Microwave dielectric ceramic material with high quality factor and high dielectric constant and preparation method thereof
By adding trace amounts of Al2O3 or Cr2O5 to SrTiO3 and incorporating (Al0.5Ta0.5)4+ or (Cr0.5Ta0.5)4+ ions, microwave dielectric ceramic materials with high quality factor and high dielectric constant can be prepared to solve the problem. It is difficult to achieve both high dielectric constant and high quality factor in the existing technology, so the improvement of dielectric constant and quality factor and the green and environmentally friendly characteristics of the material have been achieved.
Patent Information
- Application Number
- CN202410943255.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-15
AI Technical Summary
It is difficult for existing microwave dielectric ceramics to have both high dielectric constant and high quality factor, and cannot meet the needs of modern communication technology for high performance and green and environmentally friendly materials.
Using the general chemical formula of SrTi1-x(A0.5Ta0.5)xO3, by adding a trace amount of Al2O3 or Cr2O5 to SrTiO3, (Al0.5Ta0.5)4+ or (Cr0.5Ta0.5)4+ ions are incorporated , adjust the dielectric constant and inhibit the reduction of Ti4+, and prepare microwave dielectric ceramic materials with high quality factor and high dielectric constant.
The continuous change of dielectric constant in the range of 200 to 270 is achieved, and the quality factor is increased to 5000GHz to 8500GHz. The material has the characteristics of high dielectric constant, high quality factor and green and pollution-free, and is suitable for miniaturization and integrated microwave radio frequency. device.
Smart Images

Figure CN118754648A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramics. Background Art
[0002] The information technology industry is related to the development of the national economy and is a major, basic and leading industry that my country is vigorously developing. RF devices, as the cornerstone of the development of the information technology industry, are also the focus of ensuring the gradual development of the relevant industrial chain. With the continuous development of RF devices, higher requirements are placed on the integration, ultra-micronization, digitization and intelligence of devices. Microwave communication has strong anti-external interference capabilities, large carrier capacity, and a rich variety of information that can be transmitted, making it play an important role in military, satellite communications, aerospace and other fields. Microwave dielectric ceramics, as a multifunctional ceramic material that has been continuously developed in recent decades, also play an indispensable role in it. Modern wireless communication technologies represented by 5G / 6G also put forward higher and newer requirements on the performance of microwave dielectric ceramics.
[0003] In practical applications, the specific application of microwave dielectric ceramics is mainly evaluated from three aspects: dielectric constant, quality factor and resonant frequency temperature coefficient. Since the size of RF devices is inversely proportional to the dielectric constant of microwave dielectric ceramic materials, in order to achieve miniaturization and integration of microwave RF devices, improving the dielectric constant of the material itself has become the key to research. In addition, high quality factor is also the key to effectively reduce the loss of devices and ensure good frequency selection characteristics of devices. The high dielectric constant microwave dielectric ceramic systems currently under research mainly include perovskite systems, Ba-based systems, Li-based systems, Zn-based systems and lead-based perovskite systems. Among them, the dielectric constant of the perovskite system (including CaTiO3, SrTiO3, etc.) is relatively high, but there is Ti sintering at high temperatures. 4+ Reduction to Ti 3+ The quality factor is low (Qf≤5000GHz); the dielectric constant of Ba-based and Zn-based systems is relatively small (80≤ε r ≤100); the Li element in the Li-based system is volatile and the material ratio is difficult to control; the lead-based perovskite system has certain pollution to the environment.
[0004] In summary, despite the urgent need in technology and application, it is difficult for the high-k microwave dielectric ceramics currently studied to have both high dielectric constant (ε r ≥200) and high quality factor (Qf≥5000GHz), it is difficult to meet the needs of practical applications. Therefore, how to ensure high dielectric constant while meeting high quality factor, and then develop a series of microwave dielectric ceramic materials with both high performance and green environmental protection has become a key field and research hotspot of modern communication technology. Summary of the invention
[0005] The present invention aims to solve the problem that existing microwave dielectric ceramics are difficult to simultaneously have a high dielectric constant and a high quality factor, and further provides a microwave dielectric ceramic material with a high quality factor and a high dielectric constant and a preparation method thereof.
