Environment-friendly and wear-resistant ceramic tile and preparation method thereof
Through the double-layer glaze structure and pre-firing process, the problems of wear resistance and thermal shock resistance of ceramic tiles are solved, high-quality preparation of ceramic tiles is achieved, and their stability and safety during use are ensured.
Patent Information
- Application Number
- CN202410921427.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing glazed ceramic tiles have poor wear resistance, and can easily lead to strength reduction and brittle fracture when subjected to drastic changes in temperature, affecting their durability and safety.
Adopting a double-layer glaze structure and pre-firing process, by adding silicon carbide and aluminum nitride to the top glaze, and adding sodium silicate and aluminum phosphate to the base glaze, the wear resistance and bonding strength of the glaze are improved. Firing reduces residual stress in the body and glaze, preventing cracks and deformation.
It achieves good wear resistance and thermal shock resistance of ceramic tiles, ensures good combination of glaze layer and matrix, improves product stability and yield, and meets environmental protection requirements.
Smart Images

Figure CN118754601A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to an environmentally friendly, wear-resistant ceramic tile and a preparation method thereof. Background Art
[0002] Ceramic tiles are mainly made of clay, quartz, feldspar and other mineral raw materials. With the development of ceramic production technology and related industrial technologies, a wide range of products with different patterns and colors have been gradually introduced. The products are involved in covering and decorating the floor and walls of buildings. In recent years, they have also entered the fields of furniture panels and kitchen cabinet facings as panels, and have become one of the most widely used and popular building decoration materials.
[0003] Glazed ceramic tiles are a type of ceramic tile that is made by applying glaze on the surface of the ceramic tile and then firing it at high temperature. The glaze can provide ceramic tiles with a variety of colors and patterns, and the surface is smooth and easy to clean. It is often used for wall and floor decoration.
[0004] However, most of the existing glazed ceramic tiles have poor wear resistance. Scratches and wear on the glaze layer not only affect the appearance, but also affect its service life. In addition, ceramic tiles are brittle materials. When subjected to sudden temperature changes (thermal shock), they are prone to a significant decrease in strength or even brittle fracture, which seriously affects the durability and safety of ceramic tiles. Therefore, thermal shock resistance is one of the most important basic properties of ceramic tiles.
[0005] Therefore, how to improve the wear resistance of glazed ceramic tiles while ensuring their good thermal shock resistance is of great significance to improving the quality of ceramic tile products. Summary of the invention
[0006] To solve the above problems, the present invention provides an environmentally friendly, wear-resistant ceramic tile and a preparation method thereof. The method improves the wear resistance while ensuring the thermal shock resistance by adjusting the glaze composition and using specific processes such as double-layer glaze and pre-firing, thereby realizing the preparation of high-quality glazed ceramic tiles.
[0007] The method for preparing the environmentally friendly and wear-resistant ceramic tile of the present invention comprises the following steps:
[0008] S1, compression molding the green body raw material to obtain a green body;
[0009] S2, wet-milling the base glaze raw material and sieving it to obtain base glaze slurry, and then applying the base glaze slurry to the green body for pre-firing;
[0010] S3, wet-milling the glaze raw materials and sieving them to obtain glaze slurry, then applying the glaze slurry to the green body for sintering, and cooling to obtain the finished ceramic tile.
[0011] Further, the green body comprises the following raw materials by weight: 20-25 parts of kaolin, 15-20 parts of clay, 10-15 parts of aluminum sand, 2-5 parts of wollastonite, and 2-5 parts of talc. Preferably, the green body comprises the following raw materials by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc.
[0012] Further, the base glaze comprises the following raw materials by weight: 30-35 parts of potassium feldspar, 5-15 parts of kaolin, 5-15 parts of talc, 5-8 parts of quartz, 15-20 parts of dolomite, 2-5 parts of barium carbonate, 5-20 parts of sodium silicate, and 5-8 parts of aluminum phosphate. Preferably, the base glaze comprises the following raw materials by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 12 parts of sodium silicate, and 6 parts of aluminum phosphate.
