Method for preparing yttrium-magnesium multiphase transparent ceramic through non-water-based gel casting

Through a non-water-based injection molding method, large-sized and complex-shaped yttrium oxide-magnesium oxide nanocomplex ceramics were prepared, which solved the problems of uneven composition and high molding difficulty in the existing technology, and realized the production of high-performance ceramics. Preparation and simplified process flow.

CN118754662AActive Publication Date: 2024-10-11宜宾红星电子有限公司

Patent Information

Application Number
CN202410905207.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

It is difficult to prepare large-sized, complex-shaped yttrium oxide-magnesium oxide nanocomposite phase transparent ceramics with existing technology, and the composition is uneven, making it difficult to meet the high performance requirements of infrared window materials.

Method used

Using a non-water-based injection molding method, by designing a suitable non-water-based solvent system, Y2O3 nanopowder and MgO nanopowder are mixed with epoxy resin and curing agent, ball milled and solidified to obtain ceramic slurry, and passed Calcination, sintering and annealing yield yttrium-magnesium complex-phase transparent ceramics.

Benefits of technology

The preparation of large-sized and complex-shaped yttrium oxide-magnesia nanocomposite ceramics has been achieved. The molding difficulty is reduced and the sample performance is excellent. It solves the problem of difficulty in preparation by the traditional dry pressing method and avoids the interaction between yttrium oxide, magnesium oxide and water. reaction, simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754662A_ABST
    Figure CN118754662A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing yttrium-magnesium multiphase transparent ceramic through non-water-based gel casting, and belongs to the technical field of ceramic preparation. In order to overcome the problems of water-based system gel casting, the invention provides a method for preparing yttrium-magnesium multiphase transparent ceramic by non-water-based gel casting, which comprises the following steps: ball-milling Y2O3, MgO, a dispersing agent and a non-water-based solvent, then adding epoxy resin and a curing agent, ball-milling again, defoaming, curing and drying the obtained ceramic slurry, thereby obtaining the yttrium-magnesium multiphase transparent ceramic. And carrying out rubber discharging, sintering densification, cooling, hot isostatic pressing sintering, annealing and polishing to obtain the yttrium-magnesium multiphase transparent ceramic. By designing a non-water-based solvent system and selecting a proper gel system, the problems that large-size Y2O3-MgO nano complex-phase infrared transparent ceramic is difficult to prepare, uneven in components and the like are solved, and the yttrium oxide-magnesium oxide nano complex-phase ceramic with complex shape / large size and uniform components can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic preparation, and in particular relates to a method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous-based gelcasting. Background Art

[0002] Infrared imaging, infrared precision guidance and infrared countermeasure technologies have a strategic position in modern military applications, and infrared windows and fairings are key components of infrared technology. They need to bear the load of aerodynamics and prevent the external environment from corroding and damaging the imaging system. While achieving the protection function, they must also have high detection sensitivity and anti-interference capabilities. In order to meet the equipment requirements of the new generation of air-to-air missiles to effectively strike high-stealth, high-mobility and high-speed targets, and to adapt to the national defense needs of future air combat, the development of a new generation of infrared window materials that meet (1) optical properties: high transmittance and low high-temperature infrared thermal radiation; (2) mechanical properties: impact resistance, high hardness and high strength; (3) thermodynamic properties: good thermal shock resistance and small thermal expansion coefficient; (4) excellent chemical properties has become a research hotspot and research focus in various countries.

[0003] The emissivity of Y2O3 varies the least with wavelength, and it has the lowest high-temperature infrared radiation coefficient at the same temperature, and has low scattering rate and excellent high-temperature mechanical properties. However, the mechanical properties of pure phase yttrium oxide are poor and it is not suitable for high-Mach applications. By introducing cubic MgO as the second phase to inhibit the growth of Y2O3 grains, a new generation of infrared transparent materials with extremely excellent mechanical properties and optical properties can be obtained. However, how to prepare high-performance, large-sized nanocomposite ceramics with uniform phase distribution has always been the focus and difficulty in the research field.