[0006] A microwave dielectric ceramic material with a high quality factor and a high dielectric constant, whose chemical general formula is SrTi 1-x (A 0.5 Ta 0.5 ) x O3, where A is Cr or Al, and 0 < x ≤ 0.05.
[0007] A preparation method of a microwave dielectric ceramic material with a high quality factor and a high dielectric constant is carried out according to the following steps:
[0008] I. Weigh SrCO3 powder, TiO2 powder, powder containing element A and Ta2O5 powder according to the stoichiometric ratio of the chemical general formula SrTi 1-x (A 0.5 Ta 0.5 ) x O3 to obtain raw materials. Ball-mill and sieve the raw materials, and finally calcine them to obtain pre-calcined powder; the A is Cr or Al, 0 < x ≤ 0.05; the powder containing element A is Al2O3 powder or Cr2O3 powder;
[0009] II. Ball-mill and sieve the pre-calcined powder to obtain ball-milled powder;
[0010] III. Add a binder to the ball-milled powder, grind and sieve it to obtain granulated powder;
[0011] IV. Compact, debind and sinter the granulated powder to obtain a microwave dielectric ceramic material with a high quality factor and a high dielectric constant.
[0012] The beneficial effects of the present invention are as follows:
[0013] The chemical composition of the microwave dielectric ceramic material of the present invention is SrTi 1-x (A 0.5 Ta 0.5 ) x O3, where A is Cr or Al, and 0 < x ≤ 0.05. By adding a small amount of Al2O3 and Ta2O5 or adding a small amount of Cr2O3 and Ta2O5 to SrTiO3 in the present invention, (Al 4+ is doped into Ti at the B site of SrTiO3 0.5 Ta 0.5 ) 4+ or (Cr 0.5 Ta 0.5 ) 4+ions, whose dielectric constant can continuously decrease as the value of x increases, continuously varies within the range of 200 to 270. At the same time, due to the addition of composite ions, the reduction of Ti 4+ to Ti 3+ , greatly improves the grain size of the material, reduces the number of defects and grain boundaries inside the material, and endows it with a relatively high quality factor of 5000 GHz to 8500 GHz. Therefore, the microwave dielectric ceramic material of the present invention has the characteristics of high and adjustable dielectric constant, high quality factor, and green and pollution-free. Moreover, the raw materials of the present invention will not cause pollution to the environment, are suitable for antennas in communications, or are suitable for microwave radio frequency devices such as dielectric resonators or filters under different sizes and usage environments, making it adaptable to miniaturization and integration.
[0014] Description of the Drawings
[0015] Figure 1 is the XRD pattern of the crystal phase composition of the microwave dielectric ceramic materials prepared in the examples and comparative examples;
[0016] Figure 2 is the SEM micrograph of the microstructure of the microwave dielectric ceramic materials prepared in Examples 3, 8 to 9 and Comparative Examples 3, 5 to 6. Detailed Embodiments
[0017] Detailed Embodiment 1: A microwave dielectric ceramic material with a high quality factor and a high dielectric constant in this embodiment has a chemical general formula of SrTi 1-x (A 0.5 Ta 0.5 ) x O3, where A is Cr or Al, and 0 < x ≤ 0.05.
