Sealing treatment method for carbon fiber reinforced composite material

Through the impregnation and high-temperature cracking process of low-viscosity ceramic precursor solution, the carbon fiber reinforced composite material is processed multiple times to solve the problems of internal pore filling and surface sealing, and achieve the improvement of high sealing performance, which is suitable for the aerospace field. Extreme environments.

CN118754697APending Publication Date: 2024-10-11AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410991777.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Carbon fiber reinforced composite materials have high porosity due to limitations in the preparation process. Existing sealing technologies mainly focus on surface treatment and cannot meet the demand for high sealing performance in the aerospace field, especially in extreme service environments.

Method used

The low-viscosity ceramic precursor solution is used for vacuum impregnation, pressure impregnation, pressure curing and high-temperature cracking, and the carbon fiber reinforced composite material is sealed several times to fill its internal pores.

Benefits of technology

It achieves uniform sealing of the surface and interior of carbon fiber reinforced composite materials, improves the sealing effect, meets the high sealing performance requirements in the aerospace field, and can adjust the number of repetitions according to actual needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754697A_ABST
    Figure CN118754697A_ABST
Patent Text Reader

Abstract

The invention provides a carbon fiber reinforced composite material sealing treatment method, and belongs to the technical field of carbon fiber reinforced composite material sealing treatment.The sealing treatment method comprises the steps that S1, a ceramic precursor solution is adopted to conduct vacuum impregnation and pressure impregnation on a carbon fiber reinforced composite material in sequence; s2, pressurizing, curing and cracking the impregnated carbon fiber reinforced composite material; and S3, the step S1 and the step S2 are repeated for multiple times, and sealing treatment is completed. According to the sealing treatment method provided by the invention, not only can the surface of the carbon fiber reinforced composite material be sealed, but also internal pores of the carbon fiber reinforced composite material can be fully filled, so that a good sealing effect is achieved; and the requirement of the carbon fiber reinforced composite material for high sealing performance in a special extreme service environment in the aerospace field can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing treatment of carbon fiber reinforced composite materials, in particular to a sealing treatment method of carbon fiber reinforced composite materials. Background Art

[0002] Carbon fiber reinforced composite materials generally have a high porosity due to their preparation process limitations. However, there are few studies on the sealing of carbon fiber reinforced composite materials, which cannot meet the use requirements in special extreme service environments in the aerospace field. Chinese patent application CN112844999 A uses penetration sealant, polysulfide sealant, polyurethane varnish and curing agent to seal the surface of C / C throat liner composite materials. However, this method only seals the surface of the composite material and has poor stability. Summary of the invention

[0003] In response to one or more technical problems existing in the prior art, the present invention provides a sealing treatment method for carbon fiber reinforced composite materials. The sealing treatment method provided by the present invention can not only seal the surface of the carbon fiber reinforced composite materials, but also fully fill the internal pores of the carbon fiber reinforced composite materials, and has a good sealing effect. It can meet the requirements of carbon fiber reinforced composite materials for high sealing performance in special extreme service environments in the aerospace field.

[0004] The present invention provides a sealing treatment method for a carbon fiber reinforced composite material, the sealing treatment method comprising the following steps:

[0005] S1. vacuum impregnation and pressure impregnation of a carbon fiber reinforced composite material are performed sequentially using a ceramic precursor solution; the room temperature viscosity of the ceramic precursor solution is not higher than 30 mPa·s;

[0006] S2. Pressurizing and curing the impregnated carbon fiber reinforced composite material and cracking it;

[0007] S3. Repeat steps S1 and S2 multiple times to complete the sealing process.

[0008] Preferably, the ceramic precursor solution is a silicon carbide ceramic precursor solution.

[0009] Preferably, the carbon fiber reinforced composite material is one of a C / C composite material and a ceramic-based composite material.

[0010] Preferably, the vacuum degree of the vacuum impregnation is -0.15 to -0.08 MPa;

[0011] The vacuum impregnation temperature is room temperature; and / or

[0012] The vacuum impregnation time is 0.5 to 2 hours.