[0004] Gel casting is a near-net-size molding process developed after slip casting and tape casting. The principle is to solidify the ceramic powder in situ by forming a macromolecular network through the reaction of the gel system. It was successfully developed by the Oak Ridge National Laboratory in the United States. Compared with the traditional dry pressing molding method, it has the advantages of preparing complex shape molding, high green body strength, uniform components, and simple preparation process. The gel casting molding system can be divided into a water-based system and a non-water-based system. However, when using a water-based system, it is necessary to consider the wettability of the solvent system and the powder, the drying rate, and other issues. At the same time, nanopowders such as yttrium oxide and magnesium oxide will also react with water. In addition, there are currently no reports on the use of non-aqueous gel casting technology to prepare yttrium oxide-magnesium oxide nanocomposite transparent ceramics.

[0005] CN113754435A discloses a method for preparing Y2O3-MgO infrared transparent ceramics, comprising the following steps: S1: weighing Y2O3 and MgO nanopowders in proportion, respectively ball milling, drying and sieving, and mixing them evenly to obtain nanocomposite powder; S2: placing the nanocomposite powder obtained in S1 into a muffle furnace for pre-sintering and debinding treatment to remove organic matter in the powder; S3: placing the nanocomposite powder after debinding treatment in S2 into a graphite mold. , hot pressing sintering is performed at a sintering temperature of 900-1200°C, a pressure of 20-40MPa, and a time of 10-30min to obtain a composite ceramic body; S4: the composite ceramic body obtained in S3 is connected in series to the positive and negative ends of an external power supply with a platinum wire, and an electric field strength of 600-1000V / cm is applied at a furnace temperature of 1150-1350°C. After the composite ceramic body flashes, the current density is controlled to be 20-100mA / mm 2 , and keep it for 10s to 5min, and then cool it in the furnace to obtain high-density Y2O3-MgO ceramics. This method uses hot pressing to prepare multiphase samples, directly placing the powder in a graphite mold, and sintering with uniaxial pressure to complete the molding and sintering at the same time. This method has great molding limitations and is only suitable for molding The following small discs have limited preparation thickness and can only prepare one sample at a time in a single furnace, which does not have the capacity for large-scale preparation.

[0006] CN109354501A discloses a method for preparing a MgAlON transparent ceramic, comprising the following steps: step 1: taking MgAlON powder for standby use; step 2: weighing Y2O3 powder, LiF powder, and SiO2 powder, and mixing them according to a mass ratio of LiF content of 15% to 40%, Y2O3 content of 20% to 55%, and SiO2 content of 25% to 60%, to obtain a multiphase sintering aid for standby use; step 3: taking MgAlON powder and the multiphase sintering aid, and the mass ratio of the multiphase sintering aid The mass percentage is 0.2% to 1.0%, and the mass percentage of MgAlON powder is 99% to 99.8%, which are dispersed in anhydrous ethanol with an anhydrous ethanol purity of not less than 99.5%, and the slurry is obtained after ball milling; step 4: after the slurry is dried, it is pressed into a blank; step 5: the blank is loaded into a high-purity BN crucible, and then placed together in a high-temperature sintering furnace, with high-purity nitrogen as a protective gas, the temperature is raised to 1750℃ to 1850℃ and kept for 10h to 30h, and then taken out after natural cooling, and polished to obtain MgAlON transparent ceramics. Although this method uses an anhydrous ethanol non-aqueous system, its method is not suitable for the preparation of yttrium oxide-magnesium oxide nanocomposite transparent ceramics. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing complex transparent ceramics by non-aqueous injection molding, so as to overcome the difficulties in preparing large-sized Y2O3-MgO nano-composite infrared transparent ceramics and the problems of uneven components. The method of the present invention can prepare yttrium oxide-magnesium oxide nano-composite ceramics with complex shapes / large sizes and uniform components by designing a non-aqueous solvent system and selecting a suitable gel system.