[0018] The beneficial effects of this embodiment are:
[0019] The chemical composition of the microwave dielectric ceramic material in this embodiment is SrTi 1-x (A 0.5 Ta 0.5 ) x O3, where A is Cr or Al, and 0 < x ≤ 0.05. In this embodiment, by adding a small amount of Al2O3 and Ta2O5, or adding a small amount of Cr2O3 and Ta2O5 to SrTiO3, (Al 4+ Ta 0.5 ) 4+ or (Cr 0.5 Ta 0.5 ) 4+ ions are doped into the Ti 4+ in the B-site of SrTiO3. The dielectric constant of these ions can continuously decrease as the value of x increases, continuously varying within the range of 200 to 270. At the same time, due to the addition of composite ions, the reduction of Ti4+ Reduced to Ti 3+ , greatly improving the grain size of the material, reducing the number of defects and grain boundaries inside the material, and endowing it with a relatively high quality factor of 5000 GHz to 8500 GHz. Therefore, the microwave dielectric ceramic material of this embodiment has the characteristics of high and adjustable dielectric constant, high quality factor, and green pollution-free. Moreover, the raw materials of this embodiment will not cause pollution to the environment, and are suitable for antennas in communication, or for microwave radio frequency devices such as dielectric resonators or filters under different sizes and usage environments, making it adaptable to miniaturization and integration.
[0020] Specific Embodiment 2: The difference between this embodiment and Specific Embodiment 1 is that: the dielectric constant of the microwave dielectric ceramic material with high quality factor and high dielectric constant is 200 to 270, and the quality factor is 5000 GHz to 8500 GHz. Others are the same as Specific Embodiment 1.
[0021] Specific Embodiment 3: A preparation method of a microwave dielectric ceramic material with high quality factor and high dielectric constant, which is prepared according to the following steps:
[0022] 1. Weigh SrCO3 powder, TiO2 powder, powder containing element A, and Ta2O5 powder according to the stoichiometric ratio of the chemical formula SrTi 1-x (A 0.5 Ta 0.5 ) x O3 to obtain raw materials. Ball mill and screen the raw materials, and finally calcine to obtain pre-calcined powder; the A is Cr or Al, 0 < x ≤ 0.05; the powder containing element A is Al2O3 powder or Cr2O3 powder;
[0023] 2. Ball mill and screen the pre-calcined powder to obtain ball-milled powder;
[0024] 3. Add a binder to the ball-milled powder, grind and screen it to obtain granulated powder;
[0025] 4. Compact, degrease and sinter the granulated powder to obtain a microwave dielectric ceramic material with high quality factor and high dielectric constant.
[0026] Specific Embodiment 4: The difference between this embodiment and Specific Embodiment 3 is that: the ball milling in Steps 1 and 2 is specifically carried out according to the following steps: using zirconia balls as grinding balls, anhydrous ethanol as the ball milling medium, under the condition that the ball milling speed is 400 revolutions per minute to 500 revolutions per minute, ball mill for 12 h to 16 h, and then under the condition that the temperature is 80 °C to 105 °C, dry for 12 h to 24 h. Others are the same as Specific Embodiment 3.
[0027] Specific implementation method 5: This implementation method is different from specific implementation method 3 or 4 in that the sieving in step 1 and step 2 is through a 100-120 mesh screen, and the sieving in step 3 is through a 40-60 mesh screen. The rest is the same as specific implementation method 3 or 4.
[0028] Specific embodiment 6: This embodiment is different from specific embodiments 3 to 5 in that the calcination in step 1 is carried out in an air atmosphere at a pre-calcination temperature of 1200° C. to 1350° C. for 3 to 6 hours. The rest is the same as specific embodiments 3 to 5.
[0029] Specific embodiment 7: This embodiment differs from any one of specific embodiments 3 to 6 in that: the binder in step 3 is a polyvinyl alcohol solution with a mass percentage of 4% to 6%; the mass of the binder in step 3 is 12% to 18% of the mass of the ball-milled powder. The rest is the same as specific embodiments 3 to 6.
[0030] Specific embodiment 8: This embodiment is different from specific embodiments 3 to 7 in that the green compact described in step 4 is specifically made under a green compact pressure of 150 MPa to 200 MPa, and the pressure is maintained for 5 to 8 minutes to obtain a cylindrical green body with a diameter of 10 mm to 20 mm and a thickness of 3 mm to 6 mm. The rest is the same as specific embodiments 3 to 7.
