Porous material shaped composite phase change particle, preparation method, application and preparation system thereof, phase change gypsum board and preparation method thereof
By filling the pores and surface lamellae in porous materials, combined with high thermal conductivity fillers and powder-coated layers, the problems of leakage and performance attenuation of composite phase change materials in construction applications are solved, the density and thermal conductivity of the materials are improved, and the Reduce costs and loss rates, and enhance the energy efficiency and environmental adaptability of building materials.
Patent Information
- Application Number
- CN202410737620.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Existing composite phase change materials are prone to leakage and performance degradation in construction applications, leading to reduced energy consumption and environmental pollution, and the preparation method has problems such as high cost and complex operation.
Porous materials are used to shape composite phase change particles, and the density and mechanical properties are improved by filling the pores and surface lamellae of the porous materials. High thermal conductivity filler layers and powder coating layers are used to improve thermal conductivity and surface smoothness, and reduce polymer film-forming agents. Use enough to avoid phase change material loss and adhesion.
The density and thermal conductivity of composite phase change particles are improved, the cost and loss rate are reduced, the service life of phase change materials is extended, and the energy efficiency and environmental adaptability of building materials are enhanced.
Smart Images

Figure CN118754493A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of composite phase-change energy storage materials and building materials, and in particular to porous material shaped composite phase-change particles, their preparation method, use and preparation system, phase-change gypsum board and their preparation method. Background Art
[0002] With the development of social economy, the contradiction of energy supply is becoming increasingly prominent. Studies have shown that building energy consumption accounts for 20%-40% of primary energy consumption. Developing green energy storage building materials and reducing building energy consumption are effective ways to solve the contradiction of global energy supply in the future. Phase change energy storage materials are a kind of efficient energy storage material, which can not only improve the function of building materials, reduce building energy consumption and adjust the comfort of indoor environment of buildings, but also store available thermal energy in the form of phase change latent heat, thereby realizing the storage and conversion of available energy. Therefore, they have good development prospects in building energy conservation.
[0003] Phase change materials currently used in the construction field generally undergo a phase change cycle of heating up solid to liquid, and cooling down liquid to solid. Phase change materials rely on their own material properties to perform energy storage functions. Once a phase change material leaks during application, the performance of the phase change material will decay, and at the same time pollute the surrounding application environment and affect the living environment. In order to ensure that the performance of the phase change material is fully utilized and prevent leakage during application, phase change materials are usually used in building materials. They need to be combined with a carrier to form phase change energy storage particles and then incorporated into building materials to form phase change energy storage building materials products.
[0004] At present, the preparation methods of composite phase change material particles on the market mainly include: microcapsule shaping method, porous material adsorption method, etc. Microcapsule shaping method includes in-situ polymerization method, complex coacervation method, interfacial polymerization method, etc. This method uses phase change material as core material and organic polymer or inorganic material as shell layer to form capsule structure material. The production cost is high and the process is complicated. In addition, the outer wall of the capsule is mostly organic material, and the surface is hydrophobic and not easy to combine with inorganic building materials, resulting in production difficulties. Mixing is difficult and the product strength is low. The porous material adsorption method mainly uses the rich pore structure of the porous material itself as a phase change material carrier, composites the porous material with the solid-liquid phase change material, and shapes the phase change material in the pores. This method is simple to operate and low in cost, but during preparation, the phase change material remains on the mineral surface, which easily causes the mineral particles to stick to each other and form a mass. At the same time, when the phase change material is used, it is easy to leak from the pores when it is heated to liquid, which leads to the problem of declining thermal storage performance of phase change particles and polluting the living environment.
[0005] Patent CN103666380 A discloses a method for preparing composite phase change energy storage particles of porous materials, which uses porous mineral media as carriers to mix and adsorb liquid phase change materials, and then pours them into a fluidized bed, uses cold air with a certain flow rate in the fluidized bed to force convection cooling of uncooled phase change particles, and uses the impact between airflow and materials to disperse the particles. The particles prepared by this method are not easy to agglomerate, but the only obstacle to the phase change material in the porous material is the intermolecular force. Whether it is principle analysis or actual verification, the composite phase change particle energy storage particles prepared will leak from the porous material in the application because the phase change material changes from solid to liquid, which not only has a negative impact on the application environment, but also its own phase change performance is constantly attenuated, and the application value is limited. Summary of the invention
[0006] In response to the above problems, the present application provides porous material shaped composite phase change particles, their preparation method, use and preparation system, phase change gypsum board and preparation method thereof. The composite phase change particles of the present application improve the density and mechanical properties of the composite phase change particles by filling the pores and surface layers of the porous material. At the same time, it also prevents the phase change material in the composite phase change particles from absorbing heat and converting from solid to liquid, and flowing freely in the porous system, thereby causing the loss of phase change materials and the emptiness of the porous particle pores. The filler layer will not only improve the surface flatness of the composite phase change particles, but also reduce the probability of porous particles colliding with each other during the coating process, causing damage to the pores and particle adhesion, which is beneficial to protecting the porous particle pore structure and performing subsequent surface coating steps; and compared with the composite phase change particles without a filler layer, due to the improvement of the surface flatness of the composite phase change particles, the surface area of a single particle is reduced, so that the amount of polymer film-forming agent used in the surface coating step is greatly reduced, which can reduce costs. When the filler layer of the composite phase change particles of the present application includes a high thermal conductivity filler, the thermal conductivity of the phase change particles can be increased, so that the reaction rate of the phase change material to the ambient temperature is improved. At the same time, the composite phase change particle carrier is adjusted by adjusting the mixing ratio of expanded vermiculite or expanded perlite or activated carbon and expanded graphite to adjust the comprehensive thermal conductivity of the composite phase change particle carrier.
[0007] In one aspect, the present application provides a porous material shaped composite phase change particle, comprising:
[0008] Composite phase change particles, the composite phase change particles comprising a porous material and an organic phase change material adsorbed in the pores of the porous material, the porous material being selected from one or more of expanded vermiculite, expanded perlite, expanded graphite or activated carbon, and having a particle size of 0.1 mm to 5 mm;
[0009] A filler layer, wherein the filler layer is a powder filler, and the powder filler is optionally one or both of a high thermal conductivity material and an adsorption filler, and the filler layer is fully filled into the pores on the surface of the porous material and forms a dense wrapping layer on the surface of the porous material;
[0010] A coating layer, wherein the coating layer comprises an aqueous solution of a polymer film-forming agent, and the coating layer is uniformly coated on the surface of the filler layer; and
[0011] The powder coating layer is a dispersible dry powder, and the dispersible dry powder is optionally one or two of redispersible latex powder and plaster of Paris powder, and the powder coating layer is uniformly coated on the surface of the coating layer.
[0012] In an embodiment of the present application, the particle size of the porous material is 0.5 mm-3 mm;
[0013] Optionally, the pore size of the porous material is 0.1 μm-500 μm.
