High-efficiency dark blue photo-thermal exciton compound with circular polarization property and application of high-efficiency dark blue photo-thermal exciton compound in preparation of organic electroluminescent device
By designing thermal exciton materials with arylimidazole groups, we solve the problems of exciton utilization and efficiency roll-off of existing circularly polarized luminescent materials, and achieve high-efficiency deep blue light emission and low-efficiency roll-off organic electroluminescence. The device simplifies the device structure and reduces the cost, and has application potential for 3D and wide color gamut displays.
Patent Information
- Application Number
- CN202410815818.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-11
AI Technical Summary
Existing circularly polarized luminescent materials have deficiencies in exciton utilization and efficiency roll-off, making it difficult to achieve high-efficiency, low-efficiency roll-off deep blue light emission, and suffer from structural complexity and high cost.
By designing thermal excitonic materials with arylimidazole groups (such as (R/S)-PPI-OBN-CN and (R/S)-PyI-OBN-CN) and combining chiral groups, high-performance Efficient deep-blue photothermal exciton compounds are used to prepare organic electroluminescent devices with circular polarization properties, achieving high fluorescence quantum yield and low efficiency roll-off.
It achieves high-efficiency deep blue light emission, significantly improves exciton utilization and photoluminescence performance, reduces device structure complexity and cost, and has potential applications in 3D and wide color gamut displays.
Smart Images

Figure CN118754881A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of organic photoelectric materials, and in particular relates to a high-efficiency deep blue light thermoexciton compound with circular polarization properties and an application thereof in preparing an organic electroluminescent device. Background Art
[0002] Organic light-emitting diodes (OLEDs) have the advantages of ultra-thinness, flexibility, self-luminescence, and fast response. They have made rapid progress in the fields of full-color display and solid-state lighting, and are regarded as a new generation of ideal information display technology. OLEDs prepared from current materials often require the use of linear polarizers and quarter-wave plates to convert circularly polarized light to obtain higher image contrast. However, this method reduces the luminous brightness and light output efficiency, and also increases the complexity of the device structure. In addition, circularly polarized luminescence (CPL) has great application potential in optoelectronic applications such as chiral sensing, optical data storage, bio-responsive imaging, spintronics optical communications, and 3D displays, and has attracted much attention. Therefore, designing chiral non-racemic luminescent materials that can directly emit circularly polarized luminescence has become the focus of current research.
[0003] OLED technology is mainly used for full-color display and white light illumination. Full-color display is achieved by controlling the pixels of three different colors: red, green, and blue. White light illumination is achieved by matching red, green, blue or orange light and blue light. Whether it is full-color display or white light illumination, blue light is an indispensable light color. The darker the blue light color, the more energy-efficient the white light illumination is. In addition, high-efficiency deep blue light materials can not only provide blue light, one of the three primary colors, but also, due to their higher energy, can be used as a matrix or backlight source to excite other dyes to emit light, thereby simplifying the device structure and reducing production costs. Therefore, the development of high-efficiency deep blue light circularly polarized OLEDs is of great guiding significance for reducing the cost of OLEDs and promoting their practical application.
[0004] Materials are the core of OLEDs technology. At present, circularly polarized luminescent materials mainly include chiral fluorescent materials, polymers, transition metal complexes, phosphorescent materials and thermally activated delayed fluorescence (TADF) materials. Due to the limitation of spin statistics, the exciton utilization rate of traditional fluorescent materials is only 25%. In phosphorescent materials based on precious metal complexes, due to the spin-orbit coupling effect, triplet excitons can also emit light through radiative transitions, and the exciton utilization rate can reach 100%. However, phosphorescent materials still face problems such as high material cost and short life of blue light devices. TADF materials can also achieve very high device efficiency, but the strong charge transfer state characteristics between donors and acceptors make it difficult to achieve blue and deep blue light emission (CIEy < 0.15). On the other hand, due to the long lifetime of triplet excitons involved in radiative transitions in phosphorescent and TADF materials, they are easily accumulated at high current density, leading to exciton annihilation, resulting in serious efficiency roll-off, affecting the practical application of circularly polarized materials.