[0031] Specific embodiment 9: This embodiment is different from any one of specific embodiments 3 to 8 in that the debinding in step 4 is carried out at a debinding temperature of 550° C. to 620° C. for 2 h to 4 h. The rest is the same as specific embodiments 3 to 8.
[0032] Specific embodiment 10: This embodiment differs from any one of specific embodiments 3 to 9 in that the sintering in step 4 is carried out in an air atmosphere at a temperature of 1400° C. to 1550° C. for 4 to 6 hours. The rest is the same as specific embodiments 3 to 9.
[0033] The following examples are used to verify the beneficial effects of the present invention:
[0034] Embodiment 1:
[0035] A method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant is prepared according to the following steps:
[0036] 1. According to the chemical formula SrTi 0.995 (Al 0.5 Ta 0.5 ) 0.005SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed to obtain raw materials, and zirconium oxide balls were used as grinding balls and anhydrous ethanol was used as ball milling media. The raw materials were ball milled for 12 hours at a ball milling speed of 500 rpm, and then dried at a temperature of 105°C for 24 hours, and then passed through a 120-mesh sieve. Finally, the raw materials were kept warm for 6 hours in an air atmosphere at a pre-calcination temperature of 1200°C to obtain pre-calcined powder; the mass ratio of the raw materials to the grinding balls was 1:3; the mass ratio of the raw materials to the ball milling media was 1:0.8;
[0037] 2. Using zirconium oxide balls as grinding balls and anhydrous ethanol as ball milling medium, the pre-burned powder was ball milled for 16 hours at a ball milling speed of 400 rpm, and then dried at a temperature of 105°C for 24 hours, and then passed through a 120-mesh sieve to obtain ball-milled powder; the mass ratio of the pre-burned powder to the grinding balls was 1:3; the mass ratio of the pre-burned powder to the ball milling medium was 1:0.5;
[0038] 3. Add a binder to the ball-milled powder for grinding, and then pass through a 60-mesh sieve to obtain granulated powder;
[0039] The binder is a polyvinyl alcohol solution with a mass percentage of 6%; the mass of the binder is 12% of the mass of the ball-milled powder;
[0040] 4. Under the condition of a pressing pressure of 150MPa, the granulated powder is kept under pressure for 6 minutes to obtain a cylindrical green body with a diameter of 15mm and a thickness of 6mm. Then, the green body is debonded at a debinding temperature of 610℃ for 4h. Finally, it is sintered in an air atmosphere at a temperature of 1400℃ for 4h to obtain a microwave dielectric ceramic material with a high quality factor and a high dielectric constant.
[0041] Example 2: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.99 (Al 0.5 Ta 0.5 ) 0.01 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed to obtain raw materials in a stoichiometric ratio of 1:1 to 1:1. The other steps were the same as those in Example 1.
[0042] Example 3: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.985 (Al 0.5 Ta 0.5 ) 0.015SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1250°C in an air atmosphere for 6 hours; in step 4, the pre-sintering temperature was 1450°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0043] Example 4: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.98 (Al 0.5 Ta 0.5 ) 0.02 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1250°C in an air atmosphere for 6 hours; in step 4, the pre-sintering temperature was 1450°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0044] Example 5: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.97 (Al 0.5 Ta 0.5 ) 0.03 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0045] Example 6: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.95 (Al 0.5 Ta 0.5 ) 0.05 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0046] Example 7: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.99 (Cr 0.5 Ta 0.5 ) 0.01 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed to obtain raw materials in a stoichiometric ratio of 1:1 to 1:1. The rest was the same as in Example 1.
[0047] Example 8: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.985 (Cr 0.5 Ta 0.5 ) 0.015 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed to obtain raw materials in a stoichiometric ratio of 1:1 to 1:1. The rest was the same as in Example 1.
