Bio-based polyamide polyester as well as preparation method and application thereof

By using new dibasic acid monomers containing amide bonds and hydrophobic side chains to synthesize bio-based polyamide polyesters with low crystallinity, the shortcomings of existing polyamide polyesters in terms of temperature resistance and transparency are solved, and high performance is achieved Polymer materials are suitable for packaging materials, solar panels and other fields.

CN118755083AActive Publication Date: 2024-10-11NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410743217.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-11
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

Existing polyamide polyesters still have room for improvement in terms of temperature resistance, mechanical properties and optical transparency, which limits their wide application in certain fields.

Method used

A new type of dibasic acid monomer containing amide bonds and hydrophobic side chains is used to synthesize bio-based polyamide polyester with low crystallinity through polymerization reaction. The decarboxylation/decomposition of the dibasic acid is prevented through a gradual temperature rise method, and the transparency and temperature resistance of the polymer are improved. performance.

Benefits of technology

The transparency, temperature resistance and mechanical properties of polyamide polyester are significantly improved, the crystallinity is reduced, and a material with high optical transparency is obtained, which is suitable for packaging materials, solar panels and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755083A_ABST
    Figure CN118755083A_ABST
Patent Text Reader

Abstract

The invention provides bio-based polyamide polyester as well as a preparation method and application thereof. The bio-based polyamide polyester is synthesized by adopting binary acid containing amido bonds, hydrophobic side chains and biological carbon atoms, the crystallinity of the polyamide polyester is reduced by the hydrophobic side chains, and the optical transparency of the polyamide polyester is improved; the amido bonds endow the material with excellent temperature resistance, wear resistance and mechanical properties, and the ester bonds endow the material with good impact resistance and relatively high modulus and strength. The bio-based polyamide polyester provided by the invention has the advantages of engineering plastic polyamide and general-purpose plastic polyester, is a novel bio-based high polymer material, and has potential application value in the fields of packaging materials or solar light panels and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer chemistry, and specifically relates to a bio-based polyamide polyester and a preparation method and application thereof. Background Art

[0002] Polyamide polyester is a polymer containing amide bonds and ester bonds in the molecular chain structure. Therefore, it has the impact resistance, high modulus and strength of polyester, and the temperature resistance, wear resistance and mechanical properties of polyamide. Polyamide polyester is easy to process due to the presence of ester bonds, and can be processed into various profiles in a molten state, and is widely used in the pharmaceutical, biomedical, telecommunications cable, automotive and other industries. At the same time, the presence of ester bonds gives polyamide polyester biodegradability, giving it a wide range of application prospects. Although polyester amide has excellent performance and a wide range of applications, its market development is limited at this stage, and there is still much room for improvement in its technical process, production cost, and application field in the future. For example, the temperature resistance and mechanical properties of existing polyamide polyesters still need to be improved, and there is little development of related polymer materials with high optical transparency, which limits the widespread application of polyamide polyester in some fields. Summary of the invention

[0003] The main purpose of the present invention is to provide a novel bio-based polyamide polyester with low crystallinity and a preparation method thereof. The dibasic acid monomer used in the polymerization process includes a novel dibasic acid monomer (a dibasic acid containing a hydrophobic side chain of a structure shown in Formula II) synthesized from a benzene ring dibasic acid and a compound containing at least one amino group and one carboxyl group with a side chain group. Since it contains an amide bond, the polyamide polyester synthesized therefrom has higher mechanical strength and temperature resistance, and due to the presence of the side chain group, the transparency of the polymer is improved, and the ester bond contained therein gives the polyamide polyester good impact resistance, higher modulus and strength.

[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0005] The first aspect of the present invention is to provide a bio-based polyamide polyester, wherein the bio-based polyamide polyester comprises a structure shown in Formula I:

[0006]

[0007] Wherein, Y is selected from para-benzene or iso-benzene, R1, R2, and R3 are independently selected from substituted or unsubstituted alkyl or substituted or unsubstituted aryl, and n is an integer greater than 50.

[0008] The above-mentioned alkyl group may be a straight-chain alkyl group, a branched-chain alkyl group or a cycloalkyl group.

[0009] In some embodiments, R1 and R2 are independently selected from substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted phenyl, or substituted or unsubstituted aromatic heterocyclic group.

[0010] In some embodiments, R1 and R2 are independently selected from methyl, propyl, isopropyl, isobutyl, sec-butyl, ethyl methyl sulfide, benzyl or methyl indole groups.

