Solid super-strong base catalyst and method for preparing isomeric alcohol polyether by using solid super-strong base catalyst

Through the use of solid super base catalysts, the problems of heavy odor, wide molecular weight distribution and many by-products in the preparation of isomeric alcohol polyethers have been solved, and the preparation of isomeric alcohol polyethers with narrow distribution and low by-products has been achieved, improving the product quality. performance and process efficiency.

CN118755074AActive Publication Date: 2024-10-11ZHEJIANG HUANGMA TECH CO LTD +3
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410985291.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

In the existing isomeric alcohol polyether preparation process, the product has a heavy odor, a wide molecular weight distribution, and many by-products, resulting in unstable application performance, low catalyst activity, and inconvenient use.

Method used

A solid super base catalyst is used, which is composed of a catalyst carrier (such as MgO, ZrO2, Al2O3) and a supported strong base (such as CH3OK, KOH, NaOH). It is prepared by grinding and drying and is used to catalyze the synthesis of isomeric alcohols and epoxy compounds. Polymerization reaction, control reaction conditions to obtain isomeric alcohol polyethers with narrow distribution and low by-products.

Benefits of technology

It achieves low product odor, narrow molecular weight distribution, few by-products, high catalytic activity, simple process, wide range of use, and the catalyst can be reused, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958652170000041
    Figure BDA0004958652170000041
  • Figure BDA0004958652170000121
    Figure BDA0004958652170000121
  • Figure BDA0004958652170000122
    Figure BDA0004958652170000122
Patent Text Reader

Abstract

The invention belongs to the technical field of polyether preparation, and discloses a solid super base catalyst and a method for preparing isomeric alcohol polyether by using the solid super base catalyst. The solid super base catalyst comprises a catalyst carrier and strong base loaded on the catalyst carrier, the strong base is selected from at least one of CH3OK, CH3ONa, KOH and NaOH; the catalyst carrier is prepared from one of MgO, ZrO2 and Al2O3. The solid super base catalyst provided by the invention is composed of the catalyst carrier and the strong base loaded on the catalyst carrier, and has high catalytic activity and high reaction efficiency. The isomeric alcohol polyether with low product odor, narrow molecular weight distribution and few by-products can be prepared by using the isomeric alcohol polyether as a catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyether preparation, and particularly relates to a solid superbase catalyst and a method for preparing isomeric alcohol polyether by using the same. Background Art

[0002] Isomeric alcohol polyethers are polymers of isomeric alcohols and epoxy compounds, and have good wetting, emulsifying, cleaning, dispersing and lubricating properties. They have been widely used in daily chemical, washing, textile, leather, electroplating, papermaking and chemical fiber industries. However, the properties of a series of isomeric alcohol polyethers currently produced are unstable, and in actual applications, there will be quality problems such as heavy odor, unstable cleaning power, and poor repeatability. Studies have shown that the width of the structural distribution of isomeric alcohol polyethers and the amount of by-products directly affect the application performance of the product. Products with narrow distribution and low by-products have low odor, low dynamic surface tension, strong penetration, good foaming performance, and good compatibility with other components. They have been widely used in agriculture, emulsion polymerization, petroleum, personal care, mining, detergents and other fields.

[0003] At present, the process for preparing isomeric alcohol polyethers mainly uses sodium hydroxide and potassium hydroxide as catalysts to react with epoxy compounds to generate isomeric alcohol polyethers. The isomeric alcohol polyethers produced by this process have a strong odor, a wide distribution, and low catalyst activity. The required amount of catalyst is large, and the product after neutralization is opaque. Some studies have proposed a two-step method of first Lewis acid catalysis and then traditional base catalysis to synthesize isomeric alcohol polyethers with narrow distribution. Although Lewis acid catalysis can obtain isomeric alcohol polyethers with better quality, the two-step method is cumbersome, and the prepared product contains many by-products, which will also affect the application performance of the product.

