Self-cementing material prepared from secondary aluminum ash as well as preparation method and application of self-cementing material

Through mechanical ball milling and chemical excitation technology, the mixture of aeolian sand and secondary aluminum ash is formed into a high-strength, environmentally friendly self-cementing material, which solves the problems of high cost and low value in the resource utilization of aeolian sand and secondary aluminum ash. The application of green and environmentally friendly building materials has been realized.

CN118754475AActive Publication Date: 2024-10-11WUHAN POLYTECHNIC UNIVERSITY

Patent Information

Application Number
CN202410933821.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

In the existing technology, the resource utilization of aeolian sand and secondary aluminum ash has the problems of high cost, small scale, low value and inability to stimulate chemical activity, which limits its wide application in building materials.

Method used

Using mechanical ball milling and chemical excitation methods, the mixture of aeolian sand and secondary aluminum ash is ball milled, and then molded under high pressure and alkaline conditions to form a green and environmentally friendly self-cementing material, realizing the integration of aeolian sand and secondary aluminum ash. Comprehensive utilization of ash.

Benefits of technology

It reduces the material cost, improves the strength and durability of self-cementing materials, meets the strength requirements of hollow bricks or blocks, and improves the density and stability of the material through the chemical excitation process, meeting environmental standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754475A_ABST
    Figure CN118754475A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a self-cementing material by using secondary aluminum ash. The method comprises the following steps: drying and ball-milling aeolian sand, the secondary aluminum ash and an alkali activator, adding water, stirring, collecting ammonia gas, and carrying out pressure forming. The invention also discloses the self-cementing material prepared by the method and application of the self-cementing material as a hollow brick or a building block. The secondary aluminum ash cooperates with the aeolian sand and is subjected to mechanical blending and ball milling with the alkali activator, physical activation and chemical modification are carried out in the ball milling process, the compactness of the material is improved, the internal mineral crystal structure of the material is changed, active silicon and aluminum monomers are formed, the active silicon and aluminum monomers are stirred and mixed with water, secondary chemical excitation is carried out in the high-pressure state, and the high-strength silicon-aluminum composite material is obtained. The high-strength self-cementing material is obtained. The limitation of a traditional aeolian sand-based material is overcome, the strength and durability are improved, and secondary utilization of waste is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste resource utilization, and specifically relates to a self-cementing material prepared by utilizing secondary aluminum ash, and a preparation method and application thereof. Background Art

[0002] Deserts are widely distributed around the world, and nearly 41% of the land on Earth is degrading, affecting about 38% of the world's population. Natural aeolian sand (eolian sand) is a sandy granular material formed by long-term soil drying and wind action, characterized by loose structure, poor self-stability, uneven particle size and no edges. SiO2 accounts for more than 75% of its composition, and Al2O3 accounts for 5% to 10%. Sand is one of the indispensable raw materials for the construction industry. It is estimated that 15 billion tons of sand are used for construction every year worldwide, most of which are machine-made sand and river sand because of their good uniformity and stability. If aeolian sand can be used in construction, it can reduce the cost of building materials, improve the ecological environment, and meet the development trend of the construction industry from ultra-low energy consumption to near-zero energy consumption. Aeolian sand is difficult to be used directly in construction projects due to severe weathering. Therefore, the application of aeolian sand in social and industrial production is relatively limited, and it must be activated before it can be used as a building material.

[0003] At present, the main method of utilizing aeolian sand involves solidification, where cement additives are usually used to improve strength and solve the problems of brittleness and low flexural strength. In concrete synthesis, 20%-30% of aeolian sand is added to replace natural river sand as fine aggregate. The workability and strength of concrete can be improved by adjusting the ratio of aeolian sand to cement. In addition, the addition of bentonite, polymer emulsions, polypropylene fibers and other additives improve the properties of building materials. Aeolian sand can also be chemically activated using microorganisms. Low doses of vinyl acrylic acid significantly improve the compaction and BCR of aeolian sand, while the addition of sodium thiosulfate improves the unconfined compressive strength and flexural strength. The combination of enzyme-induced carbonate precipitation and polyvinyl alcohol solidification of aeolian sand improves the unconfined compressive strength, wind erosion resistance, water erosion resistance and surface strength. Despite these advantages, disadvantages such as high cost, limited availability in certain areas and lack of environmental friendliness still limit the widespread use of aeolian sand in engineering.