[0005] The hot exciton mechanism was first proposed by Ma Yuguang's research group in the world. Its core idea is to generate high-energy triplet states (T n , n≥2) to the singlet state (S m , m≥1) to improve the utilization rate of excitons. Theoretically, hot exciton materials can also utilize all excitons, and the excited state does not require the charge transfer state to dominate, and there is no participation of long-lived triplet excitons. Therefore, it is expected to achieve high-efficiency, low-efficiency roll-off deep blue light materials. The present invention proposes to develop new circularly polarized hot exciton deep blue light materials and devices by combining molecular design with chemical synthesis, taking into account the dual advantages of circularly polarized luminescence and high luminescence efficiency, which is conducive to the direct realization of 3D and wide color gamut display in the future. Summary of the invention
[0006] To this end, the purpose of the present invention is to provide a high-efficiency deep blue light thermoexciton compound with circular polarization properties, which is used as a high-efficiency, low roll-off deep blue light OLED device prepared as a light-emitting layer and has the potential for practical application.
[0007] To achieve the above-mentioned purpose, the present invention provides a high-efficiency deep blue light-induced thermal exciton compound with circular polarization properties, the structural formula of which is shown as one of the following:
[0008]
[0009] The above-mentioned deep blue photothermal exciton material with circular polarization property provided by the present invention integrates high luminous efficiency, high exciton utilization rate, significant circular polarization property and excellent electroluminescent performance.
[0010] The principle of the present invention is that the aryl imidazole group has been confirmed to be a classic structure for constructing thermoexciton materials, showing many advantages such as high solution and film photoluminescence efficiency, excellent photothermal stability, suitable electronic energy level, relatively balanced carrier injection and transmission ability, simple preparation method, and convenient structure regulation. By combining the characteristics of chiral groups and thermoexciton materials, two pairs of deep blue light enantiomers, namely (R / S)-PPI-OBN-CN and (R / S)-PyI-OBN-CN, were successfully designed and synthesized. They have high fluorescence quantum yields and obvious circularly polarized luminescence properties. The asymmetry factors in the non-doped film are +8.78×10 -4 / -1.74×10 -3 and +2.63×10 -3 / -1.19×10 -3The electroluminescent devices prepared based on the enantiomers (R / S)-PPI-OBN-CN and (R / S)-PyI-OBN-CN have deep blue emission with CIE coordinates of (0.15, 0.08) and (0.15, 0.14) at a brightness of 100 cd m -2 and 439cd m -2 The external quantum efficiency reaches its maximum value at 1000 cdm, and the maximum values are 7.25% and 8.11% respectively. In addition, (R / S)-PyI-OBN-CN has a very low efficiency roll-off. -2 The high external quantum efficiency of 7.96% is maintained at a brightness of up to 10000cd m -2 The external quantum efficiency of 6.68% is maintained at high brightness. This work provides a new perspective for the development of deep blue light-thermal exciton materials with circularly polarized luminescence, high efficiency and low roll-off, which is conducive to the direct realization of 3D and wide color gamut displays in the future.
[0011] The deep blue light thermoexciton material with circular polarization property described in the present invention can be used in preparing circular polarization organic electroluminescent devices.