[0004] Therefore, there is an urgent need to provide a method for preparing isomeric alcohol polyethers, which can prepare isomeric alcohol polyethers with low product odor, narrow molecular weight distribution and few by-products. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a solid superbase catalyst and a method for preparing isomeric alcohol polyethers using the same. The solid superbase catalyst provided by the present invention can prepare isomeric alcohol polyethers with low product odor, narrow molecular weight distribution and few by-products.

[0006] The invention provides a solid super base catalyst.

[0007] Specifically, a solid superbase catalyst comprises a catalyst carrier and a strong base supported on the catalyst carrier; the strong base is selected from CH 3 OK, CH 3 At least one of ONa, KOH, and NaOH; the catalyst carrier comprises MgO, ZrO 2 、Al2 O 3 One of them.

[0008] In some embodiments of the present invention, the loading amount of the strong base is 5% to 60%, that is, the mass ratio of the strong base to the catalyst carrier is (0.05 to 0.6): 1. Preferably, the mass ratio of the strong base to the catalyst carrier is (0.1 to 0.5): 1, such as 0.2: 1; 0.3: 1, 0.5: 1, etc.

[0009] The invention provides a method for preparing the solid superbase catalyst.

[0010] Specifically, the preparation method of the above-mentioned solid superbase catalyst comprises the following steps:

[0011] The solid super base catalyst is prepared by mixing a strong base, a catalyst carrier and water, grinding and drying.

[0012] In some embodiments of the present invention, the catalyst carrier is pre-treated by washing, filtering, drying and calcining in sequence before being mixed with the strong base.

[0013] More specifically, the preparation method of the above-mentioned solid superbase catalyst includes the following steps: weighing the catalyst carrier and the strong base, placing them in a mortar, and mixing them to obtain a mixture; adding deionized water according to the mass ratio of the mixture to water of 1: (0.8~1.2), and then grinding them thoroughly; after drying, continuing to grind them evenly, and finally placing the obtained sample in an oven and drying it at 100~120°C to constant weight.

[0014] The invention also provides a method for preparing the isomeric alcohol polyether.

[0015] Specifically, a method for preparing isomeric alcohol polyethers comprises the following steps:

[0016] The isomeric alcohol and epoxy compound are used as raw materials, and a polymerization reaction is carried out in the presence of the solid superbase catalyst to prepare the isomeric alcohol polyether.

[0017] More specifically, a method for preparing isomeric alcohol polyethers comprises the following steps:

[0018] The isomeric alcohol is mixed with the solid superbase catalyst, and the temperature is raised after nitrogen is placed, and then an epoxy compound is added to react. After the reaction pressure does not drop, the temperature is lowered and degassing is performed to obtain the isomeric alcohol polyether.

[0019] In some embodiments of the present invention, the molar ratio of the isomeric alcohol to the epoxy compound is 1:4-60.

[0020] In some embodiments of the present invention, the addition amount of the solid superbase catalyst is 0.02% to 0.04% of the total mass of the isomeric alcohol polyether.

[0021] In some embodiments of the present invention, the epoxy compound includes ethylene oxide and / or propylene oxide. That is, the epoxy compound includes ethylene oxide, propylene oxide, or a mixture of ethylene oxide and propylene oxide in any proportion. By controlling the type of epoxide and the addition method, isomeric alcohol polyethers with one block, two blocks, three blocks or irregular structures can be formed. And the structural mode of EO chain and PO chain in isomeric alcohol polyether does not affect the stability of the product.

[0022] In some embodiments of the present invention, the temperature of the nitrogen treatment is 20-50° C., and the number of nitrogen treatments is 1-4 times.

[0023] In some embodiments of the present invention, the heating process is to heat the temperature to 90-150°C.

[0024] In some embodiments of the present invention, the feeding speed of the epoxy compound is 1-15 g / min, and the pressure is controlled to be no higher than 0.5 MPa, such as 0.4 MPa, during the process of adding the epoxy compound.