[0013] Preferably, the pressure of the pressure impregnation is 0.5-2 MPa;

[0014] The pressure impregnation temperature is room temperature; and / or

[0015] The pressure impregnation time is 0.5 to 2 hours.

[0016] Preferably, the temperature of the pressurized curing is 100 to 350°C;

[0017] The pressure of the pressurized curing is 0.5 to 2.5 MPa; and / or

[0018] The time of pressurized curing is 0.5 to 2 hours.

[0019] Preferably, the pyrolysis temperature is 900-1500°C; and / or

[0020] The lysis time is 2 to 4 hours.

[0021] Preferably, step S1 and step S2 are repeated 5 to 20 times.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] The present invention adopts a low-viscosity ceramic precursor solution impregnation and cracking process to sequentially perform vacuum impregnation, pressure impregnation, pressure curing and high-temperature cracking on the carbon fiber reinforced composite material, and repeats the above steps for multiple times to seal the carbon fiber reinforced composite material. The sealing treatment method can not only seal the surface of the carbon fiber reinforced composite material, but also fully fill the internal pores of the carbon fiber reinforced composite material, and has a good sealing effect. It can meet the demand for high sealing performance of carbon fiber reinforced composite materials in special extreme service environments in the aerospace field. At the same time, the number of repetitions can be adjusted according to actual use requirements to meet different needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 is a cross-sectional microstructure diagram of a sample after sealing treatment in Example 1 of the present invention;

[0026] Figure 2 This is a partial internal microstructure diagram of a sample after sealing treatment in Example 1 of the present invention;

[0027] Figure 3 This is another partial internal microstructure diagram of the sample after sealing treatment in Example 1 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] The present invention provides a sealing treatment method for a carbon fiber reinforced composite material, the sealing treatment method comprising the following steps:

[0030] S1. vacuum impregnation and pressure impregnation of a carbon fiber reinforced composite material are performed sequentially using a ceramic precursor solution; the room temperature viscosity of the ceramic precursor solution is not higher than 30 mPa·s;

[0031] S2. Pressurizing and curing the impregnated carbon fiber reinforced composite material and cracking it;

[0032] S3. Repeat steps S1 and S2 multiple times to complete the sealing process.

[0033] The present invention adopts a low-viscosity ceramic precursor solution impregnation and cracking process to sequentially perform vacuum impregnation, pressure impregnation, pressure curing and high-temperature cracking on the carbon fiber reinforced composite material, and repeats the above steps for multiple times to seal the carbon fiber reinforced composite material. The sealing treatment method can not only seal the surface of the carbon fiber reinforced composite material, but also fully fill the internal pores of the carbon fiber reinforced composite material, and has a good sealing effect. It can meet the demand for high sealing performance of carbon fiber reinforced composite materials in special extreme service environments in the aerospace field. At the same time, the number of repetitions can be adjusted according to actual use requirements to meet different needs.

[0034] According to some preferred embodiments, the ceramic precursor solution is a silicon carbide ceramic precursor solution.

[0035] According to some preferred embodiments, the carbon fiber reinforced composite material is one of a C / C composite material and a ceramic-based composite material.

[0036] According to some preferred embodiments, the vacuum degree of the vacuum impregnation is -0.15 to -0.08 MPa (for example, it may be -0.15 MPa, -0.14 MPa, -0.13 MPa, -0.12 MPa, -0.11 MPa, -0.10 MPa, -0.09 MPa or -0.08 MPa).

[0037] According to some preferred embodiments, the vacuum impregnation temperature is room temperature.

[0038] According to some preferred embodiments, the vacuum impregnation time is 0.5 to 2 h (eg, 0.5 h, 1 h, 1.5 h or 2 h).

[0039] According to some preferred embodiments, the pressure of the pressure impregnation is 0.5-2 MPa (for example, it may be 0.5 MPa, 0.6 MPa, 0.8 MPa, 1 MPa, 1.2 MPa, 1.5 MPa, 1.6 MPa, 1.8 MPa or 2 MPa).

[0040] According to some preferred embodiments, the pressure impregnation temperature is room temperature.