[0004] Primary aluminum ash is the scum that is insoluble in aluminum liquid during the electrolytic aluminum oxide process in the production of primary aluminum. Secondary aluminum ash is the aluminum-containing waste slag produced during the re-refining process of primary aluminum ash. It is the waste after the extraction of metallic aluminum from primary aluminum ash. More than 5 million tons of secondary aluminum ash are produced worldwide each year, of which about 95% are discarded in industrial solid waste dumps. The electrolytic aluminum process in various countries in the world is mature, and the chemical composition of secondary aluminum ash in different regions is similar. AlN is the main component of secondary aluminum ash, accounting for 10%-30%, and it also contains Al, Al2O3, Al4C3, MgO and other forms, of which the content of elemental aluminum and its compounds is more than 70%. Generally, secondary aluminum ash is used in zeolite, ion exchanger, refractory material, composite material, cement and concrete products. The current utilization methods mainly include pyrolysis and wet process. In the wet process, AlN is hydrolyzed and the salt is dissolved in water to produce high crystalline active alumina powder, high purity nanostructured alumina powder and layered double hydroxide. The pyrometallurgical method involves roasting secondary aluminum ash with CaO to increase its activity and reduce heavy metals to produce glass-ceramics. In addition, the recovery of Al2O3 and other value-added products can be achieved by combining acid leaching and calcination. However, the current methods for recycling and reusing secondary aluminum ash have disadvantages such as high cost, small scale, low value, and inability to stimulate chemical activity. Since 2021, China has listed secondary aluminum ash as hazardous waste and prohibited direct landfill, making the resource utilization of secondary aluminum ash even more important. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a self-cementing material using secondary aluminum ash. The method uses secondary aluminum ash and aeolian sand as main raw materials, utilizes mechanical ball milling and chemical excitation to enhance the potential activity of the mixture of aeolian sand and secondary aluminum ash, and finally synthesizes a green and environmentally friendly self-cementing material under room temperature and high pressure conditions, realizes the comprehensive utilization of solid waste, and provides a new solution for the disposal and resource utilization of aeolian sand and secondary aluminum ash.

[0006] In order to solve the above technical problems, the method for preparing a self-cementing material using secondary aluminum ash provided by the present invention comprises the following steps:

[0007] (1) Aeolian sand, secondary aluminum ash and alkali activator are dried to constant weight respectively, wherein the alkali activator passes through a 200-mesh standard sieve.

[0008] (2) Adding secondary aluminum ash, aeolian sand and an externally mixed alkali activator into a ball mill jar of a planetary ball mill in sequence; the total mass of the secondary aluminum ash and aeolian sand is 100 parts by mass, of which the mass of the secondary aluminum ash is 45 to 55 parts by mass, and the mass of the alkali activator is 3 to 6 parts by mass.

[0009] (3) Set the rotation speed and time of the planetary ball mill to 500-650 rpm and 20-30 min, respectively, and perform ball milling under this condition.

[0010] (4) The mixed powder after ball milling is passed through a 2 mm sieve to obtain a self-binding material precursor.

[0011] (5) Add the self-binder material precursor to a planetary cement mortar mixer, and slowly add water while the planetary cement mortar mixer is stirring at a low speed. The water adding time is not less than 20 seconds and not longer than 1 minute. Stop adding water after the moisture content of the mixture increases to 9-12%. Collect the generated ammonia gas during the water adding process. After the water adding is completed, adjust the planetary cement mortar mixer to a high speed and stir for 2-3 minutes.

[0012] (6) The uniformly mixed mixture is pressurized at a loading rate of 5 to 7 kN / min, and the pressurization is stopped when the pressure reaches 40 to 60 kN. The constant pressure is maintained for 2 to 3 minutes, and then the pressure is released to obtain a self-bonding material.

[0013] (7) The high-pressure formed self-binder solidified block is cured at a temperature of 20±1°C and a humidity of 98±1% for not less than 14 days.

[0014] Preferably, the alkaline activator is at least one of CaO, quicklime, NaOH and KOH.

