Ultra-high performance additive manufacturing dry powder, preparation method, printed base material and method

By using materials such as nano-scale silica gel and micron-scale inert fillers in 3D printing, combined with specific ratios and processing methods, high-strength, high-durability additive manufacturing dry powder materials are formed, which solves the problem of insufficient strength of traditional cement-based materials. problem, improve the artistic design and durability of components, and reduce carbon emissions.

CN118754574AActive Publication Date: 2024-10-11CHINA CONSTR EIGHT ENG DIV CORP LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410758295.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The strength of traditional 3D printing cement-based materials is insufficient, which limits the innovation of special-shaped structures and the artistry of components. It also has insufficient durability and service life of building structures.

Method used

Nano-scale silica gel and micron-scale inert fillers are used for mixing, combined with PO425 cement, CSA cement, superplasticizer and hydroxypropyl methylcellulose, to form ultra-high performance additive manufacturing dry powder through drying and mixing. The maximum packing density theory adjusts the rheological properties and setting time to form a high-strength and highly durable 3D printing substrate.

Benefits of technology

It significantly improves the strength and durability of 3D printed components, reduces the bulkiness of parts, extends their service life, and reduces carbon emissions throughout the life cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754574A_ABST
    Figure CN118754574A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of ultra-high-performance dry powder for additive manufacturing, which comprises the following steps: providing nano-scale silica gel and micron-scale inert filler, and uniformly mixing to form a first batch of premix; the first batch of premix is dried; a second batch of premix is added into the dried first batch of premix and evenly mixed, the additive manufacturing dry powder with printability in both rheological characteristics and setting time is obtained, and the second batch of premix comprises PO425 cement, CSA cement, a super plasticizer and hydroxypropyl methyl cellulose. The problem that a traditional 3D printing cement-based material is insufficient in strength is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of 3D printing technology, and in particular to an ultra-high performance additive manufacturing dry powder material and a preparation method, a printing substrate and a method. Background Art

[0002] 3D printing (3DP) is a type of rapid prototyping technology, also known as additive manufacturing. It is a technology that uses 3D model files as the basis, and uses powdered metal, plastic or concrete and other bondable materials to construct objects by printing layer by layer. Its main features are rapid prototyping, reduced material waste, template-free, high degree of design freedom, and can significantly reduce carbon emissions. It is an innovative, environmentally friendly, and efficient new component manufacturing method. Among the many 3D printing materials, cement-based materials have become the mainstream material for 3D printing substrates due to their wide range of raw materials, low prices, and stable physical properties of finished products. And with the development of 3D printing technology, the demand for refinement, high strength, and high durability of 3D printed building components is becoming increasingly significant.

[0003] The most unique advantage of cement-based materials is that they can print special-shaped structures with rich designs. However, due to the low strength of cement-based materials, the degree of innovation of special-shaped structures printed with them is limited, because low-strength printing materials will force the design cross-sectional area to increase on the mechanical design side, and ultimately the components are bulky and heavy in appearance, which seriously reduces the artistic quality of the components. For example, if the strength of 3D printed art words using cement-based materials as printing ink can be doubled, the minimum number of printing layers can be reduced by half, and the structure will be lighter and more beautiful. Moreover, for 3D printed building structures, they are often used in outdoor architectural sketches, retaining walls, flower beds and other open-air structures. Therefore, the quality requirements for printed parts during service are high. If the strength of the printing material is not enough, the durability is poor and the service life is short. Summary of the invention

[0004] In order to solve the above problems, the present invention provides an ultra-high performance additive manufacturing dry powder material and preparation method, a printing substrate and method, which solves the problem of insufficient strength of traditional 3D printing cement-based materials.

[0005] The present invention is implemented by the following scheme: a method for preparing ultra-high performance additive manufacturing dry powder, comprising the steps of:

[0006] Providing nano-sized silica gel and micro-sized inert filler and mixing them evenly to form a first batch of premix;

[0007] Drying the first batch of premixes;

[0008] A second batch of premix is ​​added to the dried first batch of premix and mixed evenly to obtain an additive manufacturing dry powder material with printable rheological properties and setting time, wherein the second batch of premix includes PO425 cement, CSA cement, superplasticizer and hydroxypropyl methylcellulose.

