300-500 W, such as 350 W, 400 W, 450 W, etc.; the ultrasonic temperature can be controlled at any value between 25-45℃, such as 30℃, 35℃, 40℃, etc.; and the stirring speed can be any value between 60-100 r / min, such as 70 r / min, 80 r / min, 90 r / min, etc.

[0026] A dual-frequency ultrasonic synergistic approach is employed, utilizing the ultrasonic cavitation effect to disrupt the red mud structure and enhance mass transfer. Low-frequency ultrasound disrupts the agglomeration structure of red mud particles and the surface adsorbed water film, while high-frequency ultrasound enhances internal mass transfer, promoting the migration of alkaline components and the removal of moisture. The synergistic effect of these two approaches maximizes the ultrasonic cavitation effect, not only promoting moisture removal and alkaline component migration but also slightly disrupting the surface lattice of inert mineral phases. This creates conditions for subsequent low-temperature roasting and mineral phase reconstruction, unlike existing single-mode ultrasonic pretreatment which only achieves simple dispersion. Strict control of ultrasonic parameters and continuous stirring during the ultrasonic process ensure uniform distribution of ultrasonic energy and prevent inadequate conditioning of localized red mud particles. During ultrasonic conditioning, the microbubbles generated by ultrasonic cavitation rapidly form and burst, releasing a large amount of energy. On the one hand, this disrupts the agglomeration structure of red mud particles, making them more uniformly dispersed and increasing their specific surface area. It also breaks down the hydrophilic adsorbed water film on the surface of the red mud particles, promoting the removal of both free and bound water. On the other hand, ultrasonic cavitation enhances the mass transfer efficiency within the red mud slurry, promoting the dissolution of free alkali and the initial dissociation of bound alkali, laying the foundation for subsequent low-temperature roasting and dealkali removal. Simultaneously, ultrasonic conditioning can slightly disrupt the surface lattice of the inert mineral phases in red mud, creating conditions for subsequent low-temperature roasting and mineral phase reconstruction.

[0027] Furthermore, the drying operation involves drying at 120-150 ℃ until the moisture content is ≤ 15%.

[0028] Furthermore, the calcination process employs a two-stage calcination method, with the inert gas flow rate controlled at 0.5-1.0 L / min; the first stage calcination temperature is 180-220 ℃, and the calcination time is 1.0-2.0 h; the second stage calcination temperature is increased to 250-300 ℃, and the calcination time is 2.0-3.0 h.

[0029] Furthermore, the inert gas is either nitrogen or argon. An inert atmosphere can block the secondary combination reaction between active oxides and oxygen in red mud, preventing free alkali from being refixed into bound alkali.

[0030] The first roasting stage primarily removes bound water and residual free water from the red mud particles, while further removing free alkalis (NaOH, KOH, Na2CO3). Free alkalis are removed through volatilization and decomposition. After this stage, the red mud moisture content drops to ≤ 8%, and the free alkali removal rate is ≥ 95%. The second roasting stage achieves deep removal of bound alkalis and reconstruction of active mineral phases: bound alkalis (basic groups in nepheline, nepheline, and sodalite) undergo decomposition reactions under low-temperature conditions, dissociating Na... + K + It reacts slightly with the silica-alumina components in the red mud to achieve deep removal of bound alkali; at the same time, during the roasting process, the inert silica-alumina mineral phases (calcium nepheline, nepheline, etc.) in the red mud undergo lattice reconstruction and are transformed into active silica-alumina mineral phases (metakaolinite, active SiO2, active Al2O3, etc.), thereby enhancing the resource utilization activity of the red mud.

[0031] Furthermore, the deep-treated red mud has a pH reduced to 6.5-8.0, a total dealkali removal rate of ≥ 95%, a moisture content of ≤ 8%, an active SiO2 content of ≥ 10%, and an active Al2O3 content of ≥ 7%.

[0032] Further, the deep-processed red mud is cooled to room temperature and pulverized to a particle size ≤ 120 mesh.

[0033] Furthermore, the alkaline volatiles generated during the roasting process are condensed and recovered, then neutralized with dilute hydrochloric acid to obtain a mixed solution of sodium chloride and potassium chloride. This solution is then concentrated by evaporation, cooled, and crystallized before being recycled as an industrial raw material. The inert gases generated during roasting are purified and recycled for use in the low-temperature roasting process. The entire process produces no wastewater or waste gas emissions, aligning with the concept of green and low-carbon development.