[0008] To achieve the above object, the present invention provides a method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting, which comprises the following steps:

[0009] A. Y2O3 nanopowder, MgO nanopowder, dispersant and non-aqueous solvent are mixed, ball milled for the first time, and then epoxy resin and curing agent are added, ball milled for the second time to obtain ceramic slurry;

[0010] B. The ceramic slurry obtained in step A is defoamed, solidified and dried to obtain a ceramic blank;

[0011] C. The ceramic blank obtained in step B is calcined at 400-850° C. in air to perform binder removal treatment, and then heated to 1000-1500° C. for sintering and densification, and after cooling, hot isostatic pressing is performed at 1000-1500° C. in a high-pressure inert atmosphere, and finally annealed and polished to obtain yttrium-magnesium composite transparent ceramics;

[0012] In step A, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is 1:9 to 9:1; the non-aqueous solvent is at least one of ethanol, propanol, isopropanol, acetone, butanone or toluene; the amount of the non-aqueous solvent is 10% to 30% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

[0013] Preferably, in the above method, in step A, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is 1:5 to 5:1.

[0014] More preferably, in the above method, in step A, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is 1:1.

[0015] Wherein, in the above method, in step A, the dispersant is polyacrylic acid, herring oil, polyacrylate or castor oil.

[0016] Preferably, in the above method, in step A, the dispersant is polyacrylic acid.

[0017] Wherein, in the above method, in step A, the amount of the dispersant used is 0.1% to 5% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

[0018] Wherein, in the above method, in step A, the epoxy resin is ethylene glycol diglycidyl ether (EGDGE) or glycerol glycidyl ester.

[0019] Preferably, in the above method, in step A, the epoxy resin is ethylene glycol diglycidyl ether (EGDGE).

[0020] Wherein, in the above method, in step A, the amount of the epoxy resin used is 1% to 4% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

[0021] Wherein, in the above method, in step A, the curing agent is 3,3′-diaminodipropylamine (DPTA), triethylenediamine or ethylenediamine.

[0022] Preferably, in the above method, in step A, the curing agent is 3,3′-diaminodipropylamine (DPTA).

[0023] Wherein, in the above method, in step A, the amount of the curing agent used is 10 to 50% of the mass of the epoxy resin.

[0024] Wherein, in the above method, in step A, during the first ball milling, zirconium oxide balls are added, and the amount of zirconium oxide balls added is 2 to 10 times the total mass of the Y2O3 nanopowder and the MgO nanopowder.

[0025] Wherein, in the above method, in step A, the rotation speed of the first ball milling is 150 to 240 rad / s.

[0026] Wherein, in the above method, in step A, the time of the first ball milling is 30 to 60 hours.

[0027] Wherein, in the above method, in step A, the rotation speed of the second ball milling is 150-240 rad / s.

[0028] Wherein, in the above method, in step A, the time of the second ball milling is 0.5 to 1 hour.

[0029] Wherein, in the above method, in step A, the solid content of the obtained ceramic slurry is 40 vol.% to 60 vol.%.

[0030] Wherein, in the above method, in step B, the degassing is performed by vacuum stirring with a vacuum degree of 0.1 Mpa for a time of 1 to 10 min.

[0031] Wherein, in the above method, in step B, the curing temperature is 20 to 80°C.

[0032] Wherein, in the above method, in step B, the curing time is 30 to 300 minutes.

[0033] Wherein, in the above method, in step B, the drying is performed by gradient heating at 25 to 150°C.

[0034] Wherein, in the above method, in step B, the drying time is 12 to 48 hours.

[0035] Wherein, in the above method, in step C, the calcination time at 400-850° C. is 1-10 hours.

[0036] Wherein, in the above method, in step C, the sintering time for densification at 1000-1500° C. is 2-10 hours.

[0037] Wherein, in the above method, in step C, the gas pressure of the high-pressure inert atmosphere is 160-200 MPa.

[0038] Wherein, in the above method, in step C, the hot isostatic pressing sintering time is 0.5 to 6 hours.

[0039] Wherein, in the above method, in step C, the annealing condition is in an air atmosphere, at 1000-1400° C. for 10-80 hours.