[0012] The organic electroluminescent device is composed of a transparent glass substrate, an ITO conductive film anode, an organic functional layer including an organic light-emitting layer, and a cathode. The deep blue light thermal exciton material with circular polarization properties described in the present invention is used as a doping guest to prepare the organic light-emitting layer. The organic functional layer is a sequential structure of one or more of a hole injection layer, a hole transport layer, and an exciton blocking layer, an organic light-emitting layer, an electron transport layer, and an electron injection layer. The doping subject of the organic light-emitting layer is CBP, and the doping mass concentration of the doping guest is 15-25%. The circularly polarized organic electroluminescent device can be used to prepare a deep blue light circularly polarized organic electroluminescent display or an organic electroluminescent lighting source. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 : A schematic structural diagram of an organic electroluminescent device prepared by the present invention, in which 1 is a transparent glass substrate, 2 is an ITO conductive film anode, 3 is a hole injection layer, 4 is a hole transport layer, 5 is an exciton blocking layer, 6 is an organic light-emitting layer, 7 is an electron transport layer, and 8 is a cathode;
[0014] Figure 2 The absorption and emission spectra of (R)-PPI-OBN-CN and (R)-PyI-OBN-CN in THF solution are shown in Figure 2. The main absorption peaks are located at 365nm and 385nm respectively; the main emission peaks are located at 420nm and 430nm, which are deep blue light emissions. They can be used as organic deep blue light materials to prepare electroluminescent devices.
[0015] Figure 3is the circularly polarized photoluminescence spectrum of (R / S)-PPI-OBN-CN in the undoped thin film state ( Figure 3 a), the main peak is at 460nm, which is the emission of positive blue light; and the photoluminescence asymmetry factor curve ( Figure 3 b), is +8.78×10 -4 / -1.74×10 -3 .
[0016] Figure 4 is the circularly polarized photoluminescence spectrum of (R / S)-PyI-OBN-CN in the undoped thin film state ( Figure 4 a), the main peak is at 470nm, which is the emission of sky blue light; and the photoluminescence asymmetry factor curve ( Figure 4 a), is +2.63×10 -3 / -1.19×10 -3 .
[0017] Figure 5 The external quantum efficiency curve of the (R / S)-PPI-OBN-CN circularly polarized electroluminescent device prepared in Example 3 is shown in FIG. 1 . The maximum external quantum efficiency is 7.25% at 1000 cd m -2 It still maintains a high external quantum efficiency of 5.97% at a brightness of 6V; the inset is the electroluminescence spectrum of the device under a driving voltage of 6V, and the main peak of the spectrum is located at 436nm, which is the emission of deep blue light.
[0018] Figure 6 The external quantum efficiency curve of the (R / S)-PyI-OBN-CN circularly polarized electroluminescent device prepared in Example 4 is shown in FIG. 1 . The maximum external quantum efficiency is 8.11% at 1000 cd m -2 It still maintains a high external quantum efficiency of 7.96% at a brightness of 6V; the inset is the electroluminescence spectrum of the device under a driving voltage of 6V, and the main peak of the spectrum is at 452nm, which is the emission of positive blue light. DETAILED DESCRIPTION
[0019] Example 1: This example is the preparation of (R / S)-PPI-OBN-CN, and the steps are as follows:
[0020] Synthesis of PPIBr: 9,10-phenanthrenequinone (2.08 g, 10 mmol), aniline (3.73 g, 40 mmol), ammonium acetate (4.01 g, 50 mmol), 4-bromobenzaldehyde (1.85 g, 10 mmol) and acetic acid (80 mL) were added to a 250 mL round-bottom flask and stirred at 120 ° C for 6 hours under nitrogen protection. After the reaction, the mixture was poured into ice water and then filtered to obtain a crude product as a grass green solid, which was washed with acetic acid, water and ethanol in turn, and then further purified by column chromatography using a mixed eluent of dichloromethane / petroleum ether (volume ratio of 1:1), and a white powder was obtained after spin drying with a yield of 80%. Mass spectrum MALDI-TOF (m / z) [M + ]: The measured value is 449.33 and the theoretical value is 449.01.