[0041] According to some preferred embodiments, the pressure impregnation time is 0.5 to 2 hours (for example, 0.5 hours, 1 hour, 1.5 hours or 2 hours).

[0042] According to some preferred embodiments, the temperature of the pressurized curing is 100 to 350° C. (for example, it may be 100° C., 150° C., 200° C., 250° C., 300° C. or 350° C.);

[0043] According to some preferred embodiments, the pressure of the pressurized curing is 0.5-2.5 MPa (for example, it may be 0.5 MPa, 0.6 MPa, 0.8 MPa, 1 MPa, 1.2 MPa, 1.5 MPa, 1.6 MPa, 1.8 MPa, 2 MPa, 2.2 MPa or 2.5 MPa).

[0044] According to some preferred embodiments, the pressurized curing time is 0.5 to 2 hours (for example, 0.5 hours, 1 hour, 1.5 hours or 2 hours).

[0045] According to some preferred embodiments, the cracking temperature is 900-1500°C (for example, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C or 1500°C).

[0046] According to some preferred embodiments, the lysis time is 2 to 4 h (eg, 2 h, 2.5 h, 3 h, 3.5 h or 4 h).

[0047] According to some preferred embodiments, the number of times step S1 and step S2 are repeated is 5 to 20 times. The present invention can select different repetition times according to the sealing requirements.

[0048] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the embodiments. The present invention does not specifically limit the sources of the reagents used in the embodiments and comparative examples, and they can be directly purchased or synthesized by themselves. It should be noted that there will be deviations in the viscosity test of the silicon carbide ceramic precursor solution, resulting in the viscosity value measured each time may not be a fixed value, and will fluctuate within a certain range. Therefore, the silicon carbide ceramic precursor solution in the embodiment of the present invention is expressed by a range.

[0049] Example 1

[0050] A sealing treatment method for a carbon fiber reinforced composite material comprises the following steps:

[0051] S1. The C / C composite material sample is vacuum impregnated and pressure impregnated in sequence using a silicon carbide ceramic precursor solution with a room temperature viscosity of 10 to 20 mPa·s, wherein the vacuum degree of the vacuum impregnation is -0.1 MPa, the temperature of the vacuum impregnation is room temperature, and the vacuum impregnation time is 1.0 h; the pressure of the pressure impregnation is 2.0 MPa, the temperature of the pressure impregnation is room temperature, and the pressure impregnation time is 2.0 h;

[0052] S2. The impregnated C / C composite material sample is subjected to pressurized curing and high-temperature pyrolysis, wherein the pressurized curing temperature is 300°C, the pressurized curing pressure is 2.0MPa, and the pressurized curing time is 2.0h; the pyrolysis temperature is 1000°C, and the pyrolysis time is 2.0h;

[0053] S3. Repeat steps S1 and S2 15 times to complete the sealing process of the C / C composite material.

[0054] The microstructure of the C / C composite material sample after sealing treatment in this embodiment is as follows: Figure 1-3 As shown in the figure, the pores inside the matrix of the sealed C / C composite material are fully filled and a dense matrix structure is formed.

[0055] The C / C composite material sample treated in this embodiment was subjected to a room temperature airtightness drainage test (pressure of 0.5 MPa, time of 10 minutes), and the pressure drop of the sealed sample was 0.001 MPa.

[0056] Example 2

[0057] A sealing treatment method for a carbon fiber reinforced composite material comprises the following steps:

[0058] S1. The C / C composite material samples were vacuum impregnated and pressurized in turn using a silicon carbide ceramic precursor solution with a room temperature viscosity of 20 to 30 mPa·s, wherein the vacuum degree of the vacuum impregnation was -0.1 MPa, the temperature of the vacuum impregnation was room temperature, and the vacuum impregnation time was 1.0 h; the pressure of the pressure impregnation was 2.0 MPa, the temperature of the pressure impregnation was room temperature, and the pressure impregnation time was 2.0 h;

[0059] S2. The impregnated C / C composite material sample is subjected to pressurized curing and high-temperature pyrolysis, wherein the pressurized curing temperature is 300°C, the pressurized curing pressure is 2.0MPa, and the pressurized curing time is 2.0h; the pyrolysis temperature is 1000°C, and the pyrolysis time is 2.0h;

[0060] S3. Repeat steps S1 and S2 13 times to complete the sealing process of the C / C composite material.