[0025] In some embodiments of the present invention, the reaction temperature is 90°C to 95°C.

[0026] In some embodiments of the present invention, the cooling process is to cool to 60-120° C. When the temperature drops to 60-120° C., degassing begins. The degassing time is 5-30 min.

[0027] The invention also provides an isomeric alcohol polyether.

[0028] Specifically, an isomeric alcohol polyether is prepared by the above preparation method, and the molecular structure of the isomeric alcohol polyether is shown in formula (1):

[0029]

[0030] In formula (1): b is the number of propylene oxide in the molecule, b=0-20, a and c are the number of ethylene oxide in the molecule, a=0-20, c=0-20; ROH is an isomeric alcohol of C8-C18.

[0031] In some embodiments of the present invention, the C8-C18 isomeric alcohol refers to a primary alcohol with a carbon number ranging from 8 to 18 and having a branched chain, for example: C8 isomeric alcohol can be 2-ethyl-1-hexanol (CAS: 104-76-7), or 6-methyl-1-heptanol (CAS: 26952-21-6), or a mixture of isomeric alcohols with C8 as the main component; C10 isomeric alcohol can be 2-propyl-1-heptanol (CAS: 25339-17-7), or a mixture of isomeric alcohols with C10 as the main component; C13 isomeric alcohol can be 2-methyl-1-dodecanol (CAS: 68526-86-3), or a mixture of isomeric alcohols with C13 as the main component, etc. The C8-C18 isomeric alcohol also includes a mixture composed of any two or more compounds of C8 to C18 isomeric alcohols in any proportion.

[0032] The solid superbase catalyst provided by the present invention is composed of a catalyst carrier and a strong base supported on the catalyst carrier. In the solid superbase catalyst, the strong base (CH 3 OK, CH 3 ONa, KOH, NaOH) to MgO, ZrO 2 and Al 2 O 3 The surface of the catalyst carrier is modified to form super-alkalinity. Specifically, the generation of super-alkalinity is related to MgO, ZrO 2 and Al 2 O 3 The paramagnetic center formed by the anion holes on the surface capturing the electrons released by the alkali metal and the accompanying electron induction effect are closely related. 2- On, thus causing O 2- The increase in the net negative charge of the cluster increases the 2- The electron-donating ability of the isomeric alcohol polyether produces a super strong alkalinity. Therefore, the molecular weight distribution of the product can be narrowed and the by-product content in the product can be low by using it to prepare isomeric alcohol polyether.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The solid superbase catalyst provided by the present invention is composed of a catalyst carrier and a strong base supported on the catalyst carrier, and has high catalytic activity and high reaction efficiency. Using the solid superbase catalyst as a catalyst, isomeric alcohol polyethers with low product odor, narrow molecular weight distribution and few by-products can be prepared.

[0035] (2) The preparation method of the isomeric alcohol polyether provided by the present invention is stable, and the prepared product has excellent properties and stable quality. The increase in the molecular weight of the isomeric alcohol block polyether, the structural mode of the EO chain and the PO chain in the isomeric alcohol polyether, and the increase in the carbon number of the initiator in the isomeric alcohol polyether do not affect the stability of the product.

[0036] (3) The isomeric alcohol polyether provided by the present invention has low odor, narrow molecular weight distribution, transparent color, few by-products, and a wide range of applications; and the production process is simple, the catalyst can be reused, and the production cost is low. DETAILED DESCRIPTION

[0037] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0038] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0039] Example 1

[0040] A method for preparing a solid superbase catalyst comprises the following steps:

[0041] 1g CH 3 OK and 10g MgO were mixed in a mortar, 11g deionized water was added, and then the mixture was fully ground; dried, and then ground evenly. The obtained sample was placed in an oven and dried at 100°C overnight. 3 OK / MgO solid super base catalyst.