[0015] Preferably, the mass of the base activator is 4 to 5 parts by mass.

[0016] Preferably, the mass of the secondary aluminum ash is 47 to 50 parts by mass.

[0017] Preferably, the ball milling speed is 500-550 rpm.

[0018] Preferably, the generated ammonia gas is collected and introduced into concentrated sulfuric acid to form ammonium sulfate.

[0019] Preferably, the concentrated sulfuric acid is sulfuric acid with a concentration of 80% or more.

[0020] The present invention also provides a self-adhesive material prepared by the method and application of the self-adhesive material as a hollow brick or a building block to improve its strength.

[0021] Compared with traditional self-cementing materials, the self-cementing material prepared by the secondary aluminum ash-aeolian sand synergistic method of the present invention has the following significant beneficial effects:

[0022] 1. The present invention uses secondary aluminum ash which is difficult to consume in industry and natural low-cost aeolian sand as raw materials, which is green and environmentally friendly. The cost of synthetic self-cementing materials is properly controlled, the cost of raw materials is only 22.5 yuan / ton, the bonding effect is good, and the strength requirements of hollow bricks or blocks are met.

[0023] 2. Compared with traditional self-cementing materials, the preparation process of the present invention does not require calcination, and the molding process is quick and simple, which greatly reduces the use of energy and natural resources. The molding process can be carried out in the factory, and the waste gas generated is collected and then introduced into concentrated sulfuric acid to form ammonium sulfate, which is a valuable chemical product and can be used as a raw material for chemical fertilizers to generate secondary economic value.

[0024] 3. The present invention utilizes secondary aluminum ash in coordination with aeolian sand, and is mechanically blended and ball-milled with an alkaline activator. Physical activation and chemical modification occur during the ball-milling process to achieve the first chemical excitation process. The physical activation changes the particle morphology and fineness of the material, making the particle components more uniform, facilitating the filling of the pore structure during the synthesis of the self-cementing material, and further improving the density of the material. SiO2 accounts for more than 75% of the aeolian sand, and elemental aluminum and its oxidized form account for more than 70% of the aluminum ash, accompanied by MgO. The chemical modification process changes the internal mineral crystal structure of the material under alkaline conditions, achieving the breaking of the stable Si-O bonds, Al-O bonds, and Mg-O in the raw materials under high-energy mechanical forces and high-temperature conditions generated by the mechanical forces, forming active silicon and aluminum monomers, promoting the bonding of some Si-O-Al bonds, and forming active precursors under blending conditions, providing a basis for subsequent further chemical excitation processes.

[0025] 4. The self-cementing material in the present invention is an active precursor that has been chemically activated for the first time. When mixed with water and under high pressure, it achieves the purpose of secondary chemical activation. Under alkaline conditions, the original mineral structure is destroyed and reorganized, forming free ions in the system, such as AlO2 - and SiO3 2- , further promoting the formation of Si-O-Al structure and continuously providing OH - , which promotes the further progress of the chemical reaction. When all the free ions form a stable compound network structure (the molar ratio of active Si to active Al = 3:1~1:1), the skeleton structure of the material is formed, and a high-strength self-bonding material can be obtained.

[0026] 5. The present invention creatively uses secondary aluminum ash and aeolian sand as raw materials, reveals the intrinsic connection between "secondary activation-chemical excitation-structural reorganization", establishes a directional control method for the strength of self-cementing materials, allows the chemical components in the raw materials to participate in the chemical reaction, achieves the purpose of chemical excitation consolidation, and forms a more stable consolidation body with stronger stability. This is significantly different from the traditional self-cementing material method of using physical packaging to achieve stable strength.

[0027] 6. Desert areas usually experience extreme weathering environments, which places higher requirements on the stability of materials. The self-bonding material prepared with secondary aluminum ash and aeolian sand as the main raw materials of the present invention meets this characteristic. The self-bonding material complies with the Chinese national standard "Sintered Hollow Bricks and Blocks" (GB13545-2014). This method overcomes the limitations of traditional aeolian sand-based materials and improves strength and durability.