[0021]
[0022] Synthesis of PPIB: PPIBr (2.25 g, 5 mmol), pinacol diboron (2.54 g, 10 mmol), potassium acetate (1.47 g, 15 mmol), (1,1'-bis(diphenylphosphino)ferrocene)palladium dichloride (0.12 g, 0.15 mmol), and 50 mL of dioxane were added to a 100 mL round-bottom flask. Stir and reflux at 85 °C for 72 hours in a nitrogen atmosphere. After the reaction, V 水 :V 二氯甲烷 =1:1 multiple extractions, the organic phase was collected and concentrated, and then further purified by column chromatography using a mixed eluent of dichloromethane / petroleum ether (volume ratio of 2:1), and a white powder was obtained after spin drying with a yield of 52%. Mass spectrum MALDI-TOF (m / z) [M + ]: The measured value is 496.63 and the theoretical value is 496.23.
[0023]
[0024] Synthesis of (R / S)-OBN-CN: 2-bromo-4,5-difluorobenzonitrile (305.2 mg, 1.4 mmol), (R / S)-binaphthol (400.4 mg, 1.4 mmol) and potassium carbonate (483 mg, 3.5 mmol) were mixed, and 20 mL of anhydrous DMF was added, heated to 120 ° C and stirred for 12 hours. After cooling to room temperature, the reaction mixture was poured into water (100 mL), extracted with dichloromethane and water, and the combined organic layers were condensed in vacuo, and then further purified by column chromatography with a mixed eluent of dichloromethane / petroleum ether (volume ratio of 1:2), and a white solid (422 mg) was obtained after spin drying with a yield of 65%. Mass spectrum MALDI-TOF (m / z) [M+ ]: The measured value is 464.12 and the theoretical value is 464.3.
[0025]
[0026] Synthesis of (R / S)-PPI-OBN-CN: (R / S)-OBN-CN (464 mg, 1 mmol), PPIB (496 mg, 1 mmol), K2CO3 (2.76 g, 20 mmol), Pd(PPh3)4 (23 mg, 0.02 mmol) were mixed and added to a 100 mL flask, and then 20 mL toluene and 10 mL water were added, heated to 90 ° C and stirred for 12 hours. After cooling to room temperature, the reaction mixture was poured into water (100 mL), extracted with dichloromethane and water, and the combined organic layers were condensed in vacuo, and then further purified by column chromatography using a mixed eluent of dichloromethane / petroleum ether (volume ratio of 1:4), and a white solid (560 mg) was obtained after spin drying with a yield of 74%.
[0027] (R)-PPI-OBN-CN: 1 H NMR (500MHz, CDCl3) δ (ppm): 8.94 (d, J = 7.3Hz, 1H), 8.81 (d, J = 8.4Hz, 1H), 8.74 (d, J = 8.3Hz, 1H), 8.04 (t, J = 8.8Hz, 2H), 8.02–7.97 (m, 2H), 7. 78(m,3H),7.69(m,5H),7.60(d,J=2.5Hz,2H),7.58–7.50(m,7H),7.45(dt,J=15.2,6.6Hz,4H),7.29(d,J=7.5Hz,2H),7.22(d,J=8.2Hz,1H). 13 C NMR (126MHz, CDCl3) δ (ppm): 152.33, 150.39, 150.23, 149.85, 147.98, 141.99, 138.63, 137.25, 132.18, 131.95, 131.03, 130.38, 130.08, 129.6 2,129.44,129.10,128.51,128.06,127.39,127.11,126.67,126.35,12 5.84,125.42,125.07,124.18,123.66,123.32,120.89,117.72,106.60.
[0028] (S)-PPI-OBN-CN: 1H NMR (500MHz, CDCl3) δ (ppm): 8.94 (s, 1H), 8.81 (d, J = 8.3Hz, 1H), 8.74 (d, J = 8.2Hz, 1H), 8.13–7.96 (m, 4H), 7.78 (m, 3H), 7. 74–7.65(m,5H),7.57(dt,J=13.0,5.8Hz,9H),7.45(dt,J=15.1,6.6Hz,4H),7.29(d,J=6.4Hz,2H),7.22(d,J=8.3Hz,1H). 13 C NMR (126 MHz, CDCl3) δ (ppm): 152.33, 150.31, 147.98, 141.99, 138.65, 137.24, 132.18, 131.98, 131.03, 130.38, 130.08, 129.63, 129.44, 129.11, 128.51, 128.07, 127.40, 127.11, 126.67, 126.35, 125.84, 125.47, 125.07, 124.18, 123.52, 120.89, 117.72. Mass Spectrometry MALDI-TOF (m / z) [M + ]: The measured value is 753.86 and the theoretical value is 753.68.