[0034] Furthermore, the concentration of dilute hydrochloric acid was 5%, the neutralization temperature was 40 °C, and the purity of the resulting mixed crystals was ≥ 94%.

[0035] This invention achieves synergistic coupling of "ultrasonic conditioning and low-temperature roasting," overcoming the limitations of existing single or step-by-step treatments. Ultrasonic conditioning utilizes the cavitation effect to disrupt the agglomerate structure of red mud and enhance mass transfer, laying the foundation for low-temperature roasting. Low-temperature roasting, based on ultrasonic pretreatment, simultaneously achieves deep dehydration, deep dealkalization, and mineral phase reconstruction. The two processes work synergistically, solving the core technical bottlenecks of incomplete dehydration, insufficient dealkalization depth, and strong mineral phase inertness in existing technologies. This results in a processing efficiency increase of over 50% and an energy consumption reduction of over 60% compared to existing step-by-step processes. Furthermore, this invention constructs a fully closed-loop system of "roasting volatiles recovery - inert gas circulation," overcoming the limitations of existing processes in terms of resource waste and secondary pollution. The alkaline volatiles generated during low-temperature roasting are neutralized and recovered to prepare industrial raw materials, and the purified inert gas is recycled, resulting in no wastewater or waste gas emissions. Simultaneously, ultrasonic conditioning eliminates the need for chemical reagents, avoiding secondary pollution and truly achieving "green, low-carbon, and resource-recycling."

[0036] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0037] Example 1 A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting includes the following steps: 1. Red mud pretreatment: Bayer process red mud (initial water content 72%, pH 12.9, total alkali content 8.2%, of which bound alkali content 6.1%, SiO2 content 21%, Al2O3 content 16%) was fed into a mixing tank and stirred for 30 min to obtain homogenized red mud slurry.

[0038] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry is fed into an ultrasonic conditioning device, using a dual-frequency combination of 30 kHz (low frequency) and 90 kHz (high frequency), with an ultrasonic power of 400 W, an ultrasonic temperature of 35 ℃, an ultrasonic time of 30 min, and a stirring speed of 80 r / min.

[0039] 3. Low-temperature roasting and co-treatment: The ultrasonically pretreated red mud slurry was fed into a spray dryer and dried at 135 ℃ to a moisture content of 12% to obtain dried red mud particles; the dried red mud particles were then fed into a low-temperature roasting furnace under nitrogen protection (flow rate 0.8 L / min) for staged roasting: roasting at 200 ℃ for 1.5 h, and then raising the temperature to 280 ℃ for 2.5 h; after roasting, deeply treated red mud was obtained with a pH of 7.0, a total dealkali removal rate of 96.3%, a moisture content of 6.8%, an active SiO2 content of 11.2%, and an active Al2O3 content of 8.3%.

[0040] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, and cooled and crystallized to obtain sodium chloride-potassium chloride mixed crystals (purity 95.6%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 92%.

[0041] In this embodiment, the finished red mud powder can be directly used to prepare soil conditioner, and its performance meets relevant industry standards; the comprehensive processing cost is 40 yuan / ton, which is 58% lower than the existing step-by-step process, and the energy consumption is 28 kWh / ton, which is 72% lower than the existing high-temperature process.

[0042] Example 2 A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting includes the following steps: 1. Red mud pretreatment: Bayer process red mud (initial water content 75%, pH 13.5, total alkali content 9.1%, of which bound alkali content 6.8%, SiO2 content 20%, Al2O3 content 18%) was fed into a mixing tank and stirred for 25 min to obtain homogenized red mud slurry.

[0043] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry is fed into an ultrasonic conditioning device, using a dual-frequency combination of 40 kHz (low frequency) and 100 kHz (high frequency), with an ultrasonic power of 500 W, an ultrasonic temperature of 45 ℃, an ultrasonic time of 40 min, and a stirring speed of 100 r / min.

[0044] 3. Low-temperature roasting and co-treatment: The ultrasonically pretreated red mud slurry was fed into a spray dryer and dried at 150 ℃ to a moisture content of 10% to obtain dried red mud particles; the dried red mud particles were then fed into a low-temperature roasting furnace under nitrogen protection (flow rate 1.0 L / min) and roasted in stages: roasted at 220 ℃ for 2.0 h, and then heated to 300 ℃ for 3.0 h; after roasting, deeply treated red mud was obtained with a pH of 6.5, a total dealkalization rate of 97.5%, a moisture content of 6.2%, an active SiO2 content of 11.8%, and an active Al2O3 content of 8.7%.