[0028] 7. The present invention uses machine-made sand and secondary aluminum ash to synthesize self-cementing materials for comparison. However, since the machine-made sand particles are evenly distributed, many irregular pores are generated during the formation of the self-cementing material, which cannot be filled. As a result, the compressive strength is more than 30% lower than that of the self-cementing material synthesized by aeolian sand and secondary aluminum ash. The self-cementing material synthesized by aeolian sand and secondary aluminum ash has obvious strength advantages.

[0029] 8. The self-bonding material of the present invention has been applied in a small range. During the 360-day test, the compressive strength continued to rise to 8.57 MPa, with good long-term stability and durability. The heavy metal leaching concentration complies with the Chinese standard "Surface Water Environmental Quality Standard" (GB 3838-2002), meeting environmental requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a process flow chart for preparing the self-bonding material of the present invention.

[0031] Figure 2 This is a graph showing the effect of different ball milling speeds on particle size distribution during the ball milling process of the raw materials of the present invention.

[0032] Figure 3 This is the compressive strength diagram of self-cementing materials at different ages under different ball milling speed conditions.

[0033] Figure 4 This is a graph showing the functional relationship between the compressive strength of self-cementing materials and the ball milling speed.

[0034] Figure 5 The grinding kinetics fitting diagram of the precursor RRB model and Swrebec model under different ball milling speed conditions.

[0035] Figure 6 This is the XRD mineral composition diagram of the self-cementing material.

[0036] Figure 7 This is the SEM-EDS (scanning electron microscope-energy dispersive spectroscopy) spectrum of the self-cementing material.

[0037] Figure 8 This is the XPS photoelectron spectrum of the self-bonding material.

[0038] Fig. 9Diagram of the mechanism of chemical excitation process of self-cementing materials.

[0039] Fig.10 This is the infrared spectrum of the self-cementing material.

[0040] Fig.11 This is a graph showing the compressive strength of self-cementing materials in field tests and the relationship between the ammonia nitrogen leaching concentration.

[0041] Fig.12 This is a comparison chart of the performance of aeolian sand / mechanical sand self-cementing materials. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0043] Example 1

[0044] Figure 1 The process flow chart of the preparation of the self-cementing material of the present invention, wherein the alkaline activator is illustrated in the figure as calcium oxide. The chemical composition of aeolian sand and secondary aluminum ash in this embodiment is shown in Table 1. In the secondary aluminum ash and aeolian sand raw materials added in this embodiment, the mass proportion of aeolian sand is 50%, the external amount of the alkaline activator CaO is 5% (that is, 5% of the total mass of secondary aluminum ash and aeolian sand), and the ball milling time is set to 25min. The precursor is obtained after ball milling at 450 / 500 / 550 / 600 / 650rpm. The particle size distribution is measured by a laser particle size analyzer (Dandong Better Instrument Co., Ltd., 9300ST, China) and the experimental factors are as shown in Table 2. Figure 2 As shown. As the ball milling speed increased from 450rpm to 500rpm, the median particle size (D50) of the material showed a slight increase of 12.84%. At a ball milling speed of 550rpm, the D50 value of the precursor remained relatively stable. However, with the further increase in the ball milling speed, especially at 650rpm, the D50 of the precursor increased significantly to 34.33μm. The change pattern of the mean particle size (MGD) was similar to that of D50. Affected by particle hardness, material composition and other factors, the rapid ball milling speed increased the collision frequency of aeolian sand and secondary aluminum ash with the steel balls in the ball mill, resulting in particle agglomeration and increased D50 and MGD.

[0045] Table 1 Chemical composition of aeolian sand and secondary aluminum ash measured by X-ray fluorescence spectrometer (%)

[0046]

[0047] Note: NAS refers to aeolian sand and SAD refers to secondary aluminum ash.

[0048] Table 2 Test conditions

[0049]

[0050] After ball milling, use a planetary cement mortar mixer at a low speed (rotation 140±2rpm, revolution 62±2rpm) to slowly add water to adjust the moisture content of the mixture to 11% (water addition time is 40±10 seconds), adjust the planetary cement mortar mixer to a high speed (rotation 285±3rpm, revolution 125±3rpm) and stir quickly for 2 minutes. The ammonia released by the material when it encounters water is collected by an aspirator and passed into sulfuric acid to generate ammonium sulfate for fixation. Weigh 200g of the mixture and place it in The mold was placed in a cylindrical stainless steel mold and pressed for 15 seconds under an external pressure of 40 kN. After demoulding, the self-bonding material was obtained. The mold was cured under standard conditions (temperature: 20 ± 1 ° C, humidity: 98 ± 1%) for 3 to 14 days.

