Ultrahigh-toughness cement-based composite material and preparation method thereof
By using basalt powder and basalt sand to replace fly ash and quartz sand, and combining it with polyvinyl alcohol fiber, the problem of uneven resource distribution and insufficient performance in the preparation of ECC materials is solved, and the material performance is improved and the cost is reduced. It is suitable for Restoration and construction of various engineering structures.
Patent Information
- Application Number
- CN202410788604.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing ultra-high toughness cementitious composites (ECC) rely on fly ash and quartz sand in the preparation process, resulting in uneven resource distribution, high cost, complex processes and insufficient performance, hindering their widespread application.
Basalt powder and basalt sand are used to replace fly ash and quartz sand, combined with polyvinyl alcohol fiber, and a specific mixing process is used to prepare ultra-high toughness cement-based composite materials to improve the mechanical properties and durability of the material.
It achieves improved material performance, tensile ductility and strength, reduces preparation costs and process complexity, provides a wider source of raw materials, is suitable for the construction and repair of a variety of engineering structures, and enhances the durability and durability of the structure. Shock resistance.
Smart Images

Figure BDA0004899322170000091 
Figure BDA0004899322170000111 
Figure HDA0004899322180000011
Abstract
Description
Technical Field
[0001] The present invention belongs to cement-based composite materials and their preparation, and relates to an ultra-high toughness cement-based composite material and its preparation method. The ultra-high toughness cement-based composite material (prepared) of the present invention is particularly suitable for the construction and repair and reinforcement of engineering structures such as water conservancy projects, port and sea projects, transportation projects, bridge and tunnel projects, and underground projects, and can effectively improve the durability and earthquake resistance of the structure. Background Art
[0002] Ultra-high toughness cement-based composites are also called engineering cement-based composites (ECC for short). When stretched, the ductility of this material can reach 3% or even higher. The tensile stress-strain curve has yield and strengthening stages similar to those of steel. Before failure, it often shows multi-crack cracking. Its strain capacity is hundreds of times that of ordinary cement-based materials. The characteristics of ultra-high ductility make this material show great application potential in the fields of structural repair, spraying construction, 3D printing, etc. Due to its extremely high toughness, this material is mainly used for structural repair and reinforcement, which can significantly improve the durability and earthquake resistance of old buildings, such as the repair of old houses, the repair of slopes, and the repair of dam projects. In addition, it can be used to prepare high-toughness components in the field of 3D printing; it has also been widely used in the repair of bridge panels or tough connections.
[0003] In the prior art, the preparation of ECC materials usually requires raw materials such as cement, quartz sand, fly ash, fiber and water; among them, quartz sand and fly ash often account for more than 60%, and the demand is large, while high-quality quartz sand and fly ash are restricted by the production area and are distributed relatively concentratedly; there are many thermal power plants in the north of my country, and fly ash resources are abundant, while hydropower is the main source in the south, and fly ash resources are scarce. Quartz sand resources are also restricted by the production area. In addition, due to the light weight and porous surface of fly ash, the mechanical properties and durability of ECC materials are insufficient. The restrictions on the production area of raw materials and the shortcomings in performance have seriously hindered the promotion and application of ECC.
[0004] CN114751701A discloses "a high-toughness cement-based composite material and its preparation method". In addition to conventional raw materials such as cement, fly ash, and quartz sand, the disclosed high-toughness cement-based composite material also needs to use nano-ettringite whiskers; CN115594523A discloses "a high-toughness cement-based composite material and its preparation method". In order to further improve the toughness of ECC, a technical solution of first preparing a porous cement-based preform and then impregnating the cement-based preform with resin in a vacuum state is proposed; CN113912374A discloses "powder 3D printing high-strength and high-toughness cement-based material and its preparation method". The technical solution uses raw materials such as phosphate composite powder containing fly ash and quartz sand, a reinforcing and toughening liquid containing a variety of organic substances, and a reinforcing and toughening powder containing carbon nanotubes. These existing technologies generally have the disadvantages of complex material selection, high cost, and cumbersome preparation process, and none of them has gotten rid of the dependence on fly ash and quartz sand. Finding new materials to further improve the performance of ECC is of great significance to the promotion and application of ECC. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the above-mentioned prior art and provide an ultra-high toughness cement-based composite material and a preparation method thereof, thereby providing an ultra-high toughness cement-based composite material and a preparation method thereof with a wide source of raw materials, a simple preparation process, low cost, and good material properties.