[0040] Beneficial effects of the present invention:

[0041] The present invention realizes the preparation of large-size / complex-shaped yttrium oxide-magnesium oxide nanocomposite ceramics using non-aqueous injection molding for the first time, and has the following advantages: 1. It can prepare large-size, shape-controllable, and excellent-performance nanocomposite ceramics, and the molding difficulty is low, the yield rate is higher, and it is easier to prepare high-performance ceramic samples, which solves the problem that this type of nanoceramics is difficult to prepare by dry pressing; 2. Compared with the water-based system, the use of a non-aqueous solvent system can avoid the hydration problem of yttrium oxide and magnesium oxide, and at the same time, it is not necessary to perform complex modification treatment on yttrium oxide and magnesium oxide, and the preparation process is simpler and more stable; 3. It can prepare a ceramic slurry with a solid content of up to 40-60 vol%. After molding, the sample blank has high strength, high density, and uniform components, which is more conducive to the sintering and densification of yttrium oxide-magnesium oxide nanocomposite ceramics, and then obtains samples with better optical and mechanical properties. The method of the present invention can simply, quickly, and scale the preparation of yttrium oxide-magnesium oxide nanocomposite transparent ceramics, which is of great significance for promoting its application in the field of optical windows. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a transmittance diagram of the yttrium oxide-magnesium oxide nanocomposite transparent ceramic according to Example 1 of the present invention.

[0043] Figure 2 This is a SEM image of the yttrium oxide-magnesium oxide nanocomposite transparent ceramic according to Example 1 of the present invention. DETAILED DESCRIPTION

[0044] Specifically, a method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting comprises the following steps:

[0045] A. Y2O3 nanopowder, MgO nanopowder, dispersant and non-aqueous solvent are mixed, ball milled for the first time, and then epoxy resin and curing agent are added, ball milled for the second time to obtain ceramic slurry;

[0046] B. The ceramic slurry obtained in step A is defoamed, solidified and dried to obtain a ceramic blank;

[0047] C. The ceramic blank obtained in step B is calcined at 400-850° C. in air to perform binder removal treatment, and then heated to 1000-1500° C. for sintering and densification, and after cooling, hot isostatic pressing is performed at 1000-1500° C. in a high-pressure inert atmosphere, and finally annealed and polished to obtain yttrium-magnesium composite transparent ceramics;

[0048] In step A, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is 1:9 to 9:1; the non-aqueous solvent is at least one of ethanol, propanol, isopropanol, acetone, butanone or toluene; the amount of the non-aqueous solvent is 10% to 30% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

[0049] In step A of the method of the present invention, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is preferably 1:5 to 5:1; more preferably 1:1.

[0050] The main feature of the non-aqueous gel injection molding of the present invention as a ceramic molding process is the use of non-aqueous solvents. Therefore, it is necessary to control the dispersant, epoxy resin, curing agent and other necessary organic components for gel injection molding. Epoxy resin and curing agent are used to form a gel network, and the dispersant is a necessary condition for achieving high solid content, low viscosity and uniform slurry. The above-mentioned organic components need to be screened according to the properties of the slurry, solvent and powder, and are all necessary conditions for achieving gel injection molding.

[0051] In step A of the present invention, the dispersant is polyacrylic acid, herring oil, polyacrylate or castor oil; preferably polyacrylic acid; the amount of the dispersant is 0.1% to 5% of the total mass of the Y2O3 nanopowder and the MgO nanopowder. In step A, the epoxy resin is ethylene glycol diglycidyl ether (EGDGE) or glycerol glycidyl ester; preferably ethylene glycol diglycidyl ether (EGDGE); the amount of the epoxy resin is 1 to 4% of the total mass of the Y2O3 nanopowder and the MgO nanopowder. In step A, the curing agent is 3,3'-diaminodipropylamine (DPTA), triethylenediamine or ethylenediamine; preferably 3,3'-diaminodipropylamine (DPTA); the amount of the curing agent is 10 to 50% of the mass of the epoxy resin.