[0013] Furthermore, the weight ratio of sodium silicate to aluminum phosphate in the base glaze is (1-2): 1. Preferably, the weight ratio of sodium silicate to aluminum phosphate in the base glaze is 2:1.
[0014] Furthermore, in the wet ball milling process of the glaze raw materials, the material: ball: water = 1:3:1, the ball milling time is 3 to 5 hours, and after ball milling, the raw materials are sieved through a 200-mesh screen.
[0015] Furthermore, the base glaze application amount is 350-450 g / m 2 Preferably, the base glaze application amount is 350g / m 2 .
[0016] Furthermore, the pre-firing temperature is 600°C to 900°C, and the pre-firing time is 1 to 5 hours. Preferably, the pre-firing temperature is 900°C, and the pre-firing time is 2 hours.
[0017] Further, the glaze comprises the following raw materials by weight: 12-15 parts of albite, 10-15 parts of quartz sand, 15-25 parts of calcined kaolin, 5-10 parts of calcined alumina, 8-10 parts of kaolin, 2-5 parts of barium carbonate, 2-5 parts of silicon carbide, and 2-5 parts of aluminum nitride. Preferably, the glaze comprises the following raw materials by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0018] Furthermore, in the wet ball milling process of the glaze raw materials, the material: ball: water = 1:3:1, the ball milling time is 3 to 5 hours, and after ball milling, the raw materials are sieved through a 200-mesh screen.
[0019] Furthermore, the glaze application amount of the top glaze is 350-550 g / m 2 Preferably, the glaze application amount is 450g / m2 .
[0020] Furthermore, the sintering temperature is 1220°C to 1250°C, and the sintering time is 1 to 3 hours. Preferably, the sintering temperature is 1230°C, and the sintering time is 2 hours.
[0021] The present invention also provides a ceramic tile product prepared according to the above method.
[0022] Another object of the present invention is to provide the application of the ceramic tile in building decoration and finishing materials, including floor paving and decoration, wall paving and decoration, preparation of furniture panels and decoration, paving and decoration of building exterior walls, paving and decoration of swimming pools, bathrooms and kitchens, paving and decoration of commercial and public places, etc.
[0023] Compared with the prior art, the beneficial technical effects of the present invention are:
[0024] (1) The ceramic tile of the present invention has good wear resistance, and the glaze layer has good bonding with the substrate and is not easy to fall off;
[0025] (2) The ceramic tile of the present invention has good mechanical properties, is not easy to crack during processing, and has a high yield;
[0026] (3) The ceramic tiles of the present invention have no adverse effects on human health and the environment during the preparation process, and are in line with the industry development concept of green environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The present invention will be further described below in conjunction with the accompanying drawings.
[0028] Figure 1 The present invention is a flow chart of the preparation process of the ceramic tile. DETAILED DESCRIPTION
[0029] The present invention provides an environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, comprising the following steps:
[0030] S1, compression molding the green body raw material to obtain a green body;
[0031] S2, wet-milling the base glaze raw material and sieving it to obtain base glaze slurry, and then applying the base glaze slurry to the green body for pre-firing;
[0032] S3, wet-milling the glaze raw materials and sieving them to obtain glaze slurry, then applying the glaze slurry to the green body for sintering, and cooling to obtain the finished ceramic tile.
[0033] In one embodiment, the green body comprises the following raw materials by weight: 20-25 parts of kaolin, 15-20 parts of clay, 10-15 parts of aluminum sand, 2-5 parts of wollastonite, and 2-5 parts of talc.
[0034] In one embodiment, the green body comprises the following raw materials by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc.
[0035] In principle, the present invention does not strictly limit the raw material composition and ratio of the green body. The ceramic tile green bodies in the prior art can be used to prepare the environmentally friendly and wear-resistant ceramic tiles of the present invention.