[0042] The solid superbase catalyst prepared above is applied to the preparation of isomeric alcohol polyethers, which specifically comprises the following steps:

[0043] First, 260 g of 6-methyl-1-heptanol and 0.13 g of 10% CH 3 OK / MgO catalyst, closed reactor, stirring and vacuuming, then replaced the gas in the reactor with nitrogen 3 times, heated to 90°C, added 176g ethylene oxide at 10g / min, controlled the reaction temperature at 90°C~95°C, reaction pressure at 0~0.5MPa, matured until the pressure did not drop after addition, then added 232g propylene oxide at 1g / min, controlled the reaction temperature at 90°C~95°C, reaction pressure at 0~0.5MPa, matured until the pressure did not drop after addition, degassed (pressure less than -0.098MPa) for 10min, cooled to 60°C after degassed, filtered and discharged through silk cloth to obtain isomeric alcohol block polyether 334.

[0044] Comparative Example 1

[0045] This comparative example is the same as the method for preparing isomeric alcohol block polyether 334 in Example 1 under the same conditions except that 10% CH 3 OK / MgO replaced by CH 3 OK. 3 OK has low catalytic activity, so CH 3 The amount of OK added was 0.39 g (3 times). After degassing, the temperature was lowered to 60°C and glacial acetic acid was added for neutralization. The amount of glacial acetic acid added was 0.39 g.

[0046] Comparative Example 2

[0047] This comparative example is the same as the method for preparing isomeric alcohol block polyether 334 in Example 1 under the same conditions except that 10% CH 3 OK / MgO was replaced by MgO. Due to the low catalytic activity of MgO, the amount of MgO added was 0.39 g. After degassing, the temperature was lowered to 60°C and glacial acetic acid was added for neutralization. The amount of glacial acetic acid added was 0.39 g.

[0048] Comparative Example 3

[0049] First, 260 g of 6-methyl-1-heptanol and 0.13 g of BF were added to a 2.5 L autoclave. 3 ·(CH 3 CH 2 ) 2 O, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen for 3 times, raise the temperature to 90°C, add 176g of ethylene oxide at 10g / min, control the reaction temperature at 90°C-95°C, and the reaction pressure at 0-0.5MPa. After adding, ripen until the pressure does not drop, then degas for 10min, cool to below 40°C and fill with nitrogen to normal pressure.

[0050] Add 0.39g KOH to the reactor, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, raise the temperature to 90°C, add 232g propylene oxide at 1g / min, control the reaction temperature at 90°C~95°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 10min, neutralize with 0.39g glacial acetic acid, cool to 60°C after neutralization, filter and discharge through silk cloth to obtain isomeric alcohol block polyether 334.

[0051] Example 2

[0052] A method for preparing a solid superbase comprises the following steps:

[0053] 5g CH 3OK and 10g MgO were mixed in a mortar, 15g deionized water was added, and then the mixture was fully ground; dried, and then ground evenly. The obtained sample was placed in an oven and dried at 100°C overnight. 50% CH 3 OK / MgO solid super base catalyst.

[0054] The catalyst prepared above was applied to the preparation of isomeric alcohol polyethers, and the specific steps were the same as those in Example 1.

[0055] Example 3

[0056] A method for preparing a solid superbase comprises the following steps:

[0057] 5g KOH and 10g MgO were placed in a mortar and mixed evenly, 15g deionized water was added, and then the mixture was fully ground; dried, and then ground evenly again, and the obtained sample was placed in an oven and dried at 100°C overnight to obtain a 50% KOH / MgO solid superbase catalyst.

[0058] The catalyst prepared above was applied to the preparation of isomeric alcohol polyethers, and the specific steps were the same as those in Example 1.

[0059] Example 4

[0060] A method for preparing a solid superbase comprises the following steps:

[0061] 3g KOH and 10g ZrO 2 Place in a mortar and mix well, add 15g of deionized water, and then grind thoroughly; dry, grind evenly again, and place the obtained sample in an oven at 110°C to dry overnight. 2 Solid superbase catalyst.

[0062] The catalyst prepared above was applied to the preparation of isomeric alcohol polyethers, and the specific steps were the same as those in Example 1.