[0014] In the embodiment of the present application, the phase change temperature of the organic phase change material is 0-90°C, preferably 10-60°C, more preferably 15-45°C; the phase change enthalpy of the organic phase change material is 50-600 J / g, preferably 100-500 J / g, more preferably 120-400 J / g;
[0015] Optionally, the organic phase change material is selected from one or more of paraffin, fatty acid, linear alkane, and polyol;
[0016] Optionally, the fatty acid is selected from capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, the straight-chain alkane is selected from n-hexadecane, n-octadecane, n-eicosane or n-tetracosane, and the polyol is selected from polyethylene glycol.
[0017] In the embodiment of the present application, the powder filler is a mixture of a high thermal conductivity material and an adsorption filler, and the weight ratio of the high thermal conductivity material to the adsorption filler is 1:100-100:1;
[0018] Optionally, the high thermal conductivity material is selected from one or more of graphite, aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide; the adsorption filler is selected from one or more of diatomaceous earth powder, bentonite powder, and kaolin powder;
[0019] Optionally, the particle size of the high thermal conductivity material is 100-5000 mesh, preferably 200-3000 mesh, more preferably 300 mesh-2000 mesh; the particle size of the adsorption filler is 100-5000 mesh, preferably 200-3000 mesh, more preferably 300 mesh-2000 mesh.
[0020] In an embodiment of the present application, the polymer film-forming agent is selected from ethylene-vinyl acetate copolymer, polyacrylic acid, polyvinyl alcohol, polyurethane, polyvinyl acetate or hydroxyethyl cellulose;
[0021] Optionally, the concentration of the polymer film-forming agent is 1wt%-50wt%, preferably 3wt%-40wt%, more preferably 5wt%-30wt%;
[0022] Optionally, the coating layer is coated using a fluidized bed;
[0023] Optionally, the fluidized bed is a top-spray fluidized bed, a side-spray fluidized bed or a bottom-spray fluidized bed;
[0024] Optionally, the weight of the coating layer is 5wt%±1wt% of the weight of the composite phase-change particles encapsulating the filler layer.
[0025] In the embodiment of the present application, the particle size of the dry powder for dispersion is 50-1000 mesh, preferably 80-500 mesh, more preferably 100-300 mesh;
[0026] Optionally, the dry powder for dispersion is a mixture of redispersible latex powder and gypsum powder, and the weight ratio of the redispersible latex powder to the gypsum powder is 1:1000-1000:1.
[0027] Optionally, the weight of the powder coating layer is 5wt%±1wt% of the weight of the porous material shaped composite phase-change particles.
[0028] On the other hand, the present application provides a method for preparing the above-mentioned porous material shaped composite phase change particles, comprising the following steps:
[0029] (a1) immersing the porous material into an organic phase change material heated to a liquid state, leaving it at room temperature or under negative pressure for 0.1 to 3 hours, and obtaining composite phase change particles after solid-liquid separation;
[0030] (a2) uniformly mixing the composite phase change particles prepared in step (a1) with a powder filler until there is no obvious wetting on the surface of the composite phase change particles, and removing excess loose powder on the surface by shaking to obtain composite phase change particles including a filler layer;
[0031] (a3) coating the composite phase change particles including the filler layer prepared in step (a2) with a polymer film-forming agent in a fluidized bed until drying and forming a film, thereby obtaining porous material-shaped composite phase change particles; and
[0032] (a4) The porous material shaped composite phase change particles prepared in step (a3) are fully mixed with the redispersible latex powder in a drum coating machine until the redispersible latex powder is evenly coated on the surface of the coating layer to obtain porous material shaped composite phase change particles with a powder coating layer on the surface.
[0033] In the embodiment of the present application, the air temperature in the fluidized bed in step (a3) is lower than the phase change temperature of the phase change material, and the air flow rate is such that the composite phase change particles circulate up and down in the fluidized bed;
[0034] Optionally, the air temperature in the fluidized bed in step (a3) is 2-30°C lower than the phase change temperature of the phase change material.
[0035] On the other hand, the present application provides the use of the above-mentioned porous material shaped composite phase change particles and the porous material shaped composite phase change particles prepared according to the above-mentioned method in building materials, preferably in gypsum board, calcium silicate board, waterproof membrane, mineral wool board, putty, mortar or paint.
[0036] On the other hand, the present application provides a phase-change gypsum board, which is prepared from the porous material shaped composite phase-change particles and the porous material shaped composite phase-change particles prepared according to the above method.
[0037] On the other hand, the present application provides a method for preparing the above-mentioned phase change gypsum board, comprising the following steps:
[0038] (b1) mixing gypsum with the porous material shaped composite phase change particles and the porous material shaped composite phase change particles prepared according to the above method to obtain a mixed slurry;
[0039] (b2) The mixed slurry in step (b1) is evenly mixed with glass fiber, modified corn starch and water, poured on a face paper, and then formed and dried to obtain a phase change gypsum board.
[0040] On the other hand, the present application provides a system for preparing the above-mentioned porous material shaped composite phase change particles, comprising:
[0041] (1) A particle adsorption device, comprising:
[0042] (i) a metal container, a heating device and a cover A, wherein the metal container is used to contain an organic phase change material, the heating device heats the organic phase change material in the metal container, and the cover A is connected to the metal container by a fastening device;
[0043] (ii) a sieve barrel and a cover B, wherein the sieve mesh aperture on the sieve barrel is smaller than the aperture of the porous material and is used to contain the porous material; the sieve barrel and the cover B are immersed in the metal container as a whole, and the cover B is configured to completely immerse the porous material in the sieve barrel in the solution in the metal container;
[0044] (2) a surface filling device, which includes a mixer and a vibrator;
[0045] (3) a surface coating device comprising a fluidized bed;
[0046] (4) A material conveying device, used to lift the sieve bucket out of the metal container and convey the composite phase change particles to the mixer of the surface filler device, and to convey the material in the oscillator of the surface filler device to the fluidized bed.
[0047] In an embodiment of the present application, the fastening device is a buckle;
[0048] Optionally, the cover B is made of metal or plastic;
[0049] Optionally, the particle adsorption device further comprises: a vacuum pump, and the cover A is provided with a hole connected to the vacuum pump;
[0050] Optionally, the fluidized bed is a top-spray fluidized bed, a side-spray fluidized bed or a bottom-spray fluidized bed, preferably a bottom-spray fluidized bed.
[0051] Compared with the prior art, the advantages and beneficial effects of the present application are particularly:
[0052] (1) After the composite phase change particles are wrapped with powder fillers to form a filler layer, there are the following benefits:
[0053] a. Improve the density and mechanical properties of composite phase change particles by filling the pores and surface layers of porous materials. At the same time, it also prevents the phase change material in the composite phase change particles from absorbing heat and transforming from solid to liquid, and then flowing freely in the porous system, thereby causing the loss of phase change materials and the emptiness of porous particle channels.