[0051] like Figure 3 As shown in Figure 2, after 14 days of curing, the compressive strength of R1 is 3.19 MPa. With the increase of ball milling speed, the compressive strength shows a significant improvement.

[0052] like Figure 4 As shown in the figure, the R of the self-cementing material after curing for 14 days was obtained by fitting the compressive strength and ball milling speed with a quadratic polynomial. 2 The compressive strength of the ball mill was 0.97. When the ball milling speed reached 550-650rpm, the compressive strength remained stable between 6.19 and 6.90MPa. Although the compressive strength reached the highest value at 600rpm, the higher speed increased the activation cost. Considering the economy and experimental effect, 550rpm was determined to be the most suitable choice for mechanical activation.

[0053] Figure 5 The figure is the grinding kinetics fitting diagram of the precursor RRB model and Swrebec model under different ball milling speed conditions. The particle size distribution characteristics of the material play an important role in chemical excitation and compressive strength. By exploring the particle size distribution characteristics of the material under different ball milling speeds, the relationship between particle size distribution and compressive strength is further analyzed.

[0054] The RRB model correctly predicts the particle distribution of the precursor, R 2 The value is greater than 0.99. The fitting value of the precursor particle size distribution calculated using the RRB model is closely consistent with the measured value, confirming the applicability of the RRB model to the particle size distribution of the precursor. In addition, with the increase in grinding speed, the characteristic particle size (d*) increases from 41.35μm to 57.43μm. With the increase in grinding speed, larger particles are decomposed into smaller particles, resulting in particle agglomeration and the formation of "secondary particles", showing loose aggregates. These "secondary particles" show good gradation distribution in chemical excitation, promote hydration reaction, and help improve compressive strength.

[0055] R obtained by fitting the Swrebec model 2 The value is between 0.984 and 0.988, which is slightly lower than that of the RRB model. Although the D50 predicted by the Swrebec model is consistent with the measured value, the predicted maximum particle size fluctuates greatly and deviates from the measured value. In addition, the b value first increases and then decreases, indicating that the particle size distribution curve fluctuates greatly. Therefore, the Swrebec function further shows that the ball milling speed can affect the chemical activity of the material and the rationalization of the material particle size distribution.

[0056] The self-cementing materials were characterized by XRD mineral composition analysis, such as Figure 6 As shown. In the secondary aluminum ash, the main crystal phases are Al and AlN, and there are also diffraction peaks of Fe and spinel. In the aeolian sand, the diffraction peak of quartz is accompanied by the presence of albite and apatite. In the self-cementing material, the diffraction peaks of quartz and albite are weakened, and no new crystal structure is produced. This phenomenon can be attributed to the large amount of relatively stable crystalline substances in the aeolian sand. Under the synergistic effect of mechanical collision and high temperature during ball milling, the mineral lattice of the secondary aluminum ash produces more defects and damage than the aeolian sand. The addition of CaO and water produces an alkaline environment, which promotes the excitation and recombination of chemical bonds and produces amorphous substances. In addition, broad peaks between 18 and 25 degrees and weakened diffraction peaks of the mineral phase are observed in the self-cementing material, indicating the presence of amorphous substances, which is also the reason why the self-cementing material has a certain strength.

[0057] Scanning electron microscopy tests were performed on secondary aluminum ash, aeolian sand and self-cementing materials, such as Figure 7 As shown. Secondary aluminum ash ( Figure 7 a and partial enlargement Figure 7 The surface of b) shows a relative roughness characterized by rod-like and flake-like fragments with loose fillings and a large number of pores between them. The surface element distribution shows the presence of a large amount of aluminum ( Figure 7 i). The results explain why secondary aluminum ash can be easily broken into smaller particles by mechanical force and its excellent cementitious properties. Figure 7 c and local enlargement Figure 7 d) It is mainly composed of large particles with irregular shapes, and its microscopic morphology is highly dense. Figure 6 ) determined by analysis Figure 7 The clusters observed in d are mainly quartz (silicon dioxide), a mineral with high hardness and mechanical strength. However, these clusters can provide Si ( Figure 7 j), which has great potential for the preparation of self-cementing materials.