[0063] Example 5

[0064] A method for preparing a solid superbase comprises the following steps:

[0065] 5g KOH, 5g MgO and 5g Al 2 O 3 Place in a mortar and mix well, add 15g of deionized water, and then grind thoroughly; dry, grind evenly again, and place the obtained sample in an oven at 120°C to dry overnight. 2 O 3 Solid superbase catalyst.

[0066] The catalyst prepared above was applied to the preparation of isomeric alcohol polyethers, and the specific steps were the same as those in Example 1.

[0067] Example 6

[0068] First, 260 g of 6-methyl-1-heptanol and 0.43 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, closed reactor, stirring and evacuation, then replace the gas in the reactor with nitrogen 3 times, heat to 100 ° C, add 352g ethylene oxide at 13g / min, control the reaction temperature at 100 ° C ~ 105 ° C, reaction pressure 0 ~ 0.5MPa, after addition, mature until the pressure does not drop, then add 464g propylene oxide at 2g / min, control the reaction temperature at 100 ° C ~ 105 ° C, reaction pressure 0 ~ 0.5MPa, after addition, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 15min, degas, cool to 65 ° C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol block polyether 538.

[0069] Example 7

[0070] First, 260 g of 6-methyl-1-heptanol and 0.76 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, raise the temperature to 140°C, add 704g of ethylene oxide at 15g / min, control the reaction temperature at 140°C~150°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, then add 928g of propylene oxide at 5g / min, control the reaction temperature at 140°C~150°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 20min, cool to 65°C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol block polyether 946.

[0071] Example 8

[0072] First, 130 g of 6-methyl-1-heptanol and 0.87 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3Catalyst, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, heat to 140°C, add 880g of ethylene oxide at 15g / min, control the reaction temperature at 140°C~150°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, then add 1160g of propylene oxide at 10g / min, control the reaction temperature at 140°C~150°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 20min, cool to 65°C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol block polyether 2170.

[0073] Example 9

[0074] First, 130 g of 6-methyl-1-heptanol and 0.4 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, raise the temperature to 140°C, add 880g of ethylene oxide at 15g / min, control the reaction temperature at 140°C~150°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 20min, cool to 65°C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol polyoxyethylene ether 1010.

[0075] Example 10

[0076] First, 130 g of 6-methyl-1-heptanol and 0.4 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, raise the temperature to 140°C, add 880g of propylene oxide at 10g / min, control the reaction temperature at 140°C~150°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 20min, cool to 65°C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol polyoxypropylene ether 1010.

[0077] Embodiment 11

[0078] First, 130 g of 6-methyl-1-heptanol and 0.4 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3Catalyst, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, raise the temperature to 140°C, add 880g of a mixture of propylene oxide and propylene oxide at 10g / min, control the reaction temperature to 140°C ~ 150°C, the reaction pressure to 0 ~ 0.5MPa, mature until the pressure does not drop after adding, degas (pressure less than -0.098MPa) for 20min, cool to 65°C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol random polyether 1010.

[0079] Example 12

[0080] First, 130 g of 6-methyl-1-heptanol and 0.4 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, closed reactor, stirring and vacuuming, then replace the gas in the reactor with nitrogen 3 times, heat to 140 ℃, add 176g ethylene oxide at 15g / min, control the reaction temperature at 140 ℃ ~ 150 ℃, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, then add 550g propylene oxide at 10g / min, control the reaction temperature at 140 ℃ ~ 150 ℃, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, add 154g ethylene oxide at 15g / min, control the reaction temperature at 140 ℃ ~ 150 ℃, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, degas (pressure less than -0.098MPa) 20min, cool to 65 ℃ after degassing, filter and discharge through silk cloth to obtain isomeric alcohol block polyether 1010.