[0054] b. The filler layer will not only improve the surface smoothness of the composite phase change particles, but also reduce the probability of porous particles colliding with each other during the coating process, causing damage to the pores and particle adhesion, which is beneficial to protecting the pore structure of the porous particles and carrying out subsequent surface coating steps; and compared with the composite phase change particles without a filler layer, due to the improved surface smoothness of the composite phase change particles, the surface area of a single particle is reduced, which greatly reduces the amount of polymer film-forming agent used in the surface coating step, and can reduce costs.
[0055] (2) Since powder fillers can adsorb phase change materials, the presence of the filler layer can not only protect the inner wall of the fluidized bed from being contaminated by the phase change material during the surface coating step, thereby ensuring the continuity of the processing, but also reduce the loss rate of the composite phase change particles of the exudate phase change material during the preparation process, and at the same time increase the phase change loading rate of the composite phase change particles, thereby avoiding the loss of high-value phase change materials.
[0056] (3) The composite phase change particles of the present application have a high surface flatness, which can reduce the collision damage rate in subsequent processing and application procedures.
[0057] (4) When the filler layer of the composite phase change particles of the present application includes a high thermal conductivity filler, the thermal conductivity of the phase change particles can be increased, so that the reaction rate of the phase change material to the ambient temperature is improved. At the same time, the composite phase change particle carrier is adjusted by adjusting the mixing ratio of expanded vermiculite or expanded perlite or activated carbon and expanded graphite to adjust the comprehensive thermal conductivity of the composite phase change particle carrier.
[0058] (5) When the composite phase change particles of the present application include a powder coating layer, it can not only prevent the coated composite phase change particles from sticking to each other and forming a mass, which is beneficial to the preservation of the composite phase change particles of the present application; it can also further improve the elastic modulus of the surface of the composite phase change particles during production, and prevent the composite phase change particles from being damaged due to mechanical stirring; it can also improve the adhesion and cohesion of the product in the subsequent preparation of the building slurry including the composite phase change particles of the present application, and improve the strength degradation problem caused by the addition of porous carriers.
[0059] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be realized and obtained by the schemes described in the description. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] The accompanying drawings are used to provide an understanding of the technical solution of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present application and do not constitute a limitation on the technical solution of the present application.
[0061] Figure 1 This is a microscopic SEM electron microscope image of the product of Comparative Example 1;
[0062] Figure 2 This is a microscopic SEM electron microscope image of the product of Example 1;
[0063] Figure 3 This is a microscopic SEM electron microscope image of the product of Example 2;
[0064] Figure 4 This is a schematic diagram of the structure of the composite phase change particles of the present application;
[0065] Figure 5 Schematic diagram of the structure of traditional impregnation-type composite phase change particles.
[0066] Illustration Description:
[0067] 1-composite phase change particles, 2-filling layer, 3-coating layer, 4-powder coating layer. DETAILED DESCRIPTION
[0068] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application will be described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.
[0069] The present application provides a porous material shaped composite phase change particle, comprising:
[0070] Composite phase change particles, the composite phase change particles comprising a porous material and an organic phase change material adsorbed in the pores of the porous material, the porous material being an inorganic porous material or activated carbon, and having a particle size of 0.1 mm to 5 mm;
[0071] A filler layer, wherein the filler layer is a powder filler, wherein the powder filler is optionally one or both of a high thermal conductivity material and an adsorption filler, and the filler layer is uniformly wrapped on the surface of the porous material;
[0072] A coating layer, wherein the coating layer comprises an aqueous solution of a polymer film-forming agent, and the coating layer is uniformly coated on the surface of the filler layer; and
[0073] The powder coating layer is a dispersible dry powder, and the dispersible dry powder is optionally one or two of redispersible latex powder and plaster of Paris powder, and the powder coating layer is uniformly coated on the surface of the coating layer.
[0074] In an embodiment of the present application, the particle size of the porous material is 0.5 mm-3 mm;
[0075] Optionally, the pore size of the porous material is 0.1 μm-500 μm.
[0076] In an embodiment of the present application, the inorganic porous material is selected from one or more of expanded vermiculite, expanded perlite, expanded graphite or activated carbon.
[0077] In an embodiment of the present application, the phase change temperature of the organic phase change material is 0-90°C, preferably 10-60°C, and more preferably 15-45°C; the phase change enthalpy of the organic phase change material is 50-600 J / g, preferably 100-500 J / g, and more preferably 120-400 J / g;
[0078] Optionally, the organic phase change material is selected from one or more of paraffin, fatty acid, linear alkane, and polyol;
[0079] Optionally, the fatty acid is selected from capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, the straight-chain alkane is selected from n-hexadecane, n-octadecane, n-eicosane or n-tetracosane, and the polyol is selected from polyethylene glycol.
[0080] In an embodiment of the present application, the powder filler is a mixture of a high thermal conductivity material and an adsorption filler, and the weight ratio of the high thermal conductivity material to the adsorption filler is 1:100-100:1;
[0081] Optionally, the high thermal conductivity material is selected from one or more of graphite, aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide; the adsorption filler is selected from one or more of diatomaceous earth powder, bentonite powder, and kaolin powder;
[0082] Optionally, the particle size of the high thermal conductivity material is 100-5000 mesh, preferably 200-3000 mesh, more preferably 300 mesh-2000 mesh; the particle size of the adsorption filler is 100-5000 mesh, preferably 200-3000 mesh, more preferably 300 mesh-2000 mesh.
[0083] In an embodiment of the present application, the polymer film-forming agent is selected from ethylene-vinyl acetate copolymer, polyacrylic acid, polyvinyl alcohol, polyurethane, polyvinyl acetate or hydroxyethyl cellulose;
[0084] Optionally, the concentration of the polymer film-forming agent is 1wt%-50wt%, preferably 3wt%-40wt%, more preferably 5wt%-30wt%;
[0085] Optionally, the coating layer is coated using a fluidized bed;
[0086] Optionally, the fluidized bed is a top-spray fluidized bed, a side-spray fluidized bed or a bottom-spray fluidized bed;
[0087] Optionally, the weight of the coating layer is 5wt%±1wt% of the weight of the composite phase-change particles encapsulating the filler layer.
[0088] In the embodiments of the present application,
[0089] The particle size of the dry powder for dispersion is 50-1000 mesh, preferably 80-500 mesh, more preferably 100-300 mesh;
[0090] Optionally, the dry powder for dispersion is a mixture of redispersible latex powder and gypsum powder, and the weight ratio of the redispersible latex powder to the gypsum powder is 1:1000-1000:1.
[0091] Optionally, the weight of the powder coating layer is 5wt%±1wt% of the weight of the porous material shaped composite phase-change particles.