[0061] The C / C composite material sample treated in this embodiment was subjected to a room temperature airtightness drainage test (pressure of 0.5 MPa, time of 10 minutes), and the pressure drop of the sealed sample was 0.006 MPa.

[0062] Example 3

[0063] A sealing treatment method for a carbon fiber reinforced composite material comprises the following steps:

[0064] S1. The C / ZrC-SiC composite material samples were vacuum impregnated and pressure impregnated in sequence using a silicon carbide ceramic precursor solution with a room temperature viscosity of 10 to 20 mPa·s, wherein the vacuum degree of the vacuum impregnation was -0.1 MPa, the temperature of the vacuum impregnation was room temperature, and the time of the vacuum impregnation was 1.0 h; the pressure of the pressure impregnation was 2.0 MPa, the temperature of the pressure impregnation was room temperature, and the time of the pressure impregnation was 2.0 h;

[0065] S2. The impregnated C / ZrC-SiC composite material sample is subjected to pressurized curing and high-temperature pyrolysis, wherein the pressurized curing temperature is 300°C, the pressurized curing pressure is 2.0MPa, and the pressurized curing time is 2.0h; the pyrolysis temperature is 1000°C, and the pyrolysis time is 2.0h;

[0066] S3. Repeat steps S1 and S2 12 times to complete the sealing process of the C / ZrC-SiC composite material.

[0067] The C / ZrC-SiC composite material sample treated in this embodiment was subjected to a room temperature airtightness drainage test (pressure of 0.5 MPa, time of 10 minutes), and the pressure drop of the sealed sample was 0.003 MPa.

[0068] Example 4

[0069] A sealing treatment method for a carbon fiber reinforced composite material comprises the following steps:

[0070] S1. The C / ZrC-SiC composite material samples were vacuum impregnated and pressure impregnated in sequence using a silicon carbide ceramic precursor solution with a room temperature viscosity of 20 to 30 mPa·s, wherein the vacuum degree of the vacuum impregnation was -0.1 MPa, the temperature of the vacuum impregnation was room temperature, and the vacuum impregnation time was 1.0 h; the pressure of the pressure impregnation was 2.0 MPa, the temperature of the pressure impregnation was room temperature, and the pressure impregnation time was 2.0 h;

[0071] S2. The impregnated C / ZrC-SiC composite material sample is subjected to pressurized curing and high-temperature pyrolysis, wherein the pressurized curing temperature is 300°C, the pressurized curing pressure is 2.0MPa, and the pressurized curing time is 2.0h; the pyrolysis temperature is 1000°C, and the pyrolysis time is 2.0h;

[0072] S3. Repeat steps S1 and S2 13 times to complete the sealing process of the C / ZrC-SiC composite material.

[0073] The C / ZrC-SiC composite material sample treated in this embodiment was subjected to a room temperature airtightness drainage test (pressure of 0.5 MPa, time of 10 minutes), and the pressure drop of the sealed sample was 0.007 MPa.

[0074] Comparative Example 1

[0075] S1. The C / C composite material samples were vacuum impregnated and pressurized in turn using a silicon carbide ceramic precursor solution with a room temperature viscosity of 70 to 80 mPa·s, wherein the vacuum degree of the vacuum impregnation was -0.1 MPa, the temperature of the vacuum impregnation was room temperature, and the vacuum impregnation time was 1.0 h; the pressure of the pressure impregnation was 2.0 MPa, the temperature of the pressure impregnation was room temperature, and the pressure impregnation time was 2.0 h;

[0076] S2. The impregnated C / C composite material sample is subjected to pressurized curing and high-temperature pyrolysis, wherein the pressurized curing temperature is 300°C, the pressurized curing pressure is 2.0MPa, and the pressurized curing time is 2.0h; the pyrolysis temperature is 1000°C, and the pyrolysis time is 2.0h;

[0077] S3. Repeat steps S1 and S2 15 times to complete the sealing process of the C / C composite material.