[0006] The content of the present invention is: an ultra-high toughness cement-based composite material, characterized in that: the raw material components and mass parts of the ultra-high toughness cement-based composite material are: 1 to 5 parts of cement, 2 to 6 parts of basalt powder, 0.5 to 4 parts of basalt sand, 0.001 to 0.01 parts of water reducer, 0.05 to 0.07 parts of fiber, and 1 to 1.5 parts of water.
[0007] In the present invention, the cement can be silicate cement or ordinary silicate cement (cement strength grade is not less than 42.5). These two types of cement have high clinker content and stable mechanical properties.
[0008] In the present invention, the basalt powder is obtained by crushing and grinding basalt ore, and the specific surface area is preferably 600m 2 / kg~800m 2 / kg; when the specific surface area is too small (less than 600m 2 / kg), its reaction activity is low, which will seriously affect the mechanical properties of ECC; if the specific surface area is too large (greater than 800m 2 / kg), which will cause a surge in the amount of water required for ECC materials, affecting the construction performance of ECC; when the specific surface area is between 600m 2 / kg~800m 2 / kg, its reactivity is equivalent to that of fly ash, and it can be used as a good substitute for fly ash;
[0009] The fineness of the basalt sand is 40-100 meshes. If the sand is too coarse, the unevenness of ECC will increase, and if it is too fine, the water demand will increase, and the shrinkage of ECC will also increase.
[0010] In the content of the present invention: the main chemical composition and mass percentage of the basalt can be: SiO2 (silicon dioxide) 45% to 52%, Al2O3 (aluminum oxide) 7 to 25%, and Fe2O3 (iron oxide), CaO (calcium oxide), MgO (magnesium oxide), K2O (potassium oxide), Na2O (sodium oxide), etc., and the sum of each component is 100%.
[0011] In the content of the present invention: the water reducer is a polycarboxylate water reducer, and the product production and providing enterprises include Sichuan Tongzhou Chemical, BASF of Germany, Sichuan Tongxingyuan and other companies, or other existing commercially available polycarboxylate water reducer product production and providing enterprises.
[0012] In the context of the present invention: the fiber can be polyvinyl alcohol fiber or polyethylene fiber, both of which have sufficient toughness and elastic modulus;
[0013] The polyvinyl alcohol fiber has a diameter of 35-45 μm, a tensile strength of ≥1600 MPa, an elongation at break of ≥6.5%, an elastic modulus of ≥41 GPa, and a fiber length of 8-12 mm;
[0014] The polyethylene fiber has a diameter of 22-30 μm, a tensile strength of ≥3100 MPa, an elongation at break of ≥10%, an elastic modulus of ≥100 GPa, and a fiber length of 8-12 mm.
[0015] In the content of the present invention: the main chemical composition and mass percentage of the basalt can be specifically: SiO2 (silicon dioxide) 49.88%, Al2O3 (aluminum oxide) 15.08%, Fe2O3 (iron oxide) 12.07%, CaO (calcium oxide) 9.26%, MgO (magnesium oxide) 5.78%, K2O (potassium oxide) 1.08%, Na2O (sodium oxide) 3.67%, TiO2 (titanium dioxide) 2.3%, P2O5 (phosphorus pentoxide) 0.39%, MnO (manganese oxide) 0.15%, SO3 (sulfur trioxide) 0.08%, SrO (strontium oxide) 0.05%, Cr2O3 (chromium oxide) 0.21%, and the sum of each component is 100%.
[0016] Alternatively, the main chemical composition and mass percentage of the basalt can be specifically: SiO2 (silicon dioxide) 47.88%, Al2O3 (aluminum oxide) 13.51%, Fe2O3 (iron oxide) 15.32%, CaO (calcium oxide) 10.26%, MgO (magnesium oxide) 4.71%, K2O (potassium oxide) 1.12%, Na2O (sodium oxide) 2.65%, TiO2 (titanium dioxide) 3.21%, P2O5 (phosphorus pentoxide) 0.41%, MnO (manganese oxide) 0.11%, SO3 (sulfur trioxide) 0.09%, SrO (strontium oxide) 0.02%, Cr2O3 (chromium oxide) 0.71%, and the sum of each component is 100%.