[0045] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, and cooled and crystallized to obtain sodium chloride-potassium chloride mixed crystals (purity 94.8%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 91.2%.

[0046] In this embodiment, the finished red mud powder can be directly used to prepare soil conditioner, and its performance meets relevant industry standards; the comprehensive processing cost is 42 yuan / ton, which is 56% lower than the existing step-by-step process, and the energy consumption is 30 kWh / ton, which is 70% lower than the existing high-temperature process.

[0047] Example 3 A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting includes the following steps: 1. Red mud pretreatment: Bayer process red mud (initial water content 68%, pH 11.5, total alkali content 6.5%, of which bound alkali content 4.2%, SiO2 content 23%, Al2O3 content 17%) was fed into a mixing tank and stirred for 35 min to obtain homogenized red mud slurry.

[0048] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry is fed into an ultrasonic conditioning device, using a dual-frequency combination of 20 kHz (low frequency) and 80 kHz (high frequency), with an ultrasonic power of 300 W, an ultrasonic temperature of 25 ℃, an ultrasonic time of 20 min, and a stirring speed of 60 r / min.

[0049] 3. Low-temperature roasting and co-treatment: The ultrasonically pretreated red mud slurry was fed into a spray dryer and dried at 120 ℃ to a moisture content of 15% to obtain dried red mud particles; the dried red mud particles were fed into a low-temperature roasting furnace under nitrogen protection (flow rate 0.5 L / min) and roasted in stages: roasted at 180 ℃ for 1.0 h, and then heated to 250 ℃ for 2.0 h; after roasting, deeply treated red mud was obtained with pH 8.0, total dealkali removal rate of 95.1%, moisture content of 7.9%, active SiO2 content of 10.1%, and active Al2O3 content of 7.2%.

[0050] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, and cooled and crystallized to obtain sodium chloride-potassium chloride mixed crystals (purity 95.1%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 91.3%.

[0051] In this embodiment, the finished red mud powder can be directly used to prepare soil conditioner, and its performance meets relevant industry standards; the comprehensive processing cost is 41 yuan / ton, which is 57% lower than the existing step-by-step process, and the energy consumption is 29 kWh / ton, which is 71% lower than the existing high-temperature process.

[0052] Example 4 A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting includes the following steps: 1. Red mud pretreatment: Bayer process red mud (initial water content 70%, pH 12.2, total alkali content 7.3%, of which bound alkali content 5.1%, SiO2 content 21%, Al2O3 content 14%) was fed into a mixing tank and stirred for 32 min to obtain homogenized red mud slurry.

[0053] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry was fed into an ultrasonic conditioning device, using a dual-frequency combination of 25 kHz (low frequency) and 85 kHz (high frequency), with an ultrasonic power of 350 W, an ultrasonic temperature of 30 ℃, an ultrasonic time of 25 min, and a stirring speed of 70 r / min.

[0054] 3. Low-temperature roasting and co-treatment: The ultrasonically pretreated red mud slurry was fed into a spray dryer and dried at 130 ℃ to a moisture content of 13% to obtain dried red mud particles; the dried red mud particles were then fed into a low-temperature roasting furnace under nitrogen protection (flow rate 0.6 L / min) for staged roasting: roasting at 190 ℃ for 1.2 h, and then raising the temperature to 260 ℃ for 2.2 h; after roasting, deeply treated red mud was obtained with a pH of 7.6, a total dealkalization rate of 95.7%, a moisture content of 7.5%, an active SiO2 content of 10.5%, and an active Al2O3 content of 7.6%.

[0055] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, and cooled and crystallized to obtain sodium chloride-potassium chloride mixed crystals (purity 94.5%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 90.8%.

[0056] In this embodiment, the finished red mud powder can be directly used to prepare soil conditioner, and its performance meets relevant industry standards; the comprehensive processing cost is 43 yuan / ton, which is 55% lower than the existing step-by-step process, and the energy consumption is 31 kWh / ton, which is 69% lower than the existing high-temperature process.