[0052] In step A of the present invention, ball milling needs to be performed in stages. The first stage of ball milling is to add a dispersant to fully mix the two phases, which is the premise for continuing the second stage. In the second stage, epoxy resin and curing agent are added to form a gel network, and then solidified after mixing to achieve sample molding. In step A of the present invention, the rotation speed of the ball milling in the first stage is 150-240 rad / s, and the time of the ball milling in the first stage is 30-60h; the rotation speed of the ball milling in the second stage is 150-240 rad / s, and the time of the ball milling in the second stage is 0.5-1h.

[0053] In step A of the present invention, during the first ball milling, zirconium oxide balls are added, and the amount of zirconium oxide balls added is 2 to 10 times the total mass of the Y2O3 nanopowder and the MgO nanopowder.

[0054] The present invention adopts non-aqueous injection molding and controls the dispersant, epoxy resin and curing agent so that the solid content of the obtained ceramic slurry is 40 vol.% to 60 vol.%, so that the green body of the sample after molding has high strength, high density and uniform components, which is more conducive to the sintering and densification of yttrium oxide-magnesium oxide nanocomposite ceramics, thereby obtaining samples with better optical and mechanical properties.

[0055] In step B of the present invention, the degassing is performed by vacuum stirring with a vacuum degree of 0.1 Mpa for a time of 1 to 10 min.

[0056] In step B of the present invention, the curing temperature is 20 to 80° C.; the curing time is 30 to 300 minutes.

[0057] In step B of the present invention, the drying is performed by gradient temperature increase at 25 to 150° C.; the drying time is 12 to 48 hours.

[0058] In step C of the present invention, the calcination time at 400-850° C. is 1-10 hours.

[0059] In step C of the present invention, the sintering and densification time at 1000-1500° C. is 2-10 hours.

[0060] In step C of the present invention, the pressure of the high-pressure inert atmosphere is 160-200 MPa.

[0061] In step C of the present invention, the hot isostatic pressing sintering time is 0.5 to 6 hours.

[0062] In step C of the present invention, the annealing condition is to keep the temperature at 1000-1400° C. for 10-80 hours in an air atmosphere.

[0063] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.

[0064] In the embodiment of the present invention, the dispersant is polyacrylic acid; the gelling agent is epoxy resin, namely ethylene glycol diglycidyl ether (EGDGE); and the curing agent is 3,3′-diaminodipropylamine (DPTA).

[0065] Example 1

[0066] Step 1, slurry preparation: weigh Y2O3 and MgO nano commercial powders in a volume ratio of 1:1, weigh anhydrous ethanol as an organic solvent, add them into a ball mill in a mass ratio of composite powder (total mass of Y2O3 and MgO): anhydrous ethanol: dispersant: zirconium oxide balls = 10:1.5:0.1:40, ball mill at a speed of 180 rad / s for 40 hours, then weigh 2wt% of the composite powder mass of epoxy resin as a gelling agent, weigh 15wt% of the gelling agent mass of a curing agent, add them to the slurry, continue ball milling for 30 minutes, and obtain a ceramic slurry with a solid content of 50vol.%.

[0067] Step 2, sample molding: After the ceramic slurry obtained in step 1 is discharged, vacuum stirring is performed to degas, the vacuum degree is 0.1Mpa, and the time is 5min. The defoamed slurry is injected into the mold, heated to 40°C and cured for 150min, then demolded and the green body is taken out, and the taken green body is placed in an oven for drying, first at 25°C for 20h, and then gradually heated to 120°C for 12h, until the weight of the green body no longer decreases, to obtain a ceramic green body.

[0068] Step 3, ceramic sintering: The ceramic green body is heated to 800°C in a muffle furnace and kept for 6 hours for debinding treatment, then heated to 1350°C for 6 hours, and cooled naturally to room temperature to obtain a ceramic body with a relative density of 96%, and then the ceramic body is hot isostatically pressed for 2 hours at 1300°C and 200MPa argon atmosphere. After sintering, annealing is performed at 1200°C in an air atmosphere for 30 hours, and after double-sided polishing, yttrium-magnesium composite infrared transparent ceramics are obtained.