[0017] Another aspect of the present invention is: a method for preparing an ultra-high toughness cement-based composite material, characterized by the steps of:
[0018] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of cement 1-5 parts, basalt powder 2-6 parts, basalt sand 0.5-4 parts, water reducer 0.001-0.01 parts, fiber 0.05-0.07 parts, water 1-1.5 parts; the specific raw materials of each component are as described in the content of the present invention;
[0019] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 30s to 50s (to make the dry materials preliminarily mixed evenly);
[0020] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 60s to 80s, then stir quickly for 30s to 60s to make the material into a uniform slurry;
[0021] d. Add the fiber into the mixer twice. For the first time, add about 2 / 3 of the fiber and stir slowly for 120s to 180s. Then slowly add the remaining 1 / 3 of the fiber and stir slowly for 120s to 160s. Then stir quickly for 60s to 120s. After stirring, the ultra-high toughness cement-based composite material is obtained.
[0022] In another aspect of the present invention: the rotation speed of the slow stirring is preferably controlled at 60-70 r / min, and the rotation speed of the fast stirring is preferably controlled at 100-120 r / min.
[0023] Compared with the prior art, the present invention has the following characteristics and beneficial effects:
[0024] (1) According to the present invention, basalt is a magmatic rock that is widely distributed on the surface of the earth. It is mainly composed of pyroxene, plagioclase and olivine. It is a hard and strong mineral with extremely stable physical and chemical properties. Its mechanical properties are better than those of fly ash and quartz sand. Therefore, the ECC material prepared by using basalt powder and basalt sand instead of fly ash and quartz sand can improve the performance of ECC, and can improve the mechanical properties and durability of ECC.
[0025] (2) The present invention overcomes the dependence on fly ash and quartz sand on the one hand; on the other hand, the prepared ECC material has higher tensile ductility and strength, with the tensile ductility increased by more than 50% and the tensile strength increased by more than 100%; the reason for the improvement of tensile ductility and strength is mainly because basalt has higher density and hardness than fly ash and quartz sand. In addition, after the basalt is ultra-finely treated (the specific surface area of fly ash is about 350-450m 2 / kg, the specific surface area of the basalt powder used in the technical solution of the present invention is 600m 2 / kg-800m 2 / kg), which can play a good filling role, increase the interface transition zone between cement and basalt particles, and is conducive to the generation of small cracks (the interface transition zone is a weak link and is prone to microcracks). At the same time, the hard basalt particles in it help to eliminate the tip stress of large cracks, avoid the generation of large cracks and promote the occurrence of multiple cracks, so it helps to improve the tensile ductility and strength of ECC;
[0026] (3) The product preparation process of the present invention is simple, the raw material source is wide, the cost is low, and it is easy to operate. The prepared ultra-high toughness cement-based composite material is particularly suitable for the construction and repair and reinforcement of engineering structures such as water conservancy projects, port and marine projects, transportation projects, bridge and tunnel projects, and underground projects. It can effectively improve the durability and seismic resistance of the structure and has strong practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the tensile stress-strain curve of the ultra-high toughness cement-based composite material obtained in Example 1 of the present invention, with an elongation at break exceeding 7% and a tensile strength exceeding 5.5 MPa; the figure shows that the obtained ECC has good tensile ductility and strength;
[0028] Figure 2 This is the tensile stress-strain curve of the ultra-high toughness cement-based composite material obtained in Example 2 of the present invention, with an elongation at break exceeding 6% and a tensile strength exceeding 5.5 MPa; the figure shows that the obtained ECC has good tensile ductility and strength;
[0029] Figure 3This is the tensile stress-strain curve of the ultra-high toughness cement-based composite material obtained in Example 3 of the present invention, with an elongation at break exceeding 7% and a tensile strength exceeding 5.5 MPa; this figure shows that the obtained ECC has good tensile ductility and strength;
[0030] Figure 4 This is the tensile stress-strain curve of the ultra-high toughness cement-based composite material obtained in Example 4 of the present invention, with an elongation at break exceeding 5% and a tensile strength exceeding 5.5 MPa; the figure shows that the obtained ECC has good tensile ductility and strength;
[0031] From the test results of the samples of Examples 1-4 (i.e., the ultra-high toughness cement-based composite materials), it can be seen that the tensile stress-strain curve has typical yield and strengthening stages, the minimum elongation at break exceeds 4.3% and the maximum exceeds 7.29%. The sample photos show that the sample surface has multiple cracks, indicating that the ECC material prepared with basalt sand and basalt powder has extremely high ductility. DETAILED DESCRIPTION