[0092] The present application also provides a method for preparing the porous material shaped composite phase change particles, comprising the following steps:
[0093] (a1) immersing the porous material into an organic phase change material heated to a liquid state, leaving it at normal pressure or negative pressure for 0.1 to 3 hours, and obtaining composite phase change particles after solid-liquid separation;
[0094] (a2) uniformly mixing the composite phase change particles prepared in step (a1) with a powder filler until there is no obvious wetting on the surface of the composite phase change particles, and removing excess loose powder on the surface by shaking to obtain composite phase change particles including a filler layer;
[0095] (a3) coating the composite phase change particles including the filler layer prepared in step (a2) with a polymer film-forming agent in a fluidized bed until drying and forming a film, thereby obtaining porous material-shaped composite phase change particles; and
[0096] (a4) The porous material shaped composite phase change particles prepared in step (a3) are fully mixed with the redispersible latex powder in a drum coating machine until the redispersible latex powder is evenly coated on the surface of the coating layer to obtain porous material shaped composite phase change particles with a powder coating layer on the surface.
[0097] In the embodiment of the present application, the air temperature in the fluidized bed in step (a3) is lower than the phase change temperature of the phase change material, and the air flow rate is such that the composite phase change particles circulate up and down in the fluidized bed;
[0098] Optionally, the air temperature in the fluidized bed in step (a3) is 2-30°C lower than the phase change temperature of the phase change material.
[0099] The embodiments of the present application also provide the use of the above-mentioned porous material shaped composite phase change particles and the porous material shaped composite phase change particles prepared according to the above-mentioned method in building materials, preferably in gypsum board, calcium silicate board, waterproof membrane, mineral wool board, putty, mortar or paint.
[0100] The embodiment of the present application also provides a phase-change gypsum board, which is prepared from the above-mentioned porous material shaped composite phase-change particles and the porous material shaped composite phase-change particles prepared according to the above-mentioned method.
[0101] The present application also provides a method for preparing the above-mentioned phase change gypsum board, comprising the following steps:
[0102] (b1) mixing gypsum with the porous material shaped composite phase change particles and the porous material shaped composite phase change particles prepared according to the above method to obtain a mixed slurry;
[0103] (b2) The mixed slurry in step (b1) is evenly mixed with glass fiber, modified corn starch and water, poured on a face paper, and then formed and dried to obtain a phase change gypsum board.
[0104] The present application also provides a system for preparing the porous material shaped composite phase change particles, comprising:
[0105] (1) A particle adsorption device, comprising:
[0106] (i) a metal container, a heating device and a cover A, wherein the metal container is used to contain an organic phase change material, the heating device heats the organic phase change material in the metal container, and the cover A is connected to the metal container by a fastening device;
[0107] (ii) a sieve barrel and a cover B, wherein the sieve mesh aperture on the sieve barrel is smaller than the aperture of the porous material and is used to contain the porous material; the sieve barrel and the cover B are immersed in the metal container as a whole, and the cover B is configured to completely immerse the porous material in the sieve barrel in the solution in the metal container;
[0108] (2) a surface filling device, which includes a mixer and a vibrator;
[0109] (3) a surface coating device comprising a fluidized bed;
[0110] (4) A material conveying device, used to lift the sieve bucket out of the metal container and convey the composite phase change particles to the mixer of the surface filler device, and to convey the material in the oscillator of the surface filler device to the fluidized bed.
[0111] In an embodiment of the present application, the fastening device is a buckle;
[0112] Optionally, the cover B is made of metal or plastic;
[0113] Optionally, the particle adsorption device further comprises: a vacuum pump, and the cover A is provided with a hole connected to the vacuum pump;
[0114] Optionally, the fluidized bed is a top-spray fluidized bed, a side-spray fluidized bed or a bottom-spray fluidized bed, preferably a bottom-spray fluidized bed.
[0115] Example
[0116] The raw materials in the examples and comparative examples of the present application were all purchased from the market, wherein expanded vermiculite (specification: 1-2 mm) was purchased from Lingshou County Xuyang Mining Co., Ltd., expanded perlite (specification: 1-2 mm) was purchased from Shijiazhuang Aomai Mineral Products Co., Ltd., expanded graphite (specification: 2-3 mm) was purchased from Guangzhou Metal Metallurgy (Group) Co., Ltd., activated carbon (specification: 2-3 mm) was purchased from Henan Housen Environmental Protection Technology Co., Ltd., diatomaceous earth powder (specification: 1000 mesh) was purchased from Hebei Beiyan New Materials Co., Ltd., bentonite powder (specification: 1000 mesh) was purchased from Hebei Beiyan New Materials Co., Ltd. Mesh) was purchased from Hebei Kaicong Building Materials Technology Co., Ltd., kaolin powder (specification: 1000 mesh) was purchased from Hebei Kaicong Building Materials Technology Co., Ltd.; paraffin (purity: 99.5%) was purchased from Shanghai Ruentropy New Energy Technology Co., Ltd., capric acid (purity: 99.0%) was purchased from Guangzhou Baina Import and Export Co., Ltd., n-hexadecane (purity: 99.5%) was purchased from Dinghui Holdings (Guangzhou) Co., Ltd., polyethylene glycol (purity: 99.2%) was purchased from Jinan Yuansheng Chemical Co., Ltd., and lauric acid (purity: 99.0%) was purchased from Guangzhou Gongxin Chemical Co., Ltd.
[0117] Example 1
[0118] Expanded vermiculite and paraffin are used to prepare porous mineral-shaped composite phase-change particles. The phase change temperature of paraffin is 27°C, and the phase change enthalpy is 210 J / g; the particle size of expanded vermiculite is 1-2 mm; the powder filler is a mixture of graphite powder and diatomaceous earth powder in a weight ratio of 2:1; the polymer film-forming agent is polyurethane; and the fluidized bed is a bottom spray fluidized bed. The specific operations are as follows:
[0119] (1) Paraffin is placed in a metal barrel equipped with an electric heating device, heated to melt the paraffin, and then expanded vermiculite is placed in a metal screen to immerse it in the paraffin in the metal barrel, a plastic cover is pressed on the metal screen to ensure that the expanded vermiculite is completely immersed in the paraffin, and negative pressure is allowed to stand for half an hour. The expanded vermiculite and the paraffin are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0120] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining composite phase-change particles wrapped with the filler layer.
[0121] (3) The air temperature in the fluidized bed is set to 23°C, the composite phase change particles wrapped with the filler layer obtained in step (2) are placed in the fluidized bed, and the air flow rate in the fluidized bed is adjusted to make the composite phase change particles reciprocate up and down in the fluidized bed. A polyurethane aqueous solution with a concentration of 10% is prepared, and the polyurethane aqueous solution is sprayed through a spray gun to evenly fall on the surface of the composite phase change particles in reciprocating up and down motion, and the coating mass gain is controlled to be 5%±1%. After film formation, the product of the present application is obtained. Figure 2This is a microscopic SEM electron microscope image of the product in Example 1.
[0122] The test showed that the phase change enthalpy of the product was 129.3 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product was 0.94% and the thermal conductivity was 0.387 w / (mk).