[0058] Self-bonding materials ( Figure 7The microscopic morphology of (e, 7g) shows tightly packed particles with unreacted debris adhering to the surface. Figure 7 f, 7h), the surface shows a disordered amorphous structure, representing the gel-like microstructure of the hydration product, which contributes to the high compressive strength of the self-cementing material. The EDS spectrum analysis further confirms the presence of a large amount of silicon, aluminum and oxygen elements ( Figure 7 k). In addition, the surface of the fragments showed a dense flaky structure ( Figure 7 f), with a metallic luster in morphology. This appearance is significantly different from the morphology of secondary aluminum ash and aeolian sand at the same magnification, confirming that mechanochemical activation has led to fundamental changes in the mineral structure.

[0059] XPS photoelectron spectroscopy analysis was performed on aeolian sand, secondary aluminum ash and self-cementing materials ( Figure 8 In the XPS photoelectron spectra of silicon and aluminum, we found that the silicon in the aeolian sand exists in the form of silicon dioxide (102.80 eV) ( Figure 8 a). Aluminum in secondary aluminum ash exists in the form of Al2O3 / Al (74.80eV) and AlN (73.50eV) ( Figure 8 b), which is consistent with the XRD mineral composition analysis results. In the self-cementing material, no characteristic absorption peaks of SiO2 and AlN were detected, and Al2SiO5 (102.70 eV), SiO2 (Al2O3) 0.55 (102.20eV), Al2O3(73.24eV) and SiO2(Al2O3) 0.22 The new characteristic absorption peak (74.30 eV) Figure 8 c and 8d). This finding suggests that most Si-O chemical bonds and Al-N bonds were destroyed by alkali attack, forming active silicon and aluminum monomers, and finally forming a more stable structure (Si-O-Al).

[0060] The alkaline activator promotes chemical activation. The original secondary aluminum ash and aeolian sand have low content, low calcium content, and the characteristic absorption peak is not obvious. In the self-cementing material prepared by using calcium oxide as the alkaline activator in this embodiment, Ca 2p 3 / 2 is composed of Ca-SiO3 (347.04 eV) and Ca2[Mg5][Si8O 22 ]OH2(347.70eV) Figure 8 e).

[0061] The Ca-O bond in calcium oxide breaks under the action of mechanochemistry. In an alkaline solution environment, the Si-O bond in the aeolian sand and the Al-N bond in the secondary aluminum ash are hydrolyzed and broken to form SiO3 2- 、AlO3 3-, as well as free substances such as Si and Al active monomers, and Ca4 2- The coordination recombination reaction occurs together to form stable compound structures such as Al2SiO5 and CaSiO3. The hydration reaction of CaO also provides an alkaline environment for the system and promotes chemical excitation. Fig. 9 )

[0062] The Al2O3 binding energy of the self-cementing material is 73.24 eV, which is lower than that of the secondary aluminum ash, indicating that the aluminum-containing material is also transforming and some Al-O bonds are involved in the chemical reaction. This conclusion was verified by infrared spectroscopy ( Fig.10 ). In aeolian sand, 879cm -1 The absorption wavelength is the vibration peak of the silicon-oxygen bond of SiO2 (δSi-O-Si / νSi-O). However, in self-cementing materials, this characteristic absorption peak moves to 779cm -1 , indicating that the silicon-oxygen bond has changed, which, combined with the mineral composition analysis, confirms that it is the result of a hydration reaction. In addition, the self-cementing material has a -1 A new absorption peak (Si-O-Al) appears at the absorption wavelength of . Given the abundance of Al and AlN atoms in secondary aluminum ash, Al participates in the chemical reaction and combines with Si and O to form a stable chemical bond. Since the chemical reaction is a hydration process under alkaline conditions, the absorption wavelength of the hydroxyl peak of water decreases (1631cm -1 ), the absorption wavelength of the hydroxyl peak of the hydration product combined with water increases (3452cm -1 ), indicating that alkali excitation promotes hydroxylation. Therefore, in the process of using these materials to prepare environmentally friendly self-cementing materials, chemical cementation reactions will occur in the internal mineral structure during the ball milling and maintenance stages.