[0032] The following embodiments are intended to further illustrate the present invention, but should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] A super-toughness cement-based composite material, the raw material components and weight percentages of the super-toughness cement-based composite material are: 1 part of cement, 2.1 parts of basalt powder, 2.5 parts of basalt sand, 0.001 parts of water reducer, 0.05 parts of fiber, and 1.2 parts of water; the specific amount of each component (the weight percentages are all kilograms) is shown in Table 1;
[0035] The preparation method of the ultra-high toughness cement-based composite material comprises the following steps:
[0036] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of cement 1 part, basalt powder 2.1 parts, basalt sand 2.5 parts, water reducer 0.001 parts, fiber 0.05 parts, water 1.2 parts; the specific amount of each component (the mass parts are all kilograms) is shown in Table 1;
[0037] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 40 seconds to make the dry materials preliminarily mixed and uniform;
[0038] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 70 seconds, then stir quickly for 45 seconds to make the material form a uniform slurry;
[0039] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 150 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 140 seconds. Then, stir quickly for 80 seconds. After stirring, the ultra-high toughness cement-based composite material is obtained.
[0040] The speed of the slow stirring is controlled at 65 r / min, and the speed of the fast stirring is controlled at 120 r / min.
[0041] The test data (tensile strength, elongation at break) of the ultra-high toughness cement-based composite material prepared in this embodiment are shown in Table 1.
[0042] Embodiment 2:
[0043] A super-toughness cement-based composite material, the raw material components and weight percentages of the super-toughness cement-based composite material are: 1 part of cement, 2.0 parts of basalt powder, 2.5 parts of basalt sand, 0.001 parts of water reducer, 0.05 parts of fiber, and 1.2 parts of water; the specific amount of each component (the weight percentages are all kilograms) is shown in Table 1;
[0044] The preparation method of the ultra-high toughness cement-based composite material comprises the following steps:
[0045] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of cement 1 part, basalt powder 2.0 parts, basalt sand 2.5 parts, water reducer 0.001 parts, fiber 0.05 parts, water 1.2 parts; the specific amount of each component (the mass parts are all kilograms) is shown in Table 1;
[0046] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 40 seconds to make the dry materials preliminarily mixed and uniform;
[0047] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 70 seconds, then stir quickly for 60 seconds to make the material form a uniform slurry;
[0048] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 130 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 130 seconds. Then, stir quickly for 110 seconds. After stirring, an ultra-high toughness cement-based composite material is obtained.
[0049] The speed of the slow stirring is controlled at 62 r / min, and the speed of the fast stirring is controlled at 120 r / min.
[0050] The test data (tensile strength, elongation at break) of the ultra-high toughness cement-based composite material prepared in this embodiment are shown in Table 1.
[0051] Embodiment 3:
[0052] A super-toughness cement-based composite material, the raw material components and weight percentages of the super-toughness cement-based composite material are: 1 part of cement, 2.5 parts of basalt powder, 2.5 parts of basalt sand, 0.003 parts of water reducer, 0.05 parts of fiber, and 1.2 parts of water; the specific amount of each component (the weight percentages are all kilograms) is shown in Table 1;
[0053] The preparation method of the ultra-high toughness cement-based composite material comprises the following steps:
[0054] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of cement 1 part, basalt powder 2.5 parts, basalt sand 2.5 parts, water reducer 0.003 parts, fiber 0.05 parts, water 1.2 parts; the specific amount of each component (the mass parts are all kilograms) is shown in Table 1;
[0055] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 40 seconds to make the dry materials preliminarily mixed and uniform;
[0056] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 70 seconds, then stir quickly for 45 seconds to make the material form a uniform slurry;
[0057] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 150 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 140 seconds. Then, stir quickly for 90 seconds. After stirring, an ultra-high toughness cement-based composite material is obtained.
[0058] The speed of the slow stirring is controlled at 65 r / min, and the speed of the fast stirring is controlled at 110 r / min.
[0059] The test data (tensile strength, elongation at break) of the ultra-high toughness cement-based composite material prepared in this embodiment are shown in Table 1.