[0123] In order to fully illustrate the advantages of the product of the present application, the product of the present application is applied to the preparation of phase change gypsum board, and the specific steps are as follows:
[0124] Step 1) 100 parts by weight of gypsum powder and 42 parts by weight of phase change composite coated particles are fully mixed to obtain a mixture;
[0125] Step 2) The mixture of step 1) is thoroughly mixed with 0.5 parts by weight of modified corn starch, 5 parts by weight of glass fiber and 86 parts of water, poured on a face paper to form a molding thickness of 12 mm, and then dried to constant weight in a paper-faced gypsum board dryer to obtain a phase change gypsum board.
[0126] After testing, the phase change enthalpy value of the obtained phase change gypsum board is 317.08KJ / m 2 , the transverse breaking load is 258.7N, and the longitudinal breaking load is 590.3N.
[0127] Example 2
[0128] Expanded perlite and paraffin are used to prepare porous mineral-shaped composite phase-change particles. The phase change temperature of paraffin is 27°C, and the phase change enthalpy is 210 J / g; the particle size of expanded perlite is 1-2 mm; the powder filler is a mixture of graphite powder and bentonite powder in a weight ratio of 1:2; the polymer film-forming agent is ethylene-vinyl acetate copolymer; the fluidized bed is a bottom spray fluidized bed; and the dry powder for dispersion is 120 mesh redispersible latex powder. The specific operation is as follows:
[0129] (1) Paraffin is placed in a metal barrel equipped with an electric heating device, heated to melt the paraffin, and then expanded perlite is placed in a metal screen to immerse it in the paraffin in the metal barrel. A plastic cover is pressed on the metal screen to ensure that the expanded perlite is completely immersed in the paraffin, and the mixture is left to stand at normal pressure for 1 hour. The expanded perlite and the paraffin are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0130] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining composite phase-change particles wrapped with the filler layer.
[0131] (3) The air temperature in the fluidized bed is set to 23°C, and the composite phase change particles wrapped with the filler layer obtained in step (2) are placed in the fluidized bed, and the air flow rate in the fluidized bed is adjusted to make the composite phase change particles reciprocate up and down in the fluidized bed. A 20% concentration of ethylene-vinyl acetate copolymer solution is prepared, and the ethylene-vinyl acetate copolymer solution is sprayed through a spray gun to evenly fall on the surface of the composite phase change particles in up and down reciprocating motion, and the coating mass gain is controlled to be 5±1%. After film formation, composite phase change particles wrapped with a coating layer are obtained.
[0132] (4) After the composite phase change particles coated with the coating layer obtained in step (3) are fully mixed with the redispersible latex powder, they are shaken back and forth to remove excess loose powder on the surface, and the weight gain of the coated powder is controlled to be 5%±1% to obtain the product of the present application.
[0133] The test showed that the phase change enthalpy of the product was 136.5 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product was 1.2% and the thermal conductivity was 0.176 w / (mk).
[0134] In order to fully illustrate the advantages of the product of the present application, the product of the present application is applied to the preparation of phase change gypsum board, and the specific steps are as follows:
[0135] Step 1) 100 parts by weight of gypsum powder and 42 parts by weight of phase change composite coated particles are fully mixed to obtain a mixture;
[0136] Step 2) The mixture of step 1) is thoroughly mixed with 0.5 parts by weight of modified corn starch, 5 parts by weight of glass fiber and 86 parts of water, poured on a face paper to form a molding thickness of 12 mm, and then dried to constant weight in a paper-faced gypsum board dryer to obtain a phase change gypsum board.
[0137] After testing, the phase change enthalpy value of the obtained phase change gypsum board is 334.73KJ / m 2 , the transverse breaking load is 294.2N, and the longitudinal breaking load is 635.2N.
[0138] Example 3
[0139] Expanded graphite and paraffin are used to prepare porous mineral-shaped composite phase-change particles. The phase change temperature of paraffin is 27°C, and the phase change enthalpy is 210 J / g; the particle size of expanded graphite is 2-3 mm; the powder filler is a mixture of graphite powder and kaolin powder in a weight ratio of 2:1; the polymer film-forming agent is polyacrylic acid; the fluidized bed is a bottom spray fluidized bed; and the dry powder for dispersion is 120 mesh redispersible latex powder. The specific operation is as follows:
[0140] (1) Paraffin is placed in a metal barrel equipped with an electric heating device, heated to melt the paraffin, and then expanded graphite is placed in a metal screen to immerse it in the paraffin in the metal barrel. A plastic cover is pressed on the metal screen to ensure that the expanded graphite is completely immersed in the paraffin, and the negative pressure is left to stand for half an hour. The expanded graphite and the paraffin are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0141] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining composite phase-change particles wrapped with the filler layer.
[0142] (3) The air temperature in the fluidized bed is set to 23°C, and the composite phase-change particles wrapped with the filler layer obtained in step (2) are placed in the fluidized bed. The air flow rate in the fluidized bed is adjusted so that the composite phase-change particles move up and down in the fluidized bed. A polyacrylic acid aqueous solution with a concentration of 10% is prepared, and the polyacrylic acid aqueous solution is sprayed through a spray gun to evenly fall on the surface of the composite phase-change particles in up and down reciprocating motion, and the coating mass gain is controlled to be 5±1%. After film formation, composite phase-change particles wrapped with a coating layer are obtained.
[0143] (4) After the composite phase change particles wrapped with the coating layer obtained in step (3) are fully mixed with the gypsum powder, they are shaken back and forth to remove excess loose powder on the surface, and the weight gain of the powder coating is controlled to be 5%±1% to obtain the product of the present application.
[0144] The test showed that the phase change enthalpy of the product was 169.91 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product was 1.35%, and the thermal conductivity was 8.586 w / (mk).
[0145] In order to fully illustrate the advantages of the product of the present application, the product of the present application is applied to the preparation of phase change gypsum board, and the specific steps are as follows:
[0146] Step 1) 100 parts by weight of gypsum powder and 42 parts by weight of phase change composite coated particles are fully mixed to obtain a mixture;
[0147] Step 2) The mixture of step 1) is thoroughly mixed with 0.5 parts by weight of modified corn starch, 5 parts by weight of glass fiber and 86 parts of water, poured on a face paper to form a molding thickness of 12 mm, and then dried to constant weight in a paper-faced gypsum board dryer to obtain a phase change gypsum board.
[0148] After testing, the phase change enthalpy value of the obtained phase change gypsum board is 437.49KJ / m 2 , the transverse breaking load is 274.2N, and the longitudinal breaking load is 604.14N.
[0149] Example 4
[0150] Activated carbon and decanoic acid are used to prepare porous mineral-shaped composite phase-change particles. The decanoic acid phase change temperature is 30°C, and the phase change enthalpy is 173.6 J / g; the particle size of the activated carbon is 2-3 mm; the powder filler is a mixture of graphite powder and diatomaceous earth powder in a weight ratio of 2:1; the polymer film-forming agent is polyvinyl alcohol; the fluidized bed is a bottom spray fluidized bed; and the dry powder for dispersion is 120 mesh redispersible latex powder. The specific operation is as follows:
[0151] (1) Place capric acid in a metal barrel equipped with an electric heating device, heat it to melt the capric acid, then place activated carbon in a metal screen to immerse it in the capric acid in the metal barrel, press a plastic cover on the metal screen to ensure that the activated carbon is completely immersed in the capric acid, and let it stand for half an hour under negative pressure. The activated carbon and capric acid are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0152] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining composite phase-change particles wrapped with the filler layer.