[0057] Example 5 A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting includes the following steps: 1. Red mud pretreatment: Bayer process red mud (initial water content 73%, pH 13.0, total alkali content 8.5%, of which bound alkali content 6.3%, SiO2 content 20%, Al2O3 content 15%) was fed into a mixing tank and stirred for 28 min to obtain homogenized red mud slurry.

[0058] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry is fed into an ultrasonic conditioning device, using a dual-frequency combination of 35 kHz (low frequency) and 95 kHz (high frequency), with an ultrasonic power of 450 W, an ultrasonic temperature of 40 ℃, an ultrasonic time of 35 min, and a stirring speed of 90 r / min.

[0059] 3. Low-temperature roasting and co-treatment: The ultrasonically pretreated red mud slurry was fed into a spray dryer and dried at 140 ℃ to a moisture content of 11% to obtain dried red mud particles; the dried red mud particles were then fed into a low-temperature roasting furnace under nitrogen protection (flow rate 0.9 L / min) and roasted in stages: roasted at 210 ℃ for 1.8 h, and then heated to 290 ℃ for 2.8 h; after roasting, deeply treated red mud was obtained with a pH of 6.8, a total dealkali removal rate of 97.1%, a moisture content of 6.5%, an active SiO2 content of 11.5%, and an active Al2O3 content of 8.5%.

[0060] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, and cooled and crystallized to obtain sodium chloride-potassium chloride mixed crystals (purity 95.3%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 91.8%.

[0061] In this embodiment, the finished red mud powder can be directly used to prepare soil conditioner, and its performance meets relevant industry standards; the comprehensive processing cost is 41 yuan / ton, which is 57% lower than the existing step-by-step process, and the energy consumption is 29 kWh / ton, which is 71% lower than the existing high-temperature process.

[0062] Example 6 A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting includes the following steps: 1. Red mud pretreatment: Bayer process red mud (initial water content 72%, pH 12.9, total alkali content 8.2%, of which bound alkali content 6.1%, SiO2 content 21%, Al2O3 content 16%) was fed into a mixing tank and stirred for 30 min to obtain homogenized red mud slurry.

[0063] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry is fed into an ultrasonic conditioning device, using a dual-frequency combination of 30 kHz (low frequency) and 90 kHz (high frequency), with an ultrasonic power of 400 W, an ultrasonic temperature of 35 ℃, an ultrasonic time of 30 min, and a stirring speed of 80 r / min.

[0064] 3. Low-temperature roasting and co-treatment: The ultrasonically pretreated red mud slurry was fed into a spray dryer and dried at 135 ℃ to a moisture content of 12% to obtain dried red mud particles; the dried red mud particles were then fed into a low-temperature roasting furnace under argon protection (flow rate 0.8 L / min) and roasted in stages: roasted at 200 ℃ for 1.5 h, and then heated to 280 ℃ for 2.5 h; after roasting, deeply treated red mud was obtained with a pH of 7.2, a total dealkalization rate of 96.5%, a moisture content of 6.7%, an active SiO2 content of 11.3%, and an active Al2O3 content of 8.4%.

[0065] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 110-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, and cooled and crystallized to obtain sodium chloride-potassium chloride mixed crystals (purity 94.2%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 90.5%.

[0066] In this embodiment, the finished red mud powder can be directly used to prepare soil conditioner, and its performance meets relevant industry standards; the comprehensive processing cost is 44 yuan / ton, which is 54% lower than the existing step-by-step process, and the energy consumption is 32 kWh / ton, which is 68% lower than the existing high-temperature process.

[0067] Comparative Example 1 The existing high-temperature roasting stepwise treatment process (first dehydration, then dealkalization, and finally mineral phase activation) is adopted, and the specific steps are as follows: 1. Red mud pretreatment: Bayer process red mud (initial moisture content 72%, pH 12.9, total alkali content 8.2%, of which bound alkali content 6.1%, SiO2 content 21%, Al2O3 content 16%) was fed into a mixing tank and stirred for 30 min to obtain homogenized red mud slurry. Without ultrasonic conditioning, the homogenized red mud slurry was directly fed into the next drying step.

[0068] 2. High-temperature roasting step-by-step treatment: The homogenized red mud slurry is dried in a 150 ℃ oven until the moisture content is ≤15%, and then pulverized to 100-120 mesh; the dried red mud particles are fed into a high-temperature roasting furnace, protected by nitrogen (flow rate 0.8 L / min), and roasted at 350 ℃ for 2.0 h (to remove free alkali); then the temperature is raised to 600 ℃ and roasted for 3.0 h (to activate the mineral phase); the treated red mud is obtained after roasting.