[0060] Embodiment 4:
[0061] A super-toughness cement-based composite material, the raw material components and weight percentages of the super-toughness cement-based composite material are: 1 part of cement, 2.5 parts of basalt powder, 1.5 parts of basalt sand, 0.003 parts of water reducer, 0.05 parts of fiber, and 1.2 parts of water; the specific amount of each component (the weight percentages are all kilograms) is shown in Table 1;
[0062] The preparation method of the ultra-high toughness cement-based composite material comprises the following steps:
[0063] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of cement 1 part, basalt powder 2.5 parts, basalt sand 1.5 parts, water reducer 0.003 parts, fiber 0.05 parts, water 1.2 parts; the specific amount of each component (the mass parts are all kilograms) is shown in Table 1;
[0064] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 40 seconds to make the dry materials preliminarily mixed and uniform;
[0065] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 70 seconds, then stir quickly for 50 seconds to make the material form a uniform slurry;
[0066] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 150 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 140 seconds. Then, stir quickly for 90 seconds. After stirring, an ultra-high toughness cement-based composite material is obtained.
[0067] The speed of the slow stirring is controlled at 65 r / min, and the speed of the fast stirring is controlled at 110 r / min.
[0068] The test data (tensile strength, elongation at break) of the ultra-high toughness cement-based composite material prepared in this embodiment are shown in Table 1.
[0069] The specific dosage of each component in Examples 1-4 (the mass parts are all kilograms) and the test data of the obtained ultra-high toughness cement-based composite materials are shown in Table 1:
[0070] Table 1:
[0071]
[0072] In the above-mentioned embodiments 1-4:
[0073] The cement is ordinary Portland cement (cement strength grade is 42.5);
[0074] The basalt powder is obtained by crushing and grinding basalt ore, and has a specific surface area of 680m 2 / kg;
[0075] The fineness of the basalt sand is 40-70 mesh;
[0076] The water reducer is a polycarboxylate water reducer, and the product is produced and provided by Sichuan Tongzhou Chemical;
[0077] The fiber is a polyvinyl alcohol fiber, the polyvinyl alcohol fiber has a diameter of 35-45 μm, a tensile strength of ≥1600 MPa, an elongation at break of ≥6.5%, an elastic modulus of ≥41 GPa, and a fiber length of 8-12 mm;
[0078] The main chemical composition and mass percentage of the basalt are: SiO2 (silicon dioxide) 49.88%, Al2O3 (aluminum oxide) 15.08%, Fe2O3 (iron oxide) 12.07%, CaO (calcium oxide) 9.26%, MgO (magnesium oxide) 5.78%, K2O (potassium oxide) 1.08%, Na2O (sodium oxide) 3.67%, TiO2 (titanium dioxide) 2.3%, P2O5 (phosphorus pentoxide) 0.39%, MnO (manganese oxide) 0.15%, SO3 (sulfur trioxide) 0.08%, SrO (strontium oxide) 0.05%, Cr2O3 (chromium oxide) 0.21%, and the total of each component is 100%.
[0079] The testing method for the test data (tensile strength, elongation at break) of the above-mentioned Examples 1-4 is: the tensile strength and elongation at break of the sample (i.e., the ultra-high toughness cement-based composite material) are tested by a uniaxial tensile method, and the loading rate is 0.5 mm / min, with specific reference to JC / T 2461-2018.
[0080] Comparative Example 1:
[0081] ECC is prepared using raw materials such as cement, fly ash, quartz sand, PVA fiber (short for polyvinyl alcohol fiber), and water reducer. First, all solid components, including cement, quartz sand, and fly ash, are stirred and mixed for 3 minutes. Secondly, water and water reducer are added and stirred and mixed for another 5 minutes. When the mixture reaches a uniform state, PVA fiber is slowly added and stirred for another 10 minutes until the fibers are evenly distributed to obtain ECC. The sample (i.e., the prepared ECC) is demolded after being poured for 24 hours, and cured under sealed conditions at a relative humidity of 90±5% and a temperature of 20±2°C for 28 days for testing.