[0081] Example 13

[0082] First, 316 g of 2-propyl-1-heptanol and 0.43 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, closed reactor, stirring and evacuation, then replace the gas in the reactor with nitrogen 3 times, heat to 100 ° C, add 298g ethylene oxide at 13g / min, control the reaction temperature at 100 ° C ~ 105 ° C, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, then add 464g propylene oxide at 2g / min, control the reaction temperature at 100 ° C ~ 105 ° C, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, degas (pressure less than -0.098MPa) 15min, degas after cooling to 65 ° C and filter through silk cloth to obtain isomeric alcohol block polyether 538.

[0083] Embodiment 14

[0084] First, 400 g of isotridecanol and 0.43 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, close the reactor, start stirring and evacuate, then replace the gas in the reactor with nitrogen 3 times, raise the temperature to 100°C, add 298g of ethylene oxide at 13g / min, control the reaction temperature at 100°C~105°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, then add 380g of propylene oxide at 2g / min, control the reaction temperature at 100°C~105°C, and the reaction pressure at 0~0.5MPa. After adding, mature until the pressure does not drop, degas (pressure less than -0.098MPa) for 15min, cool to 65°C after degassing, filter and discharge through silk cloth to obtain isomeric alcohol block polyether 538.

[0085] Embodiment 15

[0086] First, 542 g of isooctadecyl alcohol and 0.43 g of 50% KOH / MgO-Al prepared in Example 5 were added to a 2.5 L autoclave. 2 O 3 Catalyst, closed reactor, stirring and evacuation, then replace the gas in the reactor with nitrogen 3 times, heat to 100 ° C, add 228g ethylene oxide at 13g / min, control the reaction temperature at 100 ° C ~ 105 ° C, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, then add 309g propylene oxide at 2g / min, control the reaction temperature at 100 ° C ~ 105 ° C, reaction pressure 0 ~ 0.5MPa, mature until the pressure does not drop after addition, degas (pressure less than -0.098MPa) 15min, degas after cooling to 65 ° C and filter through silk cloth to obtain isomeric alcohol block polyether 538.

[0087] Example 16

[0088] The catalyst filtered out in Example 15 (if less than 0.43 g, new catalyst was added to 0.43 g) was used in the preparation of isomeric alcohol polyethers, and the specific steps were the same as in Example 15.

[0089] Embodiment 17

[0090] The catalyst filtered out in Example 16 (if less than 0.43 g, new catalyst was added to make it 0.43 g) was used in the preparation of isomeric alcohol polyethers, and the specific steps were the same as in Example 15.

[0091] Embodiment 18

[0092] The catalyst filtered out in Example 17 (if less than 0.43 g, new catalyst was added to 0.43 g) was used in the preparation of isomeric alcohol polyethers, and the specific steps were the same as in Example 15.

[0093] Embodiment 19

[0094] The catalyst filtered out in Example 18 (if less than 0.43 g, new catalyst was added to 0.43 g) was used in the preparation of isomeric alcohol polyethers, and the specific steps were the same as in Example 15.

[0095] Product effect testing

[0096] 1. The products obtained in Example 1 and Comparative Examples 1 to 3 were compared in appearance, hydroxyl value and molecular weight distribution were measured, and free dioxane, ethylene oxide and propylene oxide were measured. The comparison of catalyst types between Example 1 and Comparative Examples 1 to 3 is shown in Table 1, and the comparison of product performance is shown in Table 2.

[0097] (1) The contents of free dioxane, ethylene oxide and propylene oxide were measured by gas chromatography.

[0098] (2) The hydroxyl value is determined in accordance with the method of GB / T 7383-2020 “Determination of the hydroxyl value of non-ionic surfactants”.

[0099] (3) The molecular weight distribution coefficient was determined by gel chromatography.