[0029]
[0030] Example 2: This example is the preparation of (R / S)-PyI-OBN-CN, and the steps are as follows:
[0031] Synthesis of 4,5-pyrene diquinone: Elemental pyrene (4.0 g, 20 mmol) was dissolved in a mixed organic solvent of 80 mL of dichloromethane and 80 mL of acetonitrile, then sodium periodate (17.5 g, 81.8 mmol) and 100 mL of purified water were added, and finally the catalyst RuCl3·xH2O (0.5 g, 2.4 mmol) was added. The two-phase reaction system was stirred at room temperature overnight. After the reaction was completed, the reactant was extracted with a large amount of dichloromethane and a small amount of water. The organic phase was dried with anhydrous magnesium sulfate for several hours and then filtered. The filtrate was concentrated by a rotary evaporator, and then further purified by column chromatography using a mixed eluent of dichloromethane / petroleum ether (volume ratio of 1:2). After spin drying, the product obtained a red powder (1.5 g) with a yield of 32%. Mass spectrum MALDI-TOF (m / z) [M + ]: The measured value is 2321 and the theoretical value is 23232.
[0032]
[0033] Synthesis of PyIBr: Place appropriate amounts of pyrene diquinone (1.2 g, 5.0 mmol), 4-bromobenzaldehyde (1.2 g, 6.0 mmol), aniline (2.3 mL), ammonium acetate (1.5 g, 20.0 mmol) and 15 mL of glacial acetic acid in a 50 mL round-bottom flask and degas once. Heat the entire reaction system to 120 ° C and reflux for 2 hours. After the reaction is completed, cool to room temperature and add 10 mL of water to precipitate the product and filter it. Wash the filtered dark solid with water and acetic acid (volume ratio 1:1), and then use a mixed eluent of dichloromethane / petroleum ether (volume ratio 1:1) to further purify it by column chromatography. After spin drying, 2.04 g of white powder is obtained with a yield of 86%. Mass spectrum MALDI-TOF (m / z) [M + ]: The measured value is 472.5 and the theoretical value is 472.67.
[0034]
[0035] Synthesis of PyIB: PyIBr (2.37 g, 5 mmol), bipyraclostrobin (2.54 g, 10 mmol), potassium acetate (1.47 g, 15 mmol), [1,1'-bis(diphenylphosphino)ferrocene] palladium dichloride (0.12 g, 0.15 mmol), and 50 mL of dioxane were added to a 100 mL round-bottom flask. Stir and reflux at 85 °C for 72 hours under nitrogen. After the reaction, use V 水 :V 二氯甲烷 =1:1 multiple extractions, the organic phase was collected and concentrated, and then further purified by column chromatography using a mixed eluent of dichloromethane / petroleum ether (volume ratio of 1:1), and a white powder was obtained after spin drying with a yield of 52%. Mass spectrum MALDI-TOF (m / z) [M + ]: The measured value is 520.26 and the theoretical value is 520.44.
[0036]
[0037] Synthesis of (R / S)-PyI-OBN-CN: (R / S)-OBN-CN (464 mg, 1 mmol), PyIB (520 mg, 1 mmol), K2CO3 (2.76 g, 20 mmol), Pd(PPh3)4 (23 mg, 0.02 mmol) were mixed and added to a 100 mL flask, and then 20 mL toluene and 10 mL water were added, heated to 90 ° C and stirred for 12 hours. After cooling to room temperature, the reaction mixture was poured into water (100 mL), extracted with dichloromethane and water, and the combined organic layer was condensed in vacuo, and then further purified by column chromatography using a mixed eluent of dichloromethane / petroleum ether (volume ratio of 1:4), and a white solid (560 mg) was obtained after spin drying with a yield of 74%.