[0069] 3. Post-processing and resource recycling: The treated red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, cooled and crystallized to obtain mixed crystals (purity 82.5%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 85.3%.

[0070] The final red mud had a moisture content of 12%, a total dealkali rate of 82.3%, and an active SiO2 content of 8.2%. The energy consumption for treating 1 ton of red mud was 95 kWh, and the cost was 88 yuan / ton. The red mud particles were severely agglomerated, and the mineral phase activity was low.

[0071] Comparative Example 2 The existing ultrasonic pretreatment method is used, without the low-temperature calcination step. The specific steps are as follows: 1. Red mud pretreatment: Bayer process red mud (initial water content 72%, pH 12.9, total alkali content 8.2%, of which bound alkali content 6.1%, SiO2 content 21%, Al2O3 content 16%) was fed into a mixing tank and stirred for 30 min to obtain homogenized red mud slurry.

[0072] 2. Ultrasonic conditioning pretreatment: The homogenized red mud slurry is fed into an ultrasonic conditioning device, using a dual-frequency combination of 30 kHz (low frequency) and 90 kHz (high frequency), with an ultrasonic power of 400 W, an ultrasonic temperature of 35 ℃, an ultrasonic time of 30 min, and a stirring speed of 80 r / min.

[0073] 3. Low-temperature roasting and co-processing: No roasting treatment is performed. The ultrasonically pretreated red mud slurry is directly placed in a 120 ℃ oven to dry until the moisture content is ≤ 15%, and then pulverized to 100-120 mesh to obtain the finished red mud powder.

[0074] 4. Post-processing and resource recycling: There is no roasting process and no recovery of alkaline volatiles; the water vapor generated during the drying process is directly emitted. The final red mud has a moisture content of 38%, a total dealkali removal rate of 68.7%, and no mineral phase reconstruction effect. The red mud mineral phase remains inert and cannot meet the resource utilization requirements. The processing cost is 75 yuan / ton.

[0075] Comparative Example 3 The existing single low-temperature calcination (280 ℃) process is used, without ultrasonic conditioning. The specific steps are as follows: 1. Red mud pretreatment: Bayer process red mud (initial water content 72%, pH 12.9, total alkali content 8.2%, of which bound alkali content 6.1%, SiO2 content 21%, Al2O3 content 16%) was fed into a mixing tank and stirred for 30 min to obtain homogenized red mud slurry.

[0076] 2. Ultrasonic conditioning pretreatment: Without ultrasonic conditioning, the homogenized red mud slurry is directly sent to the next drying step.

[0077] 3. Single low-temperature roasting treatment: The homogenized red mud slurry was placed in a 120 ℃ oven and dried until the moisture content was ≤15% to obtain dried red mud particles; the dried red mud particles were sent into a low-temperature roasting furnace, protected by nitrogen (flow rate 0.8 L / min), and roasted at a constant temperature of 280 ℃ for 4.0 h (single-stage roasting); after roasting, the treated red mud was obtained.

[0078] 4. Post-processing and resource recycling: The deeply processed red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles generated during roasting are recovered by condensation, neutralized by adding 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, cooled and crystallized to obtain mixed crystals (purity 89.5%), which are recycled as industrial raw materials; nitrogen is purified by activated carbon adsorption and recycled for the roasting process, with a recycling rate of 89.2%.

[0079] The final red mud had a water content of 10%, a total dealkali rate of 88.5%, and an active SiO2 content of 9.1%. The energy consumption for treating 1 ton of red mud was 65 kWh, and the cost was 70 yuan / ton. The red mud showed severe agglomeration, and the dealkali removal and mineral phase reconstruction effects were lower than those of this invention.

[0080] Comparative Example 4 The existing strong acid neutralization + high-temperature drying process is used, without ultrasonic conditioning and mineral phase reconstruction steps. The specific steps are as follows: 1. Red mud pretreatment: Bayer process red mud (initial water content 72%, pH 12.9, total alkali content 8.2%, of which bound alkali content 6.1%, SiO2 content 21%, Al2O3 content 16%) was fed into a mixing tank and stirred for 30 min to obtain homogenized red mud slurry.