[0082] Comparative Example 2:
[0083] ECC is prepared using raw materials such as cement, fly ash, quartz sand, PVA fiber (short for polyvinyl alcohol fiber), and a water reducer. First, the cementitious material and quartz sand are stirred at a low speed in a mortar mixer for 2 minutes. Then, water of the water reducer is gradually added to the mortar, while stirring for another 2 minutes until a uniform slurry is obtained. Then, the mortar is stirred at a higher speed for 1 minute. Continue to stir the slurry slowly, and gradually spread the PVA fiber into the mixer by hand to ensure uniform distribution without agglomeration. After the stirring is completed, the ECC is obtained. The sample (i.e., the prepared ECC) is poured into the mold, demolded after 24 hours, and then cured for 28 days to test the performance.
[0084] The specific dosage of each component in Comparative Example 1-2 (the mass parts are all kilograms) and the test data of the obtained ultra-high toughness cement-based composite material (ie, the obtained ECC) are shown in Table 1:
[0085] Table 2:
[0086]
[0087] Embodiment 5:
[0088] A super-toughness cement-based composite material, the raw material components and weight percentages of the super-toughness cement-based composite material are: 1 part of cement, 2 parts of basalt powder, 0.5 parts of basalt sand, 0.001 parts of water reducer, 0.05 parts of fiber and 1 part of water.
[0089] Embodiment 6:
[0090] A super-toughness cement-based composite material, wherein the raw material components and weight percentages of the super-toughness cement-based composite material are as follows: 5 parts of cement, 6 parts of basalt powder, 4 parts of basalt sand, 0.01 parts of a water reducing agent, 0.07 parts of fiber, and 1.5 parts of water.
[0091] Embodiment 7:
[0092] A super-toughness cement-based composite material, wherein the raw material components and weight percentages of the super-toughness cement-based composite material are: 3 parts of cement, 4 parts of basalt powder, 2.2 parts of basalt sand, 0.005 parts of a water reducing agent, 0.06 parts of fiber, and 1.2 parts of water.
[0093] Embodiment 8:
[0094] A method for preparing an ultra-high toughness cement-based composite material, comprising the following steps:
[0095] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of 1 part of cement, 2 parts of basalt powder, 0.5 parts of basalt sand, 0.001 parts of water reducer, 0.05 parts of fiber and 1 part of water;
[0096] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 30 seconds to make the dry materials preliminarily mixed and evenly mixed;
[0097] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 60 seconds, then stir quickly for 30 seconds to make the material form a uniform slurry;
[0098] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 120 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 120 seconds. Then, stir quickly for 60 seconds. After stirring, an ultra-high toughness cement-based composite material is obtained.
[0099] The speed of the slow stirring is controlled at 60 r / min, and the speed of the fast stirring is controlled at 100 r / min.
[0100] Embodiment 9:
[0101] A method for preparing an ultra-high toughness cement-based composite material, comprising the following steps:
[0102] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of 5 parts of cement, 6 parts of basalt powder, 4 parts of basalt sand, 0.01 parts of water reducer, 0.07 parts of fiber and 1.5 parts of water;
[0103] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 50 seconds to make the dry materials preliminarily mixed and evenly mixed;
[0104] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 80 seconds, then stir quickly for 60 seconds to make the material form a uniform slurry;
[0105] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 180 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 160 seconds. Then, stir quickly for 120 seconds. After stirring, the ultra-high toughness cement-based composite material is obtained.
[0106] The speed of the slow stirring is controlled at 70 r / min, and the speed of the fast stirring is controlled at 120 r / min.
[0107] Embodiment 10:
[0108] A method for preparing an ultra-high toughness cement-based composite material, comprising the following steps:
[0109] a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of 3 parts of cement, 4 parts of basalt powder, 2.3 parts of basalt sand, 0.006 parts of water reducer, 0.06 parts of fiber and 1.3 parts of water;
[0110] b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 40 seconds to make the dry materials preliminarily mixed and uniform;
[0111] c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 70 seconds, then stir quickly for 50 seconds to make the material form a uniform slurry;
[0112] d. Add the fibers into the mixer twice. First, add about 2 / 3 of the fibers and stir slowly for 150 seconds. Then, slowly add the remaining 1 / 3 of the fibers and stir slowly for 140 seconds. Then, stir quickly for 90 seconds. After stirring, an ultra-high toughness cement-based composite material is obtained.
[0113] The speed of the slow stirring is controlled at 65 r / min, and the speed of the fast stirring is controlled at 110 r / min.