[0038] (R)-PyI-OBN-CN: 1 H NMR (500MHz, CDCl3) δ (ppm): 8.24 (d, J = 7.3Hz, 1H), 8.19 (t, J = 7.6Hz, 1H), 8.14 (d, J = 8.8Hz, 1H), 8.06 ( m,4H),8.00(d,J=8.0Hz,2H),7.84(d,J=8.0Hz,2H),7.79–7.66(m,7H),7.53(m,9H),7.47–7.40(m,4H). 13 C NMR (126MHz, CDCl3) δ (ppm): 133.55, 132.16, 131.98, 131.71, 130.99, 130.43, 130.21, 129.68, 129.18, 128.54, 12 8.08,127.60,127.11,126.59,125.93,125.37,124.79,124.54,124.22,123.72,122.98,122.44,121.44,120.85.
[0039] (S)-PyI-OBN-CN: 1 H NMR(500MHz, CDCl3)δ(ppm):8.24(d,J=7.5Hz,1H),8.19(t,J=7.5Hz,1H),8.14(d,J=8.7Hz,1H),8.11– 8.03(m,4H),8.00(d,J=7.8Hz,2H),7.84(d,J=7.3Hz,2H),7.72(m,7H),7.52(m,9H),7.47–7.40(m,4H). 13C NMR (126 MHz, CDCl3) δ (ppm): 132.18, 131.93, 131.71, 131.04, 130.44, 130.08, 129.70, 129.17, 128.55, 128.04, 127.60, 127.11, 126.67, 125.92, 125.37, 124.81, 124.57, 124.23, 123.04, 122.49, 120.84, 118.10, 117.72, 116.97. Mass spectrum MALDI-TOF (m / z) [M + ]: The measured value is 777.54 and the theoretical value is 777.88.
[0040]
[0041] Example 3
[0042] A circularly polarized organic electroluminescent device, using the organic blue light emitting small molecule with a molecular structure of (R / S)-PPI-OBN-CN prepared in Example 1 as the light emitting layer material, the organic electroluminescent device (R / S)-PPI-OBN-CN is prepared on a transparent glass substrate, using an ITO conductive film as the anode, and the device structure is as follows:
[0043] ITO / HATCN(5nm) / TAPC(25nm) / TCTA(15nm) / CBP:(R / S)-PPI-OBN-CN(mass ratio: 4:1)(20nm) / TPBi(40nm) / LiF(1nm) / Al(100nm)
[0044] The device preparation process is as follows: Preparation of the substrate indium tin oxide (ITO) conductive glass: The substrate is cleaned in ultrasonic bath with deionized water, isopropanol, acetone, toluene, acetone, and isopropanol for 20 minutes each, and then dried in an oven for use. After the surface of the ITO conductive glass is treated in a UV ozone cleaner for 40 minutes, it is moved into a vacuum evaporation device (the pressure in the chamber is less than 2×10 -4 Pa); on the anode ITO conductive glass, a hole injection layer HATCN is vacuum-deposited with a thickness of 5 nm; on HATCN, a hole transport layer TAPC is vacuum-deposited with a thickness of 25 nm: on TAPC, an exciton blocking layer TCTA is evaporated with a thickness of 15 nm; on TCTA, a light-emitting layer CBP: (R / S)-PPI-OBN-CN (mass ratio: 4:1) is evaporated with a thickness of 20 nm; on the light-emitting layer, an electron transport layer TPBi is evaporated with a thickness of 40 nm; on TPBi, an electron transport layer LiF is evaporated with a thickness of 1 nm; on LiF, a cathode Al is evaporated with a thickness of 100 nm.