[0036] In one embodiment, the base glaze includes the following raw materials by weight: 30-35 parts of potassium feldspar, 5-15 parts of kaolin, 5-15 parts of talc, 5-8 parts of quartz, 15-20 parts of dolomite, 2-5 parts of barium carbonate, 5-20 parts of sodium silicate, and 5-8 parts of aluminum phosphate.
[0037] In one embodiment, the base glaze includes the following raw materials by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 12 parts of sodium silicate, and 6 parts of aluminum phosphate.
[0038] In one embodiment, the weight ratio of sodium silicate to aluminum phosphate in the base glaze is (1-2):1.
[0039] In one embodiment, the weight ratio of sodium silicate to aluminum phosphate in the base glaze is 2:1.
[0040] In one embodiment, in the wet ball milling process of the glaze raw material, the ratio of material: ball: water is 1:3:1, the ball milling time is 3 to 5 hours, and the raw material is sieved through a 200-mesh sieve after ball milling.
[0041] In one embodiment, the base glaze application amount is 350-450 g / m 2 .
[0042] In one embodiment, the base glaze application amount is 350g / m 2 .
[0043] In one embodiment, the pre-firing temperature is 600° C. to 900° C., and the pre-firing time is 1 to 5 hours. In one embodiment, the pre-firing temperature is 900° C., and the pre-firing time is 2 hours.
[0044] In one embodiment, the glaze comprises the following raw materials by weight: 12 to 15 parts of albite, 10 to 15 parts of quartz sand, 15 to 25 parts of calcined kaolin, 5 to 10 parts of calcined alumina, 8 to 10 parts of kaolin, 2 to 5 parts of barium carbonate, 2 to 5 parts of silicon carbide, and 2 to 5 parts of aluminum nitride.
[0045] In one embodiment, the glaze comprises the following raw materials by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0046] In one embodiment, in the wet ball milling process of the glaze raw material, the ratio of material: ball: water is 1:3:1, the ball milling time is 3 to 5 hours, and the raw material is sieved through a 200-mesh sieve after ball milling.
[0047] In one embodiment, the glaze application amount is 350-550 g / m 2 .
[0048] In one embodiment, the glaze application amount is 450g / m 2 .
[0049] In one embodiment, the sintering temperature is 1220° C. to 1250° C., and the sintering time is 1 to 3 hours.
[0050] In one embodiment, the sintering temperature is 1230° C. and the sintering time is 2 hours.
[0051] The present invention significantly improves the wear resistance of the glaze by adding a certain amount of silicon carbide and aluminum nitride to the glaze material. However, it is found in actual research that after adding silicon carbide and aluminum nitride, the expansion coefficient difference between the body and the glaze is too large, and stress is generated between the body and the glaze layer, resulting in interface cracking or glaze peeling between the glaze layer and the porcelain body. At the same time, during the long-term use of ceramic tiles, temperature changes (especially frequent temperature changes) cause repeated stress, causing micro-structural deformation between the ceramic tiles and the glaze layer, and there is a risk of cracks and overall damage to the ceramic tiles, shortening their service life.
[0052] To overcome this problem, the present invention adopts a double-layer glaze structure of a base glaze and a top glaze, and overcomes the problem of a large difference in expansion coefficients between the body and the top glaze by means of the buffering effect of the base glaze. At the same time, the present invention adds a certain amount of sodium silicate and aluminum phosphate to the base glaze, thereby improving the bonding strength between the base glaze and the body and the top glaze, and preventing the top glaze from falling off. In addition, the present invention also adopts a pre-firing process to reduce the residual stress in the body and the glaze, prevent cracks and deformation in the subsequent sintering process, improve the stability of the product, and thus improve the yield rate.
[0053] The present invention also provides a ceramic tile product prepared according to the above method.