[0069] The maximum transmittance of a 3mm thick sample in the 3-5μm band is measured to be 86%@5μm, the average transmittance is >83%, and the three-point bending strength reaches 500MPa, with excellent performance.

[0070] Example 2

[0071] Step 1, slurry preparation: weigh Y2O3 and MgO nano commercial powders in a volume ratio of 1:1, weigh anhydrous ethanol and butanone as organic solvents, add them into a ball mill in a mass ratio of composite powder: anhydrous ethanol: butanone: dispersant: zirconia ball = 10: 0.5: 0.8: 0.1: 40, ball mill at a speed of 180 rad / s for 30 hours, then weigh 1.5 wt% of the composite powder mass of epoxy resin as a gelling agent, weigh 10 wt% of the gelling agent mass of curing agent, add them to the slurry, continue ball milling for 30 minutes, and obtain a ceramic slurry with a solid content of 52 vol.%.

[0072] Step 2, sample molding: After the ceramic slurry obtained in step 1 is discharged, vacuum stirring is performed to degas, the vacuum degree is 0.1Mpa, and the time is 5min. The defoamed slurry is injected into the mold, heated to 30°C and cured for 300min, then demolded and the green body is taken out, and the taken green body is placed in an oven for drying, first at 25°C for 20h, then heated to 60°C for 12h, and finally gradually heated to 120°C, and dried until the weight of the green body no longer decreases to obtain a ceramic green body.

[0073] Step 3, ceramic sintering: The ceramic green body is heated to 800°C in a muffle furnace and kept for 6 hours for debinding treatment, then heated to 1250°C for 10 hours, and naturally cooled to room temperature to obtain a ceramic body with a relative density of 95%, and then the ceramic body is hot isostatically pressed and sintered for 6 hours at 1250°C and 200MPa argon atmosphere. After sintering, annealing is performed at 1100°C in an air atmosphere for 80 hours, and after double-sided polishing, yttrium-magnesium composite infrared transparent ceramics are obtained.

[0074] The maximum transmittance of a 3mm thick sample in the 3-5μm band is measured to be 83%@5μm, the average transmittance is 80%, and the three-point bending strength is 460MPa.

[0075] Example 3

[0076] Step 1, slurry preparation: weigh Y2O3 and MgO nano commercial powders in a volume ratio of 1:1, weigh anhydrous ethanol as an organic solvent, add them into a ball mill in the ratio of complex phase powder: anhydrous ethanol: dispersant: zirconia ball = 10:1.8:0.1:40, ball mill at a speed of 180 rad / s for 40 hours, then weigh 4 wt% of the composite powder mass of epoxy resin as a gelling agent, weigh 20 wt% of the gelling agent mass of a curing agent, add them to the slurry, continue ball milling for 30 minutes, and obtain a ceramic slurry with a solid content of 45 vol.%.

[0077] Step 2, sample molding: After the ceramic slurry obtained in step 1 is discharged, vacuum stirring is performed to degas, the vacuum degree is 0.1Mpa, and the time is 5min. The defoamed slurry is injected into the mold, heated to 35°C and cured for 60min, then demolded and the green body is taken out, and the taken green body is placed in an oven for drying, first at 25°C for 24h, then heated to 50°C for 12h, and finally gradually heated to 120°C, and dried until the weight of the green body no longer changes, to obtain a ceramic green body.

[0078] Step 3, ceramic sintering: The ceramic green body is heated to 800°C in a muffle furnace and kept for 6 hours for debinding treatment, then heated to 1400°C for 2 hours, and cooled naturally to room temperature to obtain a ceramic body with a relative density of 97%, and then the ceramic body is hot isostatically pressed for 1 hour at 1300°C and 200MPa argon atmosphere. After sintering, annealing is performed at 1250°C in an air atmosphere for 10 hours, and after double-sided polishing, yttrium-magnesium composite infrared transparent ceramics are obtained.