[0153] (3) Set the air temperature in the fluidized bed to 25°C, place the composite phase-change particles wrapped with the filler layer obtained in step (2) into the fluidized bed, adjust the air flow rate in the fluidized bed, and make the composite phase-change particles reciprocate up and down in the fluidized bed. Prepare a polyvinyl alcohol aqueous solution with a concentration of 10%, and make the polyvinyl alcohol aqueous solution fall evenly on the surface of the composite phase-change particles in up and down reciprocating motion through a spray gun, and control the coating mass gain to 5±1%. After film formation, composite phase-change particles wrapped with a coating layer are obtained.
[0154] (4) After the composite phase change particles wrapped with the coating layer obtained in step (3) are fully mixed with the gypsum powder, they are shaken back and forth to remove excess loose powder on the surface, and the weight gain of the powder coating is controlled to be 5±1% to obtain the product of the present application.
[0155] The test showed that the phase change enthalpy of the obtained product was 145.19 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product was 0.77% and the thermal conductivity was 0.653 w / (mk).
[0156] Example 5
[0157] Expanded vermiculite and n-hexadecane were used to prepare porous mineral-shaped composite phase-change particles. The phase change temperature of n-hexadecane was 18°C and the enthalpy value was 195 J / g; the particle size of expanded vermiculite was 1-2 mm; the powder filler was a mixture of graphite powder and diatomaceous earth powder in a weight ratio of 1:4; the polymer film-forming agent was polyethylene glycol; the fluidized bed was a bottom spray fluidized bed; and the dry powder for dispersion was 120 mesh redispersible latex powder. The specific operation is as follows:
[0158] (1) Put n-hexadecane into a metal barrel equipped with an electric heating device, heat it to melt the n-hexadecane, then put expanded vermiculite into a metal screen to immerse it in the n-hexadecane in the metal barrel, press a plastic cover on the metal screen to ensure that the expanded vermiculite is completely immersed in the n-hexadecane, and let it stand for half an hour under negative pressure. The expanded vermiculite and n-hexadecane are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0159] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining composite phase-change particles wrapped with the filler layer.
[0160] (3) Set the air temperature in the fluidized bed to 15°C, place the composite phase-change particles wrapped with the filler layer obtained in step (2) into the fluidized bed, adjust the air flow rate in the fluidized bed, and make the composite phase-change particles reciprocate up and down in the fluidized bed. Prepare a polyethylene glycol aqueous solution with a concentration of 10%, and make the polyethylene glycol aqueous solution fall evenly on the surface of the composite phase-change particles in reciprocating up and down motion through a spray gun, and control the coating mass gain to 5%±1%. After film formation, composite phase-change particles wrapped with a coating layer are obtained.
[0161] (4) After the composite phase change particles coated with the coating layer obtained in step (3) are fully mixed with the redispersible latex powder, they are shaken back and forth to remove excess loose powder on the surface, and the weight gain of the coated powder is controlled to be 5%±1% to obtain the product of the present application.
[0162] The test showed that the phase change enthalpy of the product was 114.35 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product was 1.68%, and the thermal conductivity was 0.316 w / (mk).
[0163] Example 6
[0164] Expanded vermiculite and polyethylene glycol were used to prepare porous mineral-shaped composite phase-change particles. The phase change temperature of polyethylene glycol PEG1000 was 45°C and the enthalpy value was 140 J / g; the particle size of expanded vermiculite was 1-2 mm; the powder filler was a mixture of graphite powder and diatomaceous earth powder in a weight ratio of 3:1; the polymer film-forming agent was polyacrylic acid; the fluidized bed was a bottom-spraying fluidized bed; and the dry powder for dispersion was 120 mesh redispersible latex powder. The specific operation is as follows:
[0165] (1) Put polyethylene glycol into a metal barrel equipped with an electric heating device, heat it to melt the polyethylene glycol, then put expanded vermiculite into a metal screen to immerse it in the polyethylene glycol in the metal barrel, press a plastic cover on the metal screen to ensure that the expanded vermiculite is completely immersed in the polyethylene glycol, and let it stand for half an hour under negative pressure. The expanded vermiculite and polyethylene glycol are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0166] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining composite phase-change particles wrapped with the filler layer.
[0167] (3) Set the air temperature in the fluidized bed to 25°C, place the composite phase-change particles wrapped with the filler layer obtained in step (2) into the fluidized bed, adjust the air flow rate in the fluidized bed, and make the composite phase-change particles reciprocate up and down in the fluidized bed. Prepare a polyacrylic acid aqueous solution with a concentration of 10%, and make the polyacrylic acid aqueous solution fall evenly on the surface of the composite phase-change particles in up and down reciprocating motion through a spray gun, and control the coating mass gain to 5±1%. After film formation, composite phase-change particles wrapped with a coating layer are obtained.
[0168] (4) After the composite phase change particles coated with the coating layer obtained in step (3) are fully mixed with the redispersible latex powder, they are shaken back and forth to remove excess loose powder on the surface, and the weight gain of the coated powder is controlled to be 5%±1% to obtain the product of the present application.
[0169] The test showed that the phase change enthalpy of the product was 82.10 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product was 1.12% and the thermal conductivity was 0.431 w / (mk).
[0170] Comparative Example 1
[0171] The difference between this comparative example and Example 1 is that the composite phase change particles prepared in (1) are dried to obtain the product of this comparative example, and the subsequent surface filling and surface coating steps are not performed. Figure 1 This is the microscopic SEM electron microscope image of the product of Comparative Example 1.
[0172] In this comparative example, expanded vermiculite and paraffin are used to prepare porous mineral-shaped composite phase-change particles. The phase-change temperature of paraffin is 27°C, the phase-change enthalpy is 210 J / g, and the particle size of expanded vermiculite is 1-2 mm. The specific operation is as follows:
[0173] Put paraffin into a metal barrel equipped with an electric heating device, heat it to melt the paraffin, then put expanded vermiculite into a metal screen to immerse it in the paraffin in the metal barrel, press a plastic cover on the metal screen to ensure that the expanded vermiculite is completely immersed in the paraffin, and let it stand for half an hour under negative pressure. The expanded vermiculite and paraffin are separated into solid and liquid by lifting the metal screen upwards, and after drying at 45°C, composite phase change particles are obtained.
[0174] The test shows that the phase change enthalpy of the product obtained in this comparative example is 136.1 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product is 42.7%, and the thermal conductivity is 0.261 w / (mk).