[0054] The ceramic bricks of the present invention are used as building decoration materials, specifically including: ground paving and decoration, wall paving and decoration, preparation of furniture panels and decoration, paving and decoration of building exterior walls, paving and decoration of swimming pools, bathrooms and kitchens, paving and decoration of commercial and public places, etc.
[0055] The technical solution provided by the present invention is further described below in conjunction with embodiments.
[0056] Example 1
[0057] An environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, the steps are as follows:
[0058] S1, compression molding the green body raw material to obtain a green body;
[0059] The green body is composed of the following raw materials in parts by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc;
[0060] S2. Wet-mill the base glaze raw materials for 3 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain base glaze slurry, and then apply the base glaze slurry to the body, and the glaze amount is 350g / m 2 , pre-sintered at 900℃ for 2h;
[0061] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 12 parts of sodium silicate, and 6 parts of aluminum phosphate;
[0062] S3. Wet-mill the surface glaze raw materials for 5 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain the surface glaze slurry. Then apply the bottom glaze slurry to the body, and the glaze amount is 450g / m 2 , sintered at 1230℃ for 2h, and the finished ceramic tile was obtained after cooling;
[0063] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0064] Example 2
[0065] Same as Example 1, except that:
[0066] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 15 parts of kaolin, 15 parts of talc, 8 parts of quartz, 20 parts of dolomite, 5 parts of barium carbonate, 20 parts of sodium silicate, and 8 parts of aluminum phosphate;
[0067] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 25 parts of calcined kaolin, 10 parts of calcined alumina, 10 parts of kaolin, 5 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0068] Example 3
[0069] Same as Example 1, except that:
[0070] The base glaze is composed of the following raw materials in parts by weight: 30 parts of potassium feldspar, 5 parts of kaolin, 5 parts of talc, 5 parts of quartz, 15 parts of dolomite, 2 parts of barium carbonate, 5 parts of sodium silicate, and 5 parts of aluminum phosphate.
[0071] The glaze is composed of the following raw materials in parts by weight: 12 parts of albite, 10 parts of quartz sand, 15 parts of calcined kaolin, 5 parts of calcined alumina, 8 parts of kaolin, 2 parts of barium carbonate, 2 parts of silicon carbide, and 2 parts of aluminum nitride.
[0072] Comparative Example 1
[0073] Same as Example 1, except that the base glaze does not contain sodium silicate and aluminum phosphate.
[0074] Comparative Example 2
[0075] Same as Example 1, except that the weight ratio of sodium silicate to aluminum phosphate in the base glaze is 0.5:1.
[0076] Comparative Example 3
[0077] Same as Example 1, except that only the top glaze is used, and no bottom glaze is used.
[0078] Comparative Example 4
[0079] Same as Example 1, except that the pre-firing temperature is 550°C.
[0080] Comparative Example 5
[0081] Same as Example 1, except that the glaze does not include silicon carbide and aluminum nitride.