[0009] A further improvement of the method for preparing ultra-high performance additive manufacturing dry powder of the present invention is that the micron-sized inert filler includes primary fly ash and S95 silica ash.

[0010] A further improvement of the method for preparing ultra-high performance additive manufacturing dry powder of the present invention is that the nano-scale silica gel in the first batch of premixes is 0.01 to 0.03 parts by weight, the primary fly ash is 0.15 to 0.2 parts by weight, and the S95 silica ash is 0.2 to 0.4 parts by weight, wherein the weight of the nano-scale silica gel is the weight minus its own water content.

[0011] A further improvement of the method for preparing ultra-high performance additive manufacturing dry powder of the present invention is that the PO425 cement in the second batch of premix is ​​1 part by weight, the CSA cement is 0.02-0.05 parts by weight, the superplasticizer is 0.01-0.03 parts by weight, and the hydroxypropyl methylcellulose is 0.001-0.005 parts by weight.

[0012] A further improvement of the method for preparing ultra-high performance additive manufacturing dry powder of the present invention is that the concentration of the nano-silica gel in the first batch of premixes does not exceed 40%.

[0013] A further improvement of the method for preparing ultra-high performance additive manufacturing dry powder of the present invention is that when the first batch of premixes are dried, stirring is maintained and the premixes are dried at 100-110° C. to constant weight so that all the water in the nano-scale silica gel is lost.

[0014] The present invention further provides an ultra-high performance additive manufacturing dry powder material, which is prepared using the method for preparing the ultra-high performance additive manufacturing dry powder material as described in any of the above items.

[0015] The present invention further provides a 3D printing substrate, which is formed by mixing the ultra-high performance additive manufacturing dry powder as described above with 0.25 to 0.3 parts by weight of water.

[0016] The present invention further provides a 3D printing method, comprising the steps of:

[0017] Before printing, a 3D printing substrate as described above is preformed;

[0018] During printing, the 3D printing substrate is pumped to the 3D printing device using a pump tube.

[0019] The present invention further provides a 3D printing method, comprising the steps of:

[0020] A dual-head 3D printing device is provided, wherein the dual-head 3D printing device is provided with a proportional dry powder spray head and a water vapor spray head;

[0021] During printing, the ultra-high performance additive manufacturing dry powder and water as described above are provided to the dry powder nozzle and the water vapor nozzle respectively, so as to form the 3D printing substrate as described above by synchronous composite feeding during the printing process.

[0022] The present invention uses micron-level inert materials and nano-level silica sol as the main materials for 3D printing substrates, uses the maximum packing density theory, and is supplemented with enhanced auxiliary materials used to change its rheological properties and setting time to make it printable, and finally obtains high-strength and high-durability additive manufacturing dry powder. The problem of insufficient strength of traditional cement-based materials is solved. The parts printed by the present invention have a dense structure and high durability, which not only has a long service life, but also can reduce its carbon emissions throughout its life cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The flowchart of the preparation method of the dry powder material of the present invention is shown. DETAILED DESCRIPTION

[0024] In order to solve the problem of insufficient strength of traditional 3D printing cement-based materials, the present invention provides an ultra-high performance additive manufacturing dry powder material and preparation method, a printed substrate and method. The ultra-high performance additive manufacturing dry powder material and preparation method, a printed substrate and method are further described below with specific embodiments and drawings.

[0025] See also Figure 1 As shown, a method for preparing ultra-high performance additive manufacturing dry powder comprises the following steps:

[0026] Step 1: Provide nano-sized silica gel and micro-sized inert filler and mix them evenly to form the first batch of premix.

[0027] Step 2: Drying the first batch of premixes.

[0028] Step 3: Add the second batch of premixes to the dried first batch of premixes and mix them evenly to obtain an additive manufacturing dry powder material with printable rheological properties and setting time. The second batch of premixes includes PO425 cement, CSA cement, superplasticizer and hydroxypropyl methylcellulose.