[0114] In the above-mentioned embodiments 5-10:
[0115] The cement can be silicate cement or ordinary silicate cement (cement strength grade is not less than 42.5), these two types of cement have high clinker content and stable mechanical properties;
[0116] The basalt powder is obtained by crushing and grinding basalt ore, and has a specific surface area of 600m 2 / kg~800m 2 / kg; when the specific surface area is too small (less than 600m 2 / kg), its reaction activity is low, which will seriously affect the mechanical properties of ECC; if the specific surface area is too large (greater than 800m 2 / kg), which will cause a surge in the amount of water required for ECC materials, affecting the construction performance of ECC; when the specific surface area is between 600m 2 / kg~800m 2 / kg, its reactivity is equivalent to that of fly ash, and it can be used as a good substitute for fly ash;
[0117] The fineness of the basalt sand is between 40 mesh and 100 mesh. If the sand is too coarse, the unevenness of the ECC will increase, and if it is too fine, the water demand will increase, and the shrinkage of the ECC will also increase.
[0118] The water reducer is a polycarboxylate water reducer, and the product production and supply enterprises include Sichuan Tongzhou Chemical, BASF of Germany, Sichuan Tongxingyuan and other companies, or other existing commercially available polycarboxylate water reducer product production and supply enterprises.
[0119] The fiber can be polyvinyl alcohol fiber or polyethylene fiber, both of which have sufficient toughness and elastic modulus;
[0120] The polyvinyl alcohol fiber has a diameter of 35-45 μm, a tensile strength of ≥1600 MPa, an elongation at break of ≥6.5%, an elastic modulus of ≥41 GPa, and a fiber length of 8-12 mm;
[0121] The polyethylene fiber has a diameter of 22-30 μm, a tensile strength of ≥3100 MPa, an elongation at break of ≥10%, an elastic modulus of ≥100 GPa, and a fiber length of 8-12 mm;
[0122] The main chemical composition and mass percentage of the basalt are: one of 45% to 52% SiO2 (silicon dioxide), one of 7% to 25% Al2O3 (aluminum oxide), and Fe2O3 (iron oxide), CaO (calcium oxide), MgO (magnesium oxide), K2O (potassium oxide), Na2O (sodium oxide), etc., and the sum of the components is 100%;
[0123] The main chemical composition and mass percentage of the basalt can be specifically: SiO2 (silicon dioxide) 49.88%, Al2O3 (aluminum oxide) 15.08%, Fe2O3 (iron oxide) 12.07%, CaO (calcium oxide) 9.26%, MgO (magnesium oxide) 5.78%, K2O (potassium oxide) 1.08%, Na2O (sodium oxide) 3.67%, TiO2 (titanium dioxide) 2.3%, P2O5 (phosphorus pentoxide) 0.39%, MnO (manganese oxide) 0.15%, SO3 (sulfur trioxide) 0.08%, SrO (strontium oxide) 0.05%, Cr2O3 (chromium oxide) 0.21%, and the sum of each component is 100%.
[0124] Alternatively, the main chemical composition and mass percentage of the basalt can be specifically: SiO2 (silicon dioxide) 47.88%, Al2O3 (aluminum oxide) 13.51%, Fe2O3 (iron oxide) 15.32%, CaO (calcium oxide) 10.26%, MgO (magnesium oxide) 4.71%, K2O (potassium oxide) 1.12%, Na2O (sodium oxide) 2.65%, TiO2 (titanium dioxide) 3.21%, P2O5 (phosphorus pentoxide) 0.41%, MnO (manganese oxide) 0.11%, SO3 (sulfur trioxide) 0.09%, SrO (strontium oxide) 0.02%, Cr2O3 (chromium oxide) 0.71%, and the sum of each component is 100%.
[0125] In the above embodiments: the percentages used, unless otherwise specified, are all mass (weight) percentages or percentages known to those skilled in the art; the proportions used, unless otherwise specified, are all mass (weight) proportions; and the weights may be in grams or kilograms.
[0126] In the above embodiments, the process parameters (time, rotation speed, etc.) in each step and the numerical values of the amount of each component are ranges, and any point can be applied.
[0127] The technical contents not specifically described in the present invention and the above embodiments are the same as the prior art, and the raw materials are all commercially available products.
[0128] The present invention is not limited to the above embodiments, and all of the contents of the present invention can be implemented and have the above good effects.