[0082] The performance of ceramic tiles was tested according to GB / T3810.7-2016 and GB / T3810.9-2016, and the results are as follows:
[0083] Wear resistance (12000 rpm) Thermal shock resistance Example 1 Level 4 More than 70 times without cracks Example 2 Level 4 More than 70 times without cracks Example 3 Level 4 More than 70 times without cracks Comparative Example 1 Level 4 More than 30 times cracks appear Comparative Example 2 Level 4 The boundary blending is not good, and cracks appear after more than 40 times Comparative Example 3 Level 4 More than 20 cracks Comparative Example 4 Level 4 More than 20 cracks Comparative Example 5 Level 2 More than 70 times without cracks
[0084] Example 4
[0085] An environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, the steps are as follows:
[0086] S1, compression molding the green body raw material to obtain a green body;
[0087] The green body is composed of the following raw materials in parts by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc;
[0088] S2. Wet-mill the base glaze raw materials for 3 hours under the condition of material: ball: water = 1:3:1, and then pass through a 200-mesh sieve to obtain base glaze slurry, and then apply the base glaze slurry to the blank, with a glaze amount of 350g / m 2 , pre-sintered at 600℃ for 3.5h;
[0089] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 12 parts of sodium silicate, and 6 parts of aluminum phosphate;
[0090] S3, wet-milling the surface glaze raw materials under the condition of material: ball: water = 1:3:1 for 5 hours, and then sifting through a 200-mesh sieve to obtain a surface glaze slurry, and then applying the bottom glaze slurry to the green body, the glaze amount is 450g / m2, sintering at 1230°C for 2 hours, and cooling to obtain a finished ceramic tile;
[0091] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0092] Example 5
[0093] An environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, the steps are as follows:
[0094] S1, compression molding the green body raw material to obtain a green body;
[0095] The green body is composed of the following raw materials in parts by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc;
[0096] S2. Wet-mill the base glaze raw materials for 3 hours under the condition of material: ball: water = 1:3:1, and then pass through a 200-mesh sieve to obtain base glaze slurry, and then apply the base glaze slurry to the body, with a glaze amount of 450g / m 2 , pre-sintered at 900℃ for 3h;
[0097] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 12 parts of sodium silicate, and 6 parts of aluminum phosphate;
[0098] S3. Wet-mill the surface glaze raw materials for 5 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain the surface glaze slurry. Then apply the bottom glaze slurry to the body, and the glaze amount is 450g / m 2 , sintered at 1220℃ for 2.5h, and the finished ceramic tile was obtained after cooling;
[0099] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0100] Example 6
[0101] An environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, the steps are as follows:
[0102] S1, compression molding the green body raw material to obtain a green body;
[0103] The green body is composed of the following raw materials in parts by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc;
[0104] S2. Wet-mill the base glaze raw materials for 3 hours under the condition of material: ball: water = 1:3:1, and then pass through a 200-mesh sieve to obtain base glaze slurry, and then apply the base glaze slurry to the blank, with a glaze amount of 350g / m 2 , pre-sintered at 900℃ for 1.5h;
[0105] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 6 parts of sodium silicate, and 6 parts of aluminum phosphate;
[0106] S3. Wet-mill the surface glaze raw materials for 5 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain the surface glaze slurry. Then apply the bottom glaze slurry to the body, and the glaze amount is 550g / m 2 , sintered at 1250℃ for 2.5h, and the finished ceramic tile was obtained after cooling;
[0107] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0108] Example 7
[0109] An environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, the steps are as follows:
[0110] S1, compression molding the green body raw material to obtain a green body;
[0111] The green body is composed of the following raw materials in parts by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc;
[0112] S2. Wet-mill the base glaze raw materials for 3 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain base glaze slurry, and then apply the base glaze slurry to the blank, with a glaze amount of 450g / m2 , pre-sintered at 850℃ for 2h;
[0113] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 12 parts of sodium silicate, and 6 parts of aluminum phosphate;
[0114] S3. Wet-mill the surface glaze raw materials for 5 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain the surface glaze slurry. Then apply the bottom glaze slurry to the body, and the glaze amount is 550g / m 2 , sintered at 1230℃ for 3h, and the finished ceramic tile was obtained after cooling;
[0115] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0116] Example 8
[0117] An environmentally friendly, wear-resistant ceramic tile and a preparation method thereof, the steps are as follows:
[0118] S1, compression molding the green body raw material to obtain a green body;
[0119] The green body is composed of the following raw materials in parts by weight: 25 parts of kaolin, 18 parts of clay, 10 parts of aluminum sand, 3 parts of wollastonite, and 2.5 parts of talc;
[0120] S2. Wet-mill the base glaze raw materials for 3 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain base glaze slurry, and then apply the base glaze slurry to the body, and the glaze amount is 350g / m 2 , pre-sintered at 750℃ for 4.5h;
[0121] The base glaze is composed of the following raw materials in parts by weight: 35 parts of potassium feldspar, 10 parts of kaolin, 12 parts of talc, 8 parts of quartz, 16 parts of dolomite, 3 parts of barium carbonate, 16 parts of sodium silicate, and 8 parts of aluminum phosphate;
[0122] S3. Wet-mill the surface glaze raw materials for 5 hours under the condition of material: ball: water = 1:3:1, and then sieve through 200 mesh to obtain the surface glaze slurry. Then apply the bottom glaze slurry to the body, and the glaze amount is 450g / m 2 , sintered at 1230℃ for 2h, and the finished ceramic tile was obtained after cooling;
[0123] The glaze is composed of the following raw materials in parts by weight: 15 parts of albite, 15 parts of quartz sand, 15 parts of calcined kaolin, 7 parts of calcined alumina, 8 parts of kaolin, 3 parts of barium carbonate, 5 parts of silicon carbide, and 5 parts of aluminum nitride.