[0081] 2. Ultrasonic conditioning pretreatment: No ultrasonic conditioning is performed. Add 5% dilute hydrochloric acid to the homogenized red mud slurry to adjust the pH to 7.0, stir for 30 min, and obtain the neutralized red mud slurry.

[0082] 3. High-temperature roasting treatment: The neutralized red mud slurry was placed in a 120 ℃ oven and dried until the moisture content was ≤ 15%, and then pulverized to 100-120 mesh; the dried red mud particles were fed into a high-temperature roasting furnace, under nitrogen protection (flow rate 0.8 L / min), and roasted at 350 ℃ in a single stage for 4.0 h; after roasting, the treated red mud was obtained.

[0083] 4. Post-treatment and resource recycling: The treated red mud is cooled to room temperature and pulverized to 100-120 mesh to obtain finished red mud powder; the alkaline volatiles produced by roasting are relatively small, and after condensation and recovery, they are neutralized with 5% dilute hydrochloric acid (40 ℃), evaporated and concentrated, cooled and crystallized to obtain mixed crystals (purity 85.6%); nitrogen is purified by activated carbon adsorption and recycled, with a recycling rate of 88.5%; the acid neutralization step produces 1.2 tons of high-salt wastewater.

[0084] The final red mud had a moisture content of 11% and a total dealkalization rate of 92.6%. The red mud particle structure was destroyed, silicon and aluminum components were lost, and 1.2 tons of high-salt wastewater were generated, with a treatment cost of 92 yuan / ton. The secondary pollution was serious.

[0085] The results of Examples 1-6 and Comparative Examples 1-4 show that, compared with existing processes, the method of the present invention increases the total alkali removal rate by more than 15%, the removal rate of bound alkali by more than 20%, the content of active mineral phase by more than 20%, reduces energy consumption by more than 70%, and reduces processing costs by more than 55%. Moreover, it has no secondary pollution, is simple and efficient, and has strong adaptability, which fully verifies the superiority of the technical solution of the present invention.

[0086] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for synergistic dehydration, dealkalization, and mineral phase reconstruction of red mud through ultrasonic conditioning and low-temperature roasting, characterized in that... Includes the following steps: The red mud was used to obtain a homogenized red mud slurry; The homogenized red mud slurry was ultrasonically treated and dried to obtain dried red mud particles. Dry red mud particles are calcined under an inert atmosphere to obtain deeply treated red mud. The deeply processed red mud is cooled and pulverized to obtain red mud powder; The ultrasonic treatment employs dual-frequency ultrasonic synergy, with ultrasonic frequencies of 20-40 kHz and 80-100 kHz working together. The roasting process employs a two-stage roasting process. The first stage roasting temperature is 180-220 ℃, and the second stage roasting temperature is raised to 250-300 ℃.

2. The method as described in claim 1, characterized in that, The stirring time is 20-60 minutes.

3. The method as described in claim 1, characterized in that, The ultrasonic power is 300-500 W, the ultrasonic time is 20-40 min, the ultrasonic temperature is controlled at 25-45 ℃, and the ultrasonic process is continuously stirred at a speed of 60-100 r / min.

4. The method as described in claim 1, characterized in that, The inert atmosphere is nitrogen or argon.

5. The method as described in claim 1, characterized in that, The drying process involves drying at 120-150 ℃ until the moisture content is ≤ 15%.

6. The method as described in claim 1, characterized in that, The inert atmosphere flow rate was controlled at 0.5-1.0 L / min; the first stage roasting time was 1.0-2.0 h; and the second stage roasting time was 2.0-3.0 h.

7. The method as described in claim 1, characterized in that, The deep-treated red mud has a pH of 6.5-8.0, a total dealkali rate of ≥95%, a moisture content of ≤8%, an active SiO2 content of ≥10%, and an active Al2O3 content of ≥7%.

8. The method as described in claim 1, characterized in that, Deeply processed red mud is cooled to room temperature and then pulverized to a particle size ≤120 mesh.

9. The method as described in claim 1, characterized in that, The alkaline volatiles produced during the roasting process are condensed and recovered, then neutralized with dilute hydrochloric acid to obtain a mixed solution of sodium chloride and potassium chloride. After evaporation, concentration, cooling and crystallization, the solution is recycled as an industrial raw material.

10. The method as described in claim 9, characterized in that, The mixed crystals obtained by neutralizing with dilute hydrochloric acid at a concentration of 5% and a neutralization temperature of 40 °C have a purity of ≥ 94%.