[0029] This method uses micron-level inert materials and nano-level silica sol as the main materials for 3D printing substrates, uses the maximum packing density theory, and is supplemented by enhanced auxiliary materials used to change its rheological properties and setting time to make it printable, and finally obtains high-strength and high-durability additive manufacturing dry powder. The above-mentioned maximum packing density theory (densified particle packing) refers to the fact that particles of different particle sizes of the constituent materials of the cementitious material form the most dense stacking in the best proportion, that is, the gaps between the accumulation of millimeter-level particles (aggregates) are filled with micron-level particles (cement, fly ash, mineral powder), and the gaps between the accumulation of micron-level particles are filled with submicron-level particles (silica ash) or even nano-level particles (nano SiO2). Through the above means, the problem of insufficient strength of traditional cement-based materials is solved. The dry powder prepared by this method is used as a 3D printing material, so that the printed parts have a dense structure and high durability, which not only has a long service life, but also can reduce its carbon emissions throughout its life cycle.

[0030] A preferred embodiment is provided below. Referring to the data in Table 1, in this embodiment, dry powder is formed in two batches: the first batch is to mix 0.01-0.03 parts by weight of nano-scale silica gel (SiO2) and micron-scale inert filler (including 0.15-0.2 parts by weight of primary fly ash and 0.2-0.4 parts by weight of S95 silica ash, and other micron-scale inert fillers can also be used according to actual needs) to form the first batch of premix. It should be noted that the nano-scale silica gel is mixed in the form of a hydrosol, and the concentration is controlled to be no more than 40% to ensure its dispersion effect. The above weight is the weight after deducting its own water content.

[0031]

[0032] The second batch is to add enhanced auxiliary materials that can adjust the rheological properties and setting time to the first batch of premixes so that both have printability, that is, the second batch of premixes. In this embodiment, the second batch of premixes includes 1 part by weight of PO425 cement, 0.02-0.05 parts by weight of CSA cement, 0.01-0.03 parts by weight of superplasticizer and 0.001-0.005 parts by weight of hydroxypropyl methylcellulose. The setting time can be adjusted by the different addition amounts of CSA cement, and the rheological properties can be adjusted by the addition and ratio relationship of all components of the second batch of premixes.

[0033] It should be noted that in order to obtain a dry and uniform powder that can be stored for a long time, it is necessary to remove the moisture in the dry powder. Therefore, in this embodiment, before the second batch operation, the first batch of premixes is dried, and stirring is maintained during drying, and dried at 100-110°C to constant weight, so that all the moisture in the nano-silica gel is lost. The components in the second batch of premixes added are all dry and do not contain moisture.

[0034] A 3D printing substrate is prepared by mixing the ultra-high performance additive manufacturing dry powder prepared by the preparation method described above with 0.25 to 0.3 parts by weight of water.

[0035] The 3D printing substrate can be used for 3D printing of fine architectural art components, with a printing layer height (vertical resolution) of less than 1 cm and a minimum of 0.1 cm. There are two ways to use the 3D printing substrate:

[0036] A 3D printing method comprises the following steps: before printing, pre-forming the 3D printing substrate as described above; during printing, pumping the 3D printing substrate to a 3D printing device using a pump tube.

[0037] Another 3D printing method includes the steps of: providing a dual-head 3D printing device, the dual-head 3D printing device is provided with a proportional dry powder nozzle and a water vapor nozzle; during printing, providing the ultra-high performance additive manufacturing dry powder and water as described above to the dry powder nozzle and the water vapor nozzle respectively, so as to form the 3D printing substrate as described above by synchronous composite feeding during the printing process.

[0038] The ultra-high performance additive manufacturing dry powder of the present invention can reach C80 in 28 days, greatly improving the strength of 3D printed components, thereby saving materials and improving the degree of innovation in the artistic design of components. It can be used by adding water, and is simple and quick to use. Ordinary 3D printed building materials have coarse layered textures. The ultra-high performance additive manufacturing dry powder of the present invention does not contain coarse particles, and the printing performance is stable, so the printing resolution is high (1mm-10mm), which is suitable for 3D printing of fine cement-based materials. The internal structure of the prepared 3D printed components is dense, and the corrosion resistance and freeze-thaw resistance are greatly improved.