Claims
1. An ultra-high toughness cement-based composite material, characterized by: The raw material components and weight percentages of the ultra-high toughness cement-based composite material are as follows: 1 to 5 parts of cement, 2 to 6 parts of basalt powder, 0.5 to 4 parts of basalt sand, 0.001 to 0.01 parts of water reducing agent, 0.05 to 0.07 parts of fiber, and 1 to 1.5 parts of water.
2. The ultra-high toughness cement-based composite material according to claim 1, characterized in that: The cement is silicate cement or ordinary silicate cement.
3. The ultra-high toughness cement-based composite material according to claim 1, characterized in that: The basalt powder is obtained by crushing and grinding basalt ore, and has a specific surface area of 600m 2 / kg~800m 2 / kg; The fineness of the basalt sand is 40-100 meshes.
4. The ultra-high toughness cement-based composite material according to claim 3, characterized in that: The main chemical composition and mass percentage of the basalt are: SiO2 45% to 52%, Al2O3 7 to 25%, and Fe2O3, CaO, MgO, K2O, Na2O, and the total of each component is 100%.
5. The ultra-high toughness cement-based composite material according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.
6. The ultra-high toughness cement-based composite material according to claim 1, characterized in that: The fibers are polyvinyl alcohol fibers or polyethylene fibers.
7. The ultra-high toughness cement-based composite material according to claim 6, characterized in that: The polyvinyl alcohol fiber has a diameter of 35-45 μm, a tensile strength of ≥1600 MPa, an elongation at break of ≥6.5%, an elastic modulus of ≥41 GPa, and a fiber length of 8-12 mm; The polyethylene fiber has a diameter of 22-30 μm, a tensile strength of ≥3100 MPa, an elongation at break of ≥10%, an elastic modulus of ≥100 GPa, and a fiber length of 8-12 mm.
8. The ultra-high toughness cement-based composite material according to claim 4, characterized in that: The main chemical composition and mass percentage of the basalt are: SiO2 49.88%, Al2O3 15.08%, Fe2O3 12.07%, CaO 9.26%, MgO 5.78%, K2O 1.08%, Na2O 3.67%, TiO2 2.3%, P2O5 0.39%, MnO 0.15%, SO3 0.08%, SrO 0.05%, Cr2O3 0.21%; Alternatively, the main chemical composition and mass percentage of the basalt are: SiO2 47.88%, Al2O3 13.51%, Fe2O3 15.32%, CaO 10.26%, MgO 4.71%, K2O 1.12%, Na2O 2.65%, TiO2 3.21%, P2O5 0.41%, MnO 0.11%, SO3 0.09%, SrO 0.02%, Cr2O3 0.71%.
9. A method for preparing an ultra-high toughness cement-based composite material, The method is characterized in that the steps are: a. Ingredients: Take the raw materials of each component according to the raw material components and mass parts of cement 1-5 parts, basalt powder 2-6 parts, basalt sand 0.5-4 parts, water reducer 0.001-0.01 parts, fiber 0.05-0.07 parts, water 1-1.5 parts; b. Place cement, basalt powder and basalt sand in a mixer and stir slowly for 30s to 50s; c. Add the water reducer into water to dissolve it, add the solution into the mixer, stir slowly for 60s to 80s, then stir quickly for 30s to 60s to make the material into a uniform slurry; d. Add the fiber into the mixer twice. First, add 2 / 3 of the fiber and stir slowly for 120s to 180s. Then, slowly add the remaining 1 / 3 of the fiber and stir slowly for 120s to 160s. Then, stir quickly for 60s to 120s to obtain an ultra-high toughness cement-based composite material.
10. The method for preparing the ultra-high toughness cement-based composite material according to claim 9, characterized in that: The speed of the slow stirring is controlled at 60-70 r / min, and the speed of the fast stirring is controlled at 100-120 r / min.
Citation Information
Patent Citations
High-compactness and ultrahigh-strength cement-based composite material for financial equipment in bank
CN103922650A
Multifunctional environment-friendly mortar modified by optimizing basalt admixture system and preparation method of multifunctional environment-friendly mortar
CN113045264A
Preparation method of basalt sand and cement-based material
CN115818995A
High-strength basalt stone powder concrete material and preparation method thereof
CN117623678A
Ultra-high strength steel fibre reinforced concrete
WO2014094692A1