[0063] Example 2

[0064] This example conducted a field test in a desert area. The self-cementing material synthesized indoors (prepared in Example 1, where the ball milling speed was 550 rpm and the curing time was 14 days) was placed in the desert area as a desert road shoulder material, and good results were achieved ( Fig.11 a), during the 360-day test, the compressive strength increased to 8.57MPa. The leaching of ammonia nitrogen from the self-cementing material showed a significant downward trend ( Fig.11 b).

[0065] Embodiments 3 to 9

[0066] The only difference between Examples 3, 4 and 5 and Example 1 is that the content of aeolian sand is changed to 40%, 45% and 55% by mass respectively, the ball milling speed is 550 rpm, and other conditions are the same as Example 1.

[0067] The only difference between Examples 6 and 7 and Example 1 is that the alkaline activator is changed to solid NaOH and KOH respectively, the ball milling speed is 550 rpm, and the other conditions are the same as Example 1.

[0068] The only difference between Examples 8 and 9 and Example 1 is that water is added to the planetary cement mortar mixer to adjust the moisture content to 9 and 12 respectively, and the ball mill speed is 550 rpm. Other conditions are the same as in Example 1.

[0069] After 14 days of curing, the compressive strengths of the self-adhesive materials prepared in Examples 3 to 9 were 4.23 MPa, 5.10 MPa, 6.11 MPa, 5.46 MPa, 5.60 MPa, 5.04 MPa, and 5.82 MPa, respectively.

[0070] Comparative Example 1

[0071] The difference between this comparative example and Example 1 is that machine-made sand is used instead of aeolian sand to prepare the self-cementing material. The mass proportions of secondary aluminum ash and machine-made sand in the self-cementing material of this comparative example are 50% and 50% respectively, and CaO accounting for 5% of the total mass ratio is added; the other process steps are the same as those in Example 1.

[0072] The compressive strength of aeolian sand-secondary aluminum ash and machine-made sand-secondary aluminum ash self-cementing materials are as follows: Fig.12 a. Fig.12 As shown in b. The compressive strength of the self-bonding material is significantly higher than that of the machine-made sand-secondary aluminum ash self-bonding material (under the same ratio of secondary aluminum ash). After 14 days of curing, the compressive strength of the machine-made sand-secondary aluminum ash self-bonding material is 5.13MPa. This comparative example also gives the strength changes of the self-bonding materials prepared under different ratios of aeolian sand and secondary aluminum ash. Among them, when the mass ratio of aeolian sand and secondary aluminum ash is 1:1, the strength of the prepared self-bonding material is the highest. However, the strength development of the self-bonding materials prepared under various ratios mainly occurs within 0-3 days ( Fig.12 a), while the strength growth of the machine-made sand-secondary aluminum ash self-cementing material mainly occurs within 7-14 days ( Fig.12 b). The compressive strength after 14 days of curing is 3.1 times higher than that after 3 days of curing.

[0073] SEM images of aeolian sand-secondary aluminum ash and machine-made sand-secondary aluminum ash self-cementing materials ( Fig.12 c and Fig.12d). The surface of the self-bonding material is highly dense, while the surface of the machine-made sand-secondary aluminum ash self-bonding material is composed of an amorphous gel-like material with uneven particle distribution. The particles are connected by an irregular fiber gel structure with dense pores and obvious cavities. Due to the artificial mechanical synthesis of machine-made sand, the macroscopic structural differences between the particles are small and the particle size distribution is relatively uniform. Therefore, the irregular gaps in the machine-made sand-secondary aluminum ash self-bonding material cannot be effectively filled. Under the action of external force, the structure is easily broken and deformed, which is one of the reasons for the low strength of the machine-made sand-secondary aluminum ash self-bonding material.

[0074] Comparative Example 2

[0075] The difference between this comparative example and Example 1 is that the water adding time is shortened to 2s and 2min, and the ball milling speed is 550rpm; the other process steps are the same as Example 1. After 14 days of curing, the compressive strength of the aeolian sand-secondary aluminum ash self-cementing material is tested to be 4.31MPa and 4.80MPa respectively.