[0078] The C / C composite material sample treated in this embodiment was subjected to a room temperature airtightness drainage test (pressure of 0.5 MPa, time of 10 minutes), and the pressure drop of the sealed sample was 0.5 MPa.

[0079] Comparative Example 2

[0080] A sealing treatment method for a carbon fiber reinforced composite material comprises the following steps:

[0081] S1. The C / ZrC-SiC composite material samples were vacuum impregnated and pressure impregnated in sequence using a silicon carbide ceramic precursor solution with a room temperature viscosity of 70 to 80 mPa·s, wherein the vacuum degree of the vacuum impregnation was -0.1 MPa, the temperature of the vacuum impregnation was room temperature, and the vacuum impregnation time was 1.0 h; the pressure of the pressure impregnation was 2.0 MPa, the temperature of the pressure impregnation was room temperature, and the pressure impregnation time was 2.0 h;

[0082] S2. The impregnated C / ZrC-SiC composite material sample is subjected to pressurized curing and high-temperature pyrolysis, wherein the pressurized curing temperature is 300°C, the pressurized curing pressure is 2.0MPa, and the pressurized curing time is 2.0h; the pyrolysis temperature is 1000°C, and the pyrolysis time is 2.0h;

[0083] S3. Repeat steps S1 and S2 12 times to complete the sealing process of the C / ZrC-SiC composite material.

[0084] The C / ZrC-SiC composite material sample treated in this embodiment was subjected to a room temperature airtightness drainage test (pressure of 0.5 MPa, time of 10 minutes), and the pressure drop of the sealed sample was 0.5 MPa.

[0085] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for sealing a carbon fiber reinforced composite material, characterized in that: The sealing treatment method comprises the following steps: S1. vacuum impregnation and pressure impregnation of a carbon fiber reinforced composite material are performed sequentially using a ceramic precursor solution; the room temperature viscosity of the ceramic precursor solution is not higher than 30 mPa·s; S2. Pressurizing and curing the impregnated carbon fiber reinforced composite material and cracking it; S3. Repeat steps S1 and S2 multiple times to complete the sealing process.

2. The sealing method according to claim 1, characterized in that: The ceramic precursor solution is a silicon carbide ceramic precursor solution.

3. The sealing method according to claim 1, characterized in that: The carbon fiber reinforced composite material is one of a C / C composite material and a ceramic-based composite material.

4. The sealing method according to claim 1, characterized in that: The vacuum degree of the vacuum impregnation is -0.15 to -0.08 MPa; The vacuum impregnation temperature is room temperature; and / or The vacuum impregnation time is 0.5 to 2 hours.

5. The sealing method according to claim 1, characterized in that: The pressure of the pressure impregnation is 0.5-2MPa; The pressure impregnation temperature is room temperature; and / or The pressure impregnation time is 0.5 to 2 hours.

6. The sealing method according to claim 1, characterized in that: The temperature of the pressurized curing is 100 to 350°C; The pressure of the pressurized curing is 0.5 to 2.5 MPa; and / or The time of pressurized curing is 0.5 to 2 hours.

7. The sealing method according to claim 1, characterized in that: The cracking temperature is 900-1500°C; and / or The lysis time is 2 to 4 hours.

8. The sealing method according to claim 1, characterized in that: The number of times of repeating step S1 and step S2 is 5 to 20 times.

Citation Information

Patent Citations

  • Preparation method of silicon carbide and silicon carbide composite material member

    CN103387405A

  • Preparation method of binary ceramic modified carbon / carbon composite

    CN103910533A

  • Composite densification method of SiC-based composite material precursors at different states through dipping cracking

    CN109180194A

  • C / SiC-ZrC multiphase ceramic matrix composite and preparation method thereof

    CN110776320A

  • Preparation method of composite material, composite material impregnation equipment and container

    CN111056845A