[0045] In this example, CBP:(R / S)-PPI-OBN-CN (mass ratio: 4:1) is used as the light-emitting layer material to prepare a circularly polarized organic electroluminescent device with an external quantum efficiency curve as shown in FIG. Figure 5 The detailed electroluminescent performance data of the device are listed in Table 1.
[0046] Table 1: Electroluminescence performance data of device (R / S)-PPI-OBN-CN
[0047]
[0048] Example 4
[0049] A circularly polarized organic electroluminescent device, using the organic blue light emitting small molecule with a molecular structure of (R / S)-PyI-OBN-CN prepared in Example 2 as the light emitting layer material, the organic electroluminescent device (R / S)-PyI-OBN-CN is prepared on a transparent glass substrate, using an ITO conductive film as the anode, and the device structure is as follows:
[0050] ITO / HATCN(5nm) / TAPC(25nm) / TCTA(15nm) / CBP:(R / S)-PyI-OBN-CN(mass ratio: 4:1)(20nm) / TPBi(40nm) / LiF(1nm) / Al(100nm)
[0051] The preparation process of the device is similar to that of Example 3. The external quantum efficiency curve of the circularly polarized organic electroluminescent device prepared by using CBP:(R / S)-PyI-OBN-CN (mass ratio: 4:1) as the light-emitting layer material is as follows: Figure 6 The detailed electroluminescent performance data of the device are listed in Table 2.
[0052] Table 2: Electroluminescence performance data of device (R / S)-PyI-OBN-CN
[0053]
[0054] The structural formulas of the materials used in the organic electroluminescent devices of Examples 3-4 are as follows, and all of them are commercially available:
[0055]
[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A deep blue light-thermal exciton material with circular polarization properties, the structural formula of which is shown in one of the following:
2. Use of the deep blue light thermoexciton material with circular polarization properties as claimed in claim 1 in the preparation of circularly polarized organic electroluminescent devices.
3. The use of a deep blue light thermoexciton material with circular polarization properties as claimed in claim 2 in the preparation of a circularly polarized organic electroluminescent device, characterized in that: The organic electroluminescent device is composed of a transparent glass substrate, an ITO conductive film anode, an organic functional layer including an organic light-emitting layer, and a cathode. The deep blue light thermoexciton material with circular polarization properties described in claim 1 is used as a doping guest to prepare the organic light-emitting layer.
4. The use of a deep blue light thermoexciton material with circular polarization properties in the preparation of a circularly polarized organic electroluminescent device as claimed in claim 3, characterized in that: The organic functional layer is a sequential structure of one or more of a hole injection layer, a hole transport layer, and an exciton blocking layer, an organic light emitting layer, an electron transport layer, and an electron injection layer.
5. The use of a deep blue light thermoexciton material with circular polarization properties in the preparation of a circularly polarized organic electroluminescent device as claimed in claim 3, characterized in that: The doping host of the organic light-emitting layer is CBP, and the doping mass concentration of the doping guest is 15-25%.
6. The use of a deep blue light thermoexciton material with circular polarization properties in the preparation of a circularly polarized organic electroluminescent device as claimed in claim 2, characterized in that: The organic electroluminescent device is used for preparing a deep blue light circularly polarized organic electroluminescent display or an organic electroluminescent lighting source.
Citation Information
Patent Citations
Pyrene and imidazole derivative and preparation method and application thereof
CN107129469A
Phenanthroimidazole electroluminescent material with circular polarization luminescence as well as preparation method and application thereof
CN113121511A
Boron-nitrogen compound, composition thereof and organic electroluminescent device
CN114736224A
Organic blue light micromolecule based on phenanthroimidazole and application of organic blue light micromolecule in preparation of non-doped organic electroluminescent device
CN114773273A
Cited By
High-color-purity near-ultraviolet heat exciton compound with circular polarization property and application of high-color-purity near-ultraviolet heat exciton compound in preparation of circular polarization organic electroluminescent device