[0076] From the forming process of self-cementing materials, it can be seen that when the water addition time is shortened to 2s, heat is released rapidly during the stirring process, and the surface temperature of the stirring pot rises significantly to above 50°C. Affected by the temperature rise, part of the water body vaporizes and escapes as water vapor, so the actual water content participating in the reaction is lower than the design value, resulting in low compressive strength. When the water addition time is extended to 2min, the stirred materials gradually agglomerate into small particles with a diameter of 0.5 to 1.5cm, with a relatively loose structure and incomplete chemical reaction, resulting in low compressive strength.

Claims

1. A method for preparing a self-cementing material using secondary aluminum ash, characterized in that: The method comprises the following steps: 1) Drying the aeolian sand, secondary aluminum ash and alkali activator to constant weight respectively, wherein the alkali activator passes through a 200-mesh standard sieve; 2) adding secondary aluminum ash, aeolian sand and an externally mixed alkali activator to the ball mill of a planetary ball mill in sequence; the total mass of the secondary aluminum ash and aeolian sand is 100 parts by mass, of which the mass of the secondary aluminum ash is 45-55 parts by mass, and the mass of the alkali activator is 3-6 parts by mass; 3) Set the speed and time of the planetary ball mill to 500-650 rpm and 20-30 min respectively, and perform ball milling under this condition; 4) The mixed powder after ball milling is passed through a 2 mm sieve to obtain a self-cementing material precursor; 5) adding the self-cementing material precursor into a planetary cement mortar mixer, slowly adding water while stirring at a low speed in the planetary cement mortar mixer, the water adding time is not less than 20 seconds and not longer than 1 minute, and the water addition is stopped after the moisture content of the mixture increases to 9-12%, and the generated ammonia gas is collected during the water addition process. After the water addition is completed, the planetary cement mortar mixer is adjusted to a high speed and stirred for 2-3 minutes; 6) The uniformly mixed mixture is pressurized at a loading rate of 5 to 7 kN / min, and the pressurization is stopped when the pressure reaches 40 to 60 kN, and the constant pressure is maintained for 2 to 3 minutes, and then the pressure is released to obtain a self-binding material.

2. The method for preparing a self-cementing material using secondary aluminum ash according to claim 1, characterized in that: The alkaline activator is at least one of CaO, quicklime, NaOH and KOH.

3. The method for preparing self-cementing material using secondary aluminum ash according to claim 1 or 2, characterized in that: The mass of the base activator is 4 to 5 parts by mass.

4. The method for preparing self-cementing material using secondary aluminum ash according to claim 1 or 2, characterized in that: The mass of the secondary aluminum ash is 47 to 50 parts by mass.

5. The method for preparing self-cementing material using secondary aluminum ash according to claim 1 or 2, characterized in that: The ball milling speed is 500-550 rpm.

6. The method for preparing self-cementing material using secondary aluminum ash according to claim 1 or 2, characterized in that: The generated ammonia gas is collected and passed into concentrated sulfuric acid to form ammonium sulfate.

7. The method for preparing a self-cementing material using secondary aluminum ash according to claim 6, characterized in that: The concentrated sulfuric acid is sulfuric acid with a concentration of 80% or more.

8. A self-binding material prepared by the method according to any one of claims 1 to 7.

9. Use of the self-bonding material according to claim 8 as a hollow brick or a building block to increase its strength.

10. The use according to claim 9, characterized in that: Self-adhesive materials need to be cured before use. The curing temperature is 20±1℃, the humidity is 98±1%, and the time is not less than 14 days.

Citation Information

Patent Citations

  • Geopolymer cementitious material based on secondary aluminum ash and preparation method of geopolymer cementitious material

    CN113998911A

  • Process for preparing baking-free brick by taking secondary aluminum ash as raw material under high pressure

    CN114409364A

  • Secondary aluminum ash for concrete and treatment method thereof

    CN115180857A

  • Refractory concrete and preparation method thereof

    CN115215592A

  • Method for co-producing sulphoaluminate cement and sulfur by using desulfurized gypsum and aluminum ash

    WO2018166220A1

Cited By

  • Method for improving gelation activity of waste glass powder through physical and chemical synergistic activation

    CN119461902A