[0124] The ceramic tiles obtained in Examples 4-8 were tested, and the results showed no significant difference from those in Example 1.
[0125] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing an environmentally friendly, wear-resistant ceramic tile, characterized in that: The following steps are involved: S1, compression molding the green body raw material to obtain a green body; S2, wet-milling the base glaze raw material and sieving it to obtain base glaze slurry, and then applying the base glaze slurry to the green body for pre-firing; S3, wet-milling the glaze raw materials and sieving them to obtain glaze slurry, then applying the glaze slurry to the green body for sintering, and cooling to obtain a finished ceramic tile; The base glaze comprises the following raw materials by weight: 30-35 parts of potassium feldspar, 5-15 parts of kaolin, 5-15 parts of talc, 5-8 parts of quartz, 15-20 parts of dolomite, 2-5 parts of barium carbonate, 5-20 parts of sodium silicate, and 5-8 parts of aluminum phosphate; The glaze comprises the following raw materials by weight: 12-15 parts of albite, 10-15 parts of quartz sand, 15-25 parts of calcined kaolin, 5-10 parts of calcined alumina, 8-10 parts of kaolin, 2-5 parts of barium carbonate, 2-5 parts of silicon carbide, and 2-5 parts of aluminum nitride.
2. The preparation method according to claim 1, characterized in that: The weight ratio of sodium silicate to aluminum phosphate in the base glaze is (1-2):
1.
3. The preparation method according to claim 1, characterized in that: In the wet ball milling process of the glaze raw materials, the ratio of material: ball: water is 1:3:1, the ball milling time is 3 to 5 hours, and the raw materials are sieved with 200 mesh after ball milling.
4. The preparation method according to claim 1, characterized in that: The base glaze application amount is 350-450g / m 2 .
5. The preparation method according to claim 1, characterized in that: The pre-firing temperature is 600° C. to 900° C., and the pre-firing time is 1 to 5 hours.
6. The preparation method according to claim 1, characterized in that: In the wet ball milling process of the glaze raw materials, the ratio of material: ball: water is 1:3:1, the ball milling time is 3 to 5 hours, and the raw materials are sieved with 200 mesh after ball milling.
7. The preparation method according to claim 1, characterized in that: The amount of glaze applied is 350-550 g / m 2 .
8. The preparation method according to claim 1, characterized in that: The sintering temperature is 1220° C. to 1250° C., and the sintering time is 1 to 3 hours.
9. An environmentally friendly, wear-resistant ceramic tile, characterized in that: Prepared by the method according to any one of claims 1 to 8.
10. The ceramic brick according to claim 9 is used as a building decoration material.
Citation Information
Patent Citations
Self-enhanced ceramic cold glaze and preparation method thereof
CN105819900A
Wear-proof anti-skid ceramic and preparation method thereof
CN108249763A
Wear-resistant ceramic tile and preparation method thereof
CN115745568A
Glazed ceramic substrate and manufacturing method therefor
JP2005153363A
Protective ceramic coating
US20060147699A1