[0048] Example 9: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.98 (Cr 0.5 Ta 0.5 ) 0.02 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1250°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1500°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0049] Embodiment 10: This embodiment differs from Embodiment 1 in that: in step 1, according to the chemical formula SrTi 0.975 (Cr 0.5 Ta 0.5 ) 0.025 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1250°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1500°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0050] Example 11: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.97 (Cr 0.5 Ta 0.5 ) 0.03 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0051] Example 12: This example is different from Example 1 in that: in step 1, according to the chemical formula SrTi 0.96 (Cr 0.5 Ta 0.5 ) 0.04SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0052] Comparative Example 1: This embodiment differs from Embodiment 1 in that: in step 1, SrCO3 powder and TiO2 powder are weighed in a stoichiometric ratio of the chemical formula SrTiO3 to obtain a raw material. The rest is the same as Embodiment 1.
[0053] Comparative Example 2: The difference between this embodiment and embodiment 1 is that in step 1, according to the chemical formula SrTi 0.9 (Al 0.5 Ta 0.5 ) 0.1 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0054] Comparative Example 3: The difference between this embodiment and embodiment 1 is that in step 1, according to the chemical formula SrTi 0.8 (Al 0.5 Ta 0.5 ) 0.2 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0055] Comparative Example 4: This embodiment differs from Embodiment 1 in that: in step 1, according to the chemical formula SrTi 0.94 (Cr 0.5 Ta 0.5 ) 0.06 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0056] Comparative Example 5: This embodiment differs from Embodiment 1 in that: in step 1, according to the chemical formula SrTi 0.9 (Cr 0.5 Ta 0.5 )0.1 SrCO3 powder, TiO2 powder, Cr2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of O3 to obtain raw materials; in step 1, the pre-sintering temperature was 1300°C in an air atmosphere for 6 hours; in step 4, the sintering temperature was 1550°C in an air atmosphere for 4 hours. The rest was the same as in Example 1.
[0057] Comparative Example 6: This embodiment differs from Embodiment 1 in that: in step 1, according to the chemical formula SrTi 0.985 (Al 0.5 Ta 0.5 ) 0.015 SrCO3 powder, TiO2 powder, Al2O3 powder and Ta2O5 powder were weighed in a stoichiometric ratio of 1.250°C to obtain raw materials; in step 1, the pre-sintering temperature was kept at 1250°C in an air atmosphere for 6 hours; in step 4, the pre-sintering temperature was 1450°C in a nitrogen atmosphere for 4 hours. The rest was the same as in Example 1.
[0058] The microwave dielectric ceramic materials prepared in the examples and comparative examples were polished on both sides and kept parallel to each other, and then the dielectric properties (i.e., the resonant frequency f, the dielectric constant ε r , dielectric loss tanδ (Q=1 / tanδ), quality factor Qf). After testing, the content of each component and the dielectric properties of the embodiments and comparative examples are shown in Table 1:
[0059] Table 1
[0060]
[0061]
[0062] It can be seen from Table 1 that the microwave dielectric ceramic material prepared in the embodiment can achieve a dielectric constant ε r It is 200-270, the quality factor Qf is 5000GHz-8500GHz, and the dielectric constant range can be adjusted according to different values of x.
[0063] Figure 1 XRD diagrams of the crystalline phase composition of microwave dielectric ceramic materials prepared in the embodiment and the comparative example; as can be seen from the figure, the embodiment has a relatively low doping amount and can achieve solid solution, so the main crystalline phase of the prepared ceramic material is single-phase SrTiO3, while the comparative example has a relatively high doping amount and some impure phases appear. The material quality factor of the comparative example is reduced due to the presence of impurities such as TiO2.