[0079] The maximum transmittance of a 3mm thick sample in the 3-5μm band was measured to be 84%@5μm, and the three-point bending strength reached 400MPa.

Claims

1. A method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting, characterized in that: The following steps are involved: A. Y2O3 nanopowder, MgO nanopowder, dispersant and non-aqueous solvent are mixed, ball milled for the first time, and then epoxy resin and curing agent are added, ball milled for the second time to obtain ceramic slurry; B. The ceramic slurry obtained in step A is defoamed, solidified and dried to obtain a ceramic blank; C. The ceramic blank obtained in step B is calcined at 400-850° C. in air to perform binder removal treatment, and then heated to 1000-1500° C. for sintering and densification, and after cooling, hot isostatic pressing is performed at 1000-1500° C. in a high-pressure inert atmosphere, and finally annealed and polished to obtain yttrium-magnesium composite transparent ceramics; In step A, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is 1:9 to 9:1; the non-aqueous solvent is at least one of ethanol, propanol, isopropanol, acetone, butanone or toluene; the amount of the non-aqueous solvent is 10% to 30% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

2. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step A, the volume ratio of the Y2O3 nanopowder to the MgO nanopowder is 1:5 to 5:1, preferably 1:

1.

3. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step A, the dispersant is polyacrylic acid, herring oil, polyacrylate or castor oil; the amount of the dispersant is 0.1% to 5% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

4. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step A, the epoxy resin is ethylene glycol diglycidyl ether (EGDGE) or glycerol glycidyl ester; the amount of the epoxy resin used is 1-4% of the total mass of the Y2O3 nanopowder and the MgO nanopowder.

5. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step A, the curing agent is 3,3′-diaminodipropylamine (DPTA), triethylenediamine or ethylenediamine; the amount of the curing agent is 10-50% of the mass of the epoxy resin.

6. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step A, at least one of the following must be met: During the first ball milling, zirconium oxide balls are added, and the amount of zirconium oxide balls added is 2 to 10 times the total mass of the Y2O3 nanopowder and the MgO nanopowder; The rotation speed of the first ball milling is 150-240 rad / s; The first ball milling time is 30 to 60 hours; The rotation speed of the second ball milling is 150-240 rad / s; The second ball milling time is 0.5 to 1 h.

7. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step A, the solid content of the obtained ceramic slurry is 40 vol.% to 60 vol.%.

8. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step B, at least one of the following is met: The degassing method is vacuum stirring degassing, the vacuum degree is 0.1Mpa, and the time is 1 to 10min; The curing temperature is 20 to 80°C; The curing time is 30 to 300 minutes; The drying is performed by gradient heating at 25-150°C; The drying time is 12 to 48 hours.

9. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to claim 1, characterized in that: In step C, at least one of the following conditions must be met: The calcination time at 400-850° C. is 1-10 hours; The sintering time for densification at 1000-1500°C is 2-10h; The gas pressure of the high-pressure inert atmosphere is 160-200 MPa; The hot isostatic pressing sintering time is 0.5 to 6 hours.

10. The method for preparing yttrium-magnesium composite transparent ceramics by non-aqueous gelcasting according to any one of claims 1 to 9, characterized in that: In step C, the annealing condition is in air atmosphere, 1000-1400° C. for 10-80 hours.

Citation Information

Patent Citations

  • Method for preparing alumina-based ceramic material by environmentally-friendly gelcasting

    CN101698607A

  • Method for precisely shaping non-water-base injection molding gel of ceramic body

    CN102085688A

  • Responsive gel casting formation method

    CN102249691A

  • Method for preparing Y3Al5O12 transparent ceramics by using gelcasting and reactive sintering

    CN105218095A

  • Method for producing garnet-based transparent ceramic through non-aqueous gel casting molding

    CN107540367A

Cited By

  • Yttrium-magnesium multiphase transparent ceramic with high etching resistance as well as preparation method and application of yttrium-magnesium multiphase transparent ceramic