[0100] Table 1 Catalyst types used in Example 1 and Comparative Examples 1 to 3

[0101] project Catalyst type Example 1 <![CDATA[10%CH 3 OK / MgO]]> Comparative Example 1 <![CDATA[CH 3 OK]]> Comparative Example 2 MgO Comparative Example 3 <![CDATA[The first step is BF 3 ·(CH 3 CH 2 ) 2 O, and the second step is KOH]]>

[0102] Table 2 Comparison of product performance obtained in Example 1 and Comparative Examples 1 to 3

[0103]

[0104] As can be seen from Table 2: the product obtained in Example 1 has a narrow molecular weight distribution, the lowest content of free EO, PO and dioxane (all below the lower limit of instrument detection), a transparent appearance, and a hydroxyl value that conforms to the molecular weight corresponding to the feed. The molecular weight distribution of the products obtained in Comparative Examples 1 to 2 is wider than that of Example 1, the hydroxyl value is also quite different from the molecular weight corresponding to the feed, and the product is opaque. The product obtained in Comparative Example 3 has a narrower molecular weight distribution, but a high dioxane content, and the product is opaque.

[0105] 2. The products obtained in Examples 1 to 5 were compared in appearance, hydroxyl value and molecular weight distribution were determined, and free dioxane, ethylene oxide and propylene oxide were determined. The comparison of catalyst types in Examples 1 to 5 is shown in Table 3, and the comparison of product performance is shown in Table 4.

[0106] Table 3 Catalyst types used in Examples 1 to 5

[0107]

[0108]

[0109] Table 4 Comparison of product performance obtained in Examples 1 to 5

[0110]

[0111] It can be seen from Table 4 that the products obtained in Examples 1 to 5 have narrow molecular weight distribution, low free EO, PO and dioxane contents, transparent appearance, and hydroxyl values ​​that meet the molecular weight corresponding to the feed.

[0112] 3. The products obtained in Example 1 and Examples 6 to 8 were compared in appearance, hydroxyl value and molecular weight distribution were determined, and free dioxane, ethylene oxide and propylene oxide were determined. The comparison of catalyst types in Examples 6 to 8 is shown in Table 5, and the comparison of product performance is shown in Table 6.

[0113] Table 5 Process parameters of Example 1, Example 6 to 8

[0114]

[0115] Table 6 Comparison of product performance obtained in Example 1 and Examples 6 to 8

[0116]

[0117] It can be seen from Table 6 that the products prepared in Example 1 and Examples 6 to 8 have narrow molecular weight distribution, low free EO, PO and dioxane content, transparent appearance, and hydroxyl value consistent with the molecular weight corresponding to the feed material. This shows that as the molecular weight of the isomeric alcohol block polyether increases, the quality of the product prepared by the preparation method of the present invention is stable.

[0118] 4. The products obtained in Example 1 and Examples 9 to 12 were compared in appearance, hydroxyl value and molecular weight distribution, and free dioxane, ethylene oxide and propylene oxide. The comparison of catalyst types in Examples 9 to 12 is shown in Table 7, and the comparison of product performance is shown in Table 8.

[0119] Table 7 Process parameters of Example 1, Example 9 to 12

[0120]

[0121] Table 8 Comparison of product performance obtained in Example 1 and Examples 9 to 12

[0122]

[0123] As can be seen from Table 8, the products prepared in Example 1 and Examples 9 to 12 have narrow molecular weight distribution, low free EO, PO and dioxane content, transparent appearance, and hydroxyl value consistent with the molecular weight corresponding to the feed. The data show that the structural mode of EO chain and PO chain in isomeric alcohol polyether does not affect the stability of the preparation method of the present invention.

[0124] 5. The products obtained in Example 1 and Examples 13 to 15 were compared in appearance, and the hydroxyl value and molecular weight distribution, as well as the free dioxane, ethylene oxide and propylene oxide were measured. The comparison of catalyst types of Examples 13 to 15 is shown in Table 9, and the comparison of product performance is shown in Table 10.