[0064] Figure 2The microscopic morphology SEM images of microwave dielectric ceramic materials prepared in Examples 3, 8-9 and Comparative Examples 3, 5-6; it can be seen from the figure that the grain size of the ceramic material prepared in the examples is very large, and the large grain size reduces the number of grain boundaries and has fewer pores, thereby improving the quality factor of the material, while in Comparative Examples 3 and 5, the grain size is smaller, the pores are more, and there are impure phases of TiO2 of different colors, all of which lead to the quality factor of the comparative materials being much smaller than that of the example materials. The grain size of Comparative Example 6 is larger than that of the other comparative examples. This may be because nitrogen sintering promotes the volatilization of oxygen ions in the ceramic lattice in the form of oxygen to form oxygen vacancies. The presence of a certain amount of oxygen vacancies in the ceramic promotes the transfer of substances in the grains, resulting in an increase in the grain size; however, nitrogen sintering also releases electrons while generating oxygen vacancies, accelerating the Ti 4+ The reduction of ions causes the dielectric loss of the material to increase and the quality factor to decrease rapidly compared to the embodiment, so microwave dielectric ceramics with both high dielectric and high quality factor can be prepared by sintering in an air atmosphere.
Claims
1. A microwave dielectric ceramic material with high quality factor and high dielectric constant, characterized in that Its general chemical formula is SrTi 1-x (A 0.5 Ta 0.5 ) x O3, where A is Cr or Al, 0 <x≤0.05。 2. The microwave dielectric ceramic material with high quality factor and high dielectric constant according to claim 1, characterized in that The microwave dielectric ceramic material with high quality factor and high dielectric constant has a dielectric constant of 200 to 270 and a quality factor of 5000 GHz to 8500 GHz.
3. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant as claimed in claim 1, characterized in that It is carried out in the following steps:
1. According to the chemical general formula SrTi 1-x (A 0.5 Ta 0.5 ) x O3, weigh SrCO3 powder, TiO2 powder, powder containing element A and Ta2O5 powder according to the stoichiometric ratio to obtain raw materials. Ball-mill and sieve the raw materials, and finally calcine to obtain pre-calcined powder; A is Cr or Al, 0 < x ≤ 0.05; the powder containing element A is Al2O3 powder or Cr2O3 powder; 2. ball-milling and sieving the pre-calcined powder to obtain ball-milled powder; 3. Adding a binder to the ball-milled powder, grinding and sieving to obtain granulated powder; Fourth, the granulated powder is pressed, debinded and sintered to obtain a microwave dielectric ceramic material with a high quality factor and a high dielectric constant.
4. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The ball milling described in step 1 and step 2 is specifically carried out according to the following steps: using zirconium oxide balls as grinding balls and anhydrous ethanol as ball milling media, ball milling for 12h to 16h at a ball milling speed of 400 rpm to 500 rpm, and then drying for 12h to 24h at a temperature of 80°C to 105°C.
5. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The sieving in step 1 and step 2 is through a 100-mesh to 120-mesh sieve; the sieving in step 3 is through a 40-mesh to 60-mesh sieve.
6. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The calcination in step 1 is specifically carried out in an air atmosphere at a pre-calcination temperature of 1200° C. to 1350° C. for 3 h to 6 h.
7. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The binder described in step three is a polyvinyl alcohol solution with a mass percentage of 4% to 6%; the mass of the binder described in step three is 12% to 18% of the mass of the ball-milled powder.
8. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The green compact described in step 4 is specifically made under a green compact pressure of 150 MPa to 200 MPa, maintained at pressure for 5 to 8 minutes, to obtain a cylindrical green compact with a diameter of 10 mm to 20 mm and a thickness of 3 mm to 6 mm.
9. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The debinding described in step 4 is specifically performed at a debinding temperature of 550° C. to 620° C. for 2 h to 4 h.
10. The method for preparing a microwave dielectric ceramic material with a high quality factor and a high dielectric constant according to claim 3, characterized in that The sintering described in step 4 is specifically carried out in an air atmosphere at a temperature of 1400° C. to 1550° C. for 4 h to 6 h.
Citation Information
Patent Citations
High-permittivity microwave dielectric ceramic material and preparation method thereof
CN105693235A
Ta and Al co-doped strontium titanate-based giant dielectric ceramic material and preparation method thereof
CN117401970A
Electronic part, dielectric porcelain composition, and method for manufacturing the same
JP2007246347A