[0175] Compared with Example 1, the phase change enthalpy of the product obtained in this comparative example is higher because no surface filler and surface coating are performed. However, surface oil seepage occurs during the test, resulting in a mass loss rate of 42.7% for the product.
[0176] Comparative Example 2
[0177] The difference between this comparative example and Example 1 is that after the composite phase change particles in (1) are prepared, the surface filling process is not performed, and the surface coating process is directly performed.
[0178] In this comparative example, expanded vermiculite and paraffin are used to prepare porous mineral-shaped composite phase-change particles. The phase-change temperature of paraffin is 27°C, and the phase-change enthalpy is 210 J / g; the particle size of expanded vermiculite is 1-2 mm; the polymer film-forming agent is polyurethane; and the fluidized bed is a bottom-spraying fluidized bed. The specific operation is as follows:
[0179] (1) Paraffin is placed in a metal barrel equipped with an electric heating device, heated to melt the paraffin, and then expanded vermiculite is placed in a metal screen to immerse it in the paraffin in the metal barrel, a plastic cover is pressed on the metal screen to ensure that the expanded vermiculite is completely immersed in the paraffin, and negative pressure is allowed to stand for half an hour. The expanded vermiculite and the paraffin are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0180] (2) The air temperature in the fluidized bed is set to 23°C, the composite phase change particles obtained in step (1) are placed in the fluidized bed, and the air flow rate in the fluidized bed is adjusted to make the composite phase change particles reciprocate up and down in the fluidized bed. A polyurethane aqueous solution with a concentration of 10% is prepared, and the polyurethane aqueous solution is sprayed through a spray gun to evenly fall on the surface of the composite phase change particles in reciprocating up and down motion, and the coating mass gain is controlled to be 5±1%. After film formation, the product of this comparative example is obtained.
[0181] After testing, the phase change enthalpy of the product obtained in this comparative example is 132.7 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product is 10.76%, and the thermal conductivity is 0.233w / (mk).
[0182] Compared with Example 1, the amount of polyurethane aqueous solution used increased by about 66.1%. During the coating process, due to the low flatness of the particle surface, the coating was uneven, resulting in particle overlapping, which led to an unsatisfactory final coating effect. The main reason is the lack of fillers on the particle surface, the uneven particle surface, the polymer film-forming agent cannot fall evenly on the surface of the mineral particles, and the protruding parts of the particle surface obtain more polymer film-forming agent than the concave parts of the particle surface, which results in the polymer film-forming agent on the protruding parts of the adjacent particle surfaces cannot be dried in time to form a film, resulting in adhesion and overlapping, forming a clumping of three or two, and the coating process cannot be carried out effectively.
[0183] Comparative Example 3
[0184] The difference between this comparative example and Example 1 is that after the composite phase-change particles wrapped with the filler layer in (2) are prepared, the product of this comparative example is obtained, and no subsequent surface coating process is performed.
[0185] In this comparative example, expanded vermiculite and paraffin are used to prepare porous mineral-shaped composite phase-change particles. The phase-change temperature of paraffin is 27°C, and the phase-change enthalpy is 210 J / g; the particle size of expanded vermiculite is 1-2 mm; and the powder filler is a mixture of graphite powder and diatomaceous earth powder in a weight ratio of 2:1. The specific operation is as follows:
[0186] (1) Paraffin is placed in a metal barrel equipped with an electric heating device, heated to melt the paraffin, and then expanded vermiculite is placed in a metal screen to immerse it in the paraffin in the metal barrel, a plastic cover is pressed on the metal screen to ensure that the expanded vermiculite is completely immersed in the paraffin, and negative pressure is allowed to stand for half an hour. The expanded vermiculite and the paraffin are separated into solid and liquid by lifting the metal screen upward to obtain composite phase change particles.
[0187] (2) The composite phase-change particles obtained in step (1) are thoroughly mixed with the powder filler, and then shaken back and forth to remove excess loose powder on the surface, thereby obtaining the product of this comparative example.
[0188] After testing, the phase change enthalpy of the product obtained in this comparative example is 123.14 J / g. After 1000 high and low temperature melting-solidification cycle tests, the mass loss rate of the product is 38.4%, and the thermal conductivity is 0.392 w / (mk).
[0189] The phase change composite particles prepared in this comparative example are mixed with building plaster powder to prepare a phase change gypsum board in the following steps:
[0190] Step 1) 100 parts by weight of gypsum powder and 42 parts by weight of phase change composite coated particles are fully mixed to obtain a mixture;
[0191] Step 2) The mixture of step 1) is thoroughly mixed with 0.5 parts by weight of modified corn starch, 5 parts by weight of glass fiber and 86 parts of water, poured on a face paper to form a molding thickness of 12 mm, and then dried to constant weight in a paper-faced gypsum board dryer to obtain a phase change gypsum board.
[0192] After testing, the phase change enthalpy value of the obtained phase change gypsum board is 224.38KJ / m 2 , the transverse breaking load is 167.22N, and the longitudinal breaking load is 351.75N.
[0193] Compared with Example 1, the phase-change gypsum board prepared in this comparative example has the phenomenon that the face paper is partially not stained and the face paper has stains. This is mainly due to the paraffin exudation, which hinders the starch migration process of the gypsum board core and cannot smoothly reach the face paper layer, affecting the bonding effect between the face paper and the board core. In addition, the dryer can smell obvious paraffin odor, and the surface of the gypsum board conveyor roller is oily. This shows that the paraffin of the phase-change composite particles melts into liquid and accelerates the leakage to the face paper layer and the equipment surface during the gypsum board drying process, which not only wastes materials and fails to produce qualified phase-change products, but also has a negative impact on the gypsum board production line, and the roller needs to be cleaned, causing an additional burden.
[0194] Figure 4 This is a schematic diagram of the structure of the composite phase change particles of the present application; Figure 5 Schematic diagram of the structure of traditional impregnation composite phase change particles
[0195] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.
Claims
1. A porous material shaped composite phase change particle, comprising: Composite phase change particles, the composite phase change particles comprising a porous material and an organic phase change material adsorbed in the pores of the porous material, the porous material being an inorganic porous material or activated carbon, and having a particle size of 0.1 mm to 5 mm; A filler layer, wherein the filler layer is a powder filler, wherein the powder filler is optionally one or both of a high thermal conductivity material and an adsorption filler, and the filler layer is uniformly wrapped on the surface of the porous material; A coating layer, the coating layer comprising an aqueous solution of a polymer film-forming agent, and the coating layer is uniformly wrapped on the surface of the filler layer; as well as The powder coating layer is a dry powder for dispersion, wherein the dry powder for dispersion is optionally one or both of redispersible latex powder and plaster of Paris powder, and the powder coating layer is uniformly coated on the surface of the coating layer.
2. The porous material shaped composite phase change particle according to claim 1, wherein: The particle size of the porous material is 0.5 mm to 3 mm; Optionally, the pore size of the porous material is 0.1 μm-500 μm.