[0125] Table 9 Types of isomeric alcohols used in Examples 1 and 13 to 15

[0126] project Isomeric alcohol types Example 1 6-Methyl-1-heptanol Example 13 2-Propyl-1-heptanol Embodiment 14 Isotridecyl alcohol Embodiment 15 Isostearyl alcohol

[0127] Table 10 Comparison of product performance obtained in Example 1 and Examples 13 to 15

[0128]

[0129]

[0130] The data in Table 10 show that the increase in the carbon number of the initiator in the isomeric alcohol polyether does not affect the stability of the preparation method of the present invention.

[0131] 6. The products prepared in Example 1 and Examples 15 to 19 were compared in appearance, and the hydroxyl value and molecular weight distribution were determined, as well as the free dioxane, ethylene oxide and propylene oxide. The performance comparison results of the products prepared in Examples 15 to 19 are shown in Table 11.

[0132] Table 11 Comparison of product performance obtained in Examples 15 to 19

[0133]

[0134] It can be seen from Table 11 that when the solid superbase catalyst prepared by the present invention is reused 4 times, it still maintains excellent catalytic activity and the quality of the prepared product is stable. When it is reused for the 5th time, the catalytic activity decreases, the hydroxyl value increases, and the distribution becomes wider. Therefore, it is shown that the solid superbase catalyst prepared by the present invention can be reused at least 4 times.

[0135] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A solid superbase catalyst, characterized in that: It comprises a catalyst carrier and a strong base loaded on the catalyst carrier; the strong base is selected from at least one of CH3OK, CH3ONa, KOH and NaOH; the catalyst carrier comprises one of MgO, ZrO2 and Al2O3.

2. The solid superbase catalyst according to claim 1, characterized in that The mass ratio of the strong base to the catalyst carrier is (0.05-0.6):

1.

3. The method for preparing the solid superbase catalyst according to claim 1 or 2, characterized in that: The following steps are involved: The solid super base catalyst is prepared by mixing a strong base, a catalyst carrier and water, grinding and drying.

4. A method for preparing isomeric alcohol polyethers, characterized in that: The following steps are involved: The isomeric alcohol and epoxy compound are used as raw materials, and a polymerization reaction is carried out in the presence of the solid superbase catalyst described in claim 1 or 2 to prepare the isomeric alcohol polyether.

5. The preparation method according to claim 4, characterized in that: The following steps are involved: The isomeric alcohol is mixed with the solid superbase catalyst, and the temperature is raised after nitrogen is placed, and then an epoxy compound is added to react. After the reaction pressure does not drop, the temperature is lowered and degassing is performed to obtain the isomeric alcohol polyether.

6. The preparation method according to claim 4 or 5, characterized in that: The molar ratio of the isomeric alcohol to the epoxy compound is 1:4-60.

7. The preparation method according to claim 4 or 5, characterized in that: The addition amount of the solid super base catalyst is 0.02% to 0.04% of the total mass of the isomeric alcohol polyether.

8. The preparation method according to claim 4 or 5, characterized in that: The epoxy compound includes ethylene oxide and / or propylene oxide.

9. The preparation method according to claim 5, characterized in that: The feeding speed of the epoxy compound is 1-15 g / min, and the pressure is controlled not to be higher than 0.5 MPa during the process of adding the epoxy compound.

10. An isomeric alcohol polyether, characterized in that: The isomeric alcohol polyether is prepared by the preparation method according to any one of claims 3 to 9, and the molecular structure of the isomeric alcohol polyether is shown in formula (1): In formula (1): b is the number of propylene oxide in the molecule, b=0-20, a and c are the number of ethylene oxide in the molecule, a=0-20, c=0-20; ROH is an isomeric alcohol of C8-C18.

Citation Information

Patent Citations

  • Methods for preparation and use of strong base catalysts

    CA2620879A1

  • Iso-alcohol alkoxy polyether and preparation method thereof

    CN106554492A

  • Asymmetrical polyether gemini surfactant and preparation method thereof

    CN106929179A

  • Supported solid base catalyst as well as preparation method and application thereof

    CN116284730A

  • METHOD FOR PRODUCING POLYESTERS

    RU2008143136A