[0039] The present invention is described in detail above in conjunction with the embodiments of the accompanying drawings. A person skilled in the art can make various variations of the present invention according to the above description. Therefore, certain details in the embodiments should not be construed as limiting the present invention, and the scope of protection of the present invention shall be the scope defined by the attached claims.

Claims

1. A method for preparing ultra-high performance additive manufacturing dry powder, It is characterized in that Includes steps: Providing nano-sized silica gel and micro-sized inert filler and mixing them evenly to form a first batch of premix; Drying the first batch of premixes; A second batch of premix is ​​added to the dried first batch of premix and mixed evenly to obtain an additive manufacturing dry powder material with printable rheological properties and setting time, wherein the second batch of premix includes PO425 cement, CSA cement, superplasticizer and hydroxypropyl methylcellulose.

2. The method for preparing the ultra-high performance additive manufacturing dry powder according to claim 1, It is characterized in that The micron-sized inert filler includes primary fly ash and S95 silica ash.

3. The method for preparing the ultra-high performance additive manufacturing dry powder according to claim 2, It is characterized in that The first batch of premixes contains 0.01-0.03 parts by weight of the nano-silica gel, 0.15-0.2 parts by weight of the primary fly ash, and 0.2-0.4 parts by weight of the S95 silica ash, wherein the weight of the nano-silica gel is the weight after deducting its own water content.

4. The method for preparing the ultra-high performance additive manufacturing dry powder according to claim 3, It is characterized in that The second batch of premix contains 1 part by weight of the PO425 cement, 0.02-0.05 part by weight of the CSA cement, 0.01-0.03 part by weight of the superplasticizer, and 0.001-0.005 part by weight of the hydroxypropyl methylcellulose.

5. The method for preparing the ultra-high performance additive manufacturing dry powder according to claim 1, It is characterized in that The concentration of the nano-silica gel in the first batch of premixes does not exceed 40%.

6. The method for preparing the ultra-high performance additive manufacturing dry powder according to claim 1, It is characterized in that When the first batch of premix is ​​dried, stirring is maintained and the premix is ​​dried at 100-110° C. to a constant weight so that all the water in the nano-scale silica gel is lost.

7. An ultra-high performance dry powder for additive manufacturing, It is characterized in that The ultra-high performance additive manufacturing dry powder is prepared using the method for preparing the ultra-high performance additive manufacturing dry powder as described in any one of claims 1 to 6.

8. A 3D printing substrate, It is characterized in that The ultra-high performance additive manufacturing dry powder as claimed in claim 7 is mixed with 0.25 to 0.3 parts by weight of water.

9. A 3D printing method, It is characterized in that Includes steps: Before printing, pre-forming the 3D printing substrate as claimed in claim 8; During printing, the 3D printing substrate is pumped to the 3D printing device using a pump tube.

10. A 3D printing method, It is characterized in that Includes steps: A dual-head 3D printing device is provided, wherein the dual-head 3D printing device is provided with a proportional dry powder spray head and a water vapor spray head; During printing, the ultra-high performance additive manufacturing dry powder and water as described in claim 7 are provided to the dry powder nozzle and the water vapor nozzle respectively, so as to form the 3D printing substrate as described in claim 8 by synchronous composite feeding during the printing process.

Citation Information

Patent Citations

  • Non-cement-based cementitious material for 3D printing and preparation method of non-cement-based cementitious material

    CN106045435A

  • Thixotropic agent suitable for 3D printed sulphoaluminate cement-based material

    CN109455973A

  • Fiber reinforced cement-based material for 3D printing, preparation, performance evaluation and application

    CN109942262A

  • 3D printing concrete with adjustable rheological property, preparation method and printing process

    CN114804791A

  • A method for preparing high-early-strength fiber reinforced cement composites and high-early-strength fiber reinforced cement composites preparing from the method

    KR1020080013350A