3. The porous material shaped composite phase change particle according to claim 1, wherein: The inorganic porous material is selected from one or more of expanded vermiculite, expanded perlite, expanded graphite or activated carbon.
4. The porous material shaped composite phase change particle according to claim 1, wherein: The phase change temperature of the organic phase change material is 0-90°C, preferably 10-60°C, more preferably 15-45°C; the phase change enthalpy of the organic phase change material is 50-600 J / g, preferably 100-500 J / g, more preferably 120-400 J / g; Optionally, the organic phase change material is selected from one or more of paraffin, fatty acid, linear alkane, and polyol; Optionally, the fatty acid is selected from capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, the straight-chain alkane is selected from n-hexadecane, n-octadecane, n-eicosane or n-tetracosane, and the polyol is selected from polyethylene glycol.
5. The porous material shaped composite phase change particle according to claim 1, wherein: The powder filler is a mixture of a high thermal conductivity material and an adsorption filler, and the weight ratio of the high thermal conductivity material to the adsorption filler is 1:100-100:1; Optionally, the high thermal conductivity material is selected from one or more of graphite, aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide; the adsorption filler is selected from one or more of diatomaceous earth powder, bentonite powder, and kaolin powder; Optionally, the particle size of the high thermal conductivity material is 100-5000 mesh, preferably 200-3000 mesh, more preferably 300 mesh-2000 mesh; the particle size of the adsorption filler is 100-5000 mesh, preferably 200-3000 mesh, more preferably 300 mesh-2000 mesh.
6. The porous material shaped composite phase change particle according to claim 1, wherein: The polymer film-forming agent is selected from ethylene-vinyl acetate copolymer, polyacrylic acid, polyvinyl alcohol, polyurethane, polyvinyl acetate or hydroxyethyl cellulose; Optionally, the concentration of the polymer film-forming agent is 1wt%-50wt%, preferably 3wt%-40wt%, more preferably 5wt%-30wt%; Optionally, the coating layer is coated using a fluidized bed; Optionally, the fluidized bed is a top-spray fluidized bed, a side-spray fluidized bed or a bottom-spray fluidized bed; Optionally, the weight of the coating layer is 5wt%±1wt% of the weight of the composite phase-change particles encapsulating the filler layer.
7. The porous material shaped composite phase-change particle according to any one of claims 1 to 6, wherein: The particle size of the dry powder for dispersion is 50-1000 mesh, preferably 80-500 mesh, more preferably 100-300 mesh; Optionally, the dry powder for dispersion is a mixture of redispersible latex powder and plaster of Paris powder, and the weight ratio of the redispersible latex powder to the plaster of Paris powder is 1:1000-1000:1; Optionally, the weight of the powder coating layer is 5wt%±1wt% of the weight of the porous material shaped composite phase-change particles.
8. A method for preparing the porous material shaped composite phase change particles according to any one of claims 1 to 7, comprising the following steps: (a1) immersing the porous material into an organic phase change material heated to a liquid state, leaving it at normal pressure or negative pressure for 0.1 to 3 hours, and obtaining composite phase change particles after solid-liquid separation; (a2) uniformly mixing the composite phase change particles prepared in step (a1) with a powder filler until there is no obvious wetting on the surface of the composite phase change particles, and removing excess loose powder on the surface by shaking to obtain composite phase change particles including a filler layer; (a3) coating the composite phase change particles including the filler layer prepared in step (a2) with a polymer film-forming agent in a fluidized bed until drying and forming a film, thereby obtaining porous material-shaped composite phase change particles; and (a4) The porous material shaped composite phase change particles prepared in step (a3) are fully mixed with the redispersible latex powder in a drum coating machine until the redispersible latex powder is evenly coated on the surface of the coating layer to obtain porous material shaped composite phase change particles with a powder coating layer on the surface.
9. The method according to claim 8, wherein: The air temperature in the fluidized bed in step (a3) is lower than the phase change temperature of the phase change material, and the air flow rate is such that the composite phase change particles circulate up and down in the fluidized bed; Optionally, the air temperature in the fluidized bed in step (a3) is 2-30°C lower than the phase change temperature of the phase change material.
10. Use of the porous material shaped composite phase-change particles according to any one of claims 1 to 7 and the porous material shaped composite phase-change particles prepared by the method according to any one of claims 8 to 9 in building materials, preferably in gypsum boards, calcium silicate boards, waterproof membranes, mineral wool boards, putties, mortars or coatings.
11. A phase-change gypsum board, wherein the phase-change gypsum board is made of the porous material shaped composite phase-change particles according to any one of claims 1 to 7 and the porous material shaped composite phase-change particles prepared by the method according to any one of claims 8 to 9.
12. A method for preparing the phase change gypsum board according to claim 11, comprising the following steps: (b1) mixing gypsum with the porous material shaped composite phase-change particles according to any one of claims 1 to 7 and the porous material shaped composite phase-change particles prepared by the method according to any one of claims 8 to 9 to obtain a mixed slurry; (b2) The mixed slurry in step (b1) is evenly mixed with glass fiber, modified corn starch and water, poured on a face paper, and then formed and dried to obtain a phase change gypsum board.
13. A system for preparing porous material shaped composite phase-change particles according to any one of claims 1 to 7, comprising: (1) A particle adsorption device, comprising: (i) a metal container, a heating device and a cover A, wherein the metal container is used to contain an organic phase change material, the heating device heats the organic phase change material in the metal container, and the cover A is connected to the metal container by a fastening device; (ii) a sieve barrel and a cover B, wherein the sieve mesh aperture on the sieve barrel is smaller than the aperture of the porous material and is used to contain the porous material; the sieve barrel and the cover B are immersed in the metal container as a whole, and the cover B is configured to completely immerse the porous material in the sieve barrel in the solution in the metal container; (2) a surface filling device, which includes a mixer and a vibrator; (3) a surface coating device comprising a fluidized bed; (4) A material conveying device, used to lift the sieve bucket out of the metal container and convey the composite phase change particles to the mixer of the surface filler device, and to convey the material in the oscillator of the surface filler device to the fluidized bed.
14. The system according to claim 13, wherein: The fastening device is a buckle; Optionally, the cover B is made of metal or plastic; Optionally, the particle adsorption device further comprises: a vacuum pump, and the cover A is provided with a hole connected to the vacuum pump; Optionally, the fluidized bed is a top-spray fluidized bed, a side-spray fluidized bed or a bottom-spray fluidized bed, preferably a bottom-spray fluidized bed.
Citation Information
Patent Citations
Preparation method of porous medium composite phase change energy storage particles
CN103666380A
Form-stable phase change material with multilevel package structure and preparation method thereof
CN108048043A
Porous graphite-based phase-transition heat-accumulation gypsum board, and preparation method thereof
CN109180125A
Molecular sieve / diatomite-based low-thermal-conductivity composite shape-stabilized phase change material and preparation method thereof
CN115044351A
High-strength anti-seepage phase change particle for cement-based material and preparation method of high-strength anti-seepage phase change particle