[0011] In some embodiments, R3 is selected from substituted or unsubstituted C2-C 10 or a substituted or unsubstituted phenyl group.

[0012] In some embodiments, R3 is selected from ethyl, butyl, hexyl, decyl, neopentyl, 1,4-cyclohexanedimethyl or 1,4-di(ethoxy)phenyl.

[0013] In some embodiments, the intrinsic viscosity of the bio-based polyamide polyester is 0.4 dL / g to 2.0 dL / g

[0014] In some embodiments, the bio-based polyamide polyester has a crystallinity of less than 10%.

[0015] In some embodiments, the bio-based polyamide polyester has a transparency of more than 85%.

[0016] In some embodiments, the glass transition temperature of the bio-based polyamide polyester is 90-120°C.

[0017] In some embodiments, the number average molecular weight of the bio-based polyamide polyester is greater than 20,000.

[0018] The second aspect of the present invention is to provide a method for preparing a bio-based polyamide polyester, comprising: subjecting a mixed reaction system containing a dibasic acid, a diol and a catalyst to a polymerization reaction to obtain a bio-based polyamide polyester; the dibasic acid comprises a dibasic acid containing a hydrophobic side chain having a structure shown in Formula II;

[0019]

[0020] Wherein, Y is selected from para-benzene or iso-benzene, and R1 and R2 are independently selected from substituted or unsubstituted alkyl or substituted or unsubstituted aryl.

[0021] The dibasic acid of formula II structure contains a hydrophobic side chain and an amide bond, and the polyamide polyester synthesized therefrom has lower crystallinity, higher transparency, and improved water resistance.

[0022] In some embodiments, the polymerization reaction specifically includes: under inert atmosphere conditions, the mixed reaction system is first subjected to a first-stage reaction at a temperature of 100-130°C, then heated to 150-180°C for a second-stage reaction, and then the vacuum degree is adjusted to below 500 Pa, and the temperature is raised to 220-270°C for a third-stage reaction. Since the dibasic acid of formula II has certain defects in stability during the polymerization process, it is first subjected to an esterification reaction at low temperature to improve its stability, and then the temperature is raised to increase the molecular weight of the prepolymer, further improving its stability, and finally polycondensed at high temperature to obtain polyamide polyester. The use of a gradual heating method can prevent the dibasic acid from decarboxylating / decomposing and thus affecting the degree of polymerization and chromaticity of the polymer.

[0023] Furthermore, the reaction time of the first stage is 1 to 3 hours, the reaction time of the second stage is 1 to 3 hours, and the reaction time of the third stage is 1 to 6 hours.

[0024] In some embodiments, R1 and R2 are independently selected from substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted phenyl, or substituted or unsubstituted aromatic heterocyclic group.

[0025] In some embodiments, R1 and R2 are independently selected from methyl, propyl, isopropyl, isobutyl, sec-butyl, ethyl methyl sulfide, benzyl or methyl indole groups. These groups can be derived from bio-based groups and have the advantages of low toxicity and good biocompatibility. At the same time, by adjusting the R1 and R2 groups, the crystallinity of the obtained polymer can be adjusted, thereby adjusting the transparency of the polymer.

[0026] In some embodiments, the diol includes an aliphatic diol and / or an aromatic diol.

[0027] In some embodiments, the aliphatic diol includes a carbon chain length of C2 to C 10 A linear, branched or cyclic aliphatic diol.

[0028] In some embodiments, the aromatic diol includes an aromatic diol containing a benzene ring.

[0029] In some embodiments, the diol includes one or more of ethylene glycol, butanediol, propylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, hydroquinone bis(hydroxyethyl) ether, resorcinol bis(hydroxyethyl) ether, hexanediol, and decanediol.

[0030] In some embodiments, the dibasic acid further includes an aliphatic dibasic acid and / or an aromatic dibasic acid.

[0031] In some embodiments, the aliphatic diacid includes a carbon chain length of C4 to C 10A linear, branched or cyclic aliphatic diol.

[0032] In some embodiments, the aromatic diacid includes an aromatic diacid containing a benzene ring.

[0033] In some embodiments, the dibasic acid further comprises one or more of adipic acid, sebacic acid, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid.

[0034] In some embodiments, the catalyst includes one or more of antimony glycol, antimony trioxide, tetrabutyl titanate, stannous octoate, and germanium dioxide.

[0035] In some embodiments, the content of the catalyst in the mixed reaction system is less than 1000 ppm.

[0036] In some embodiments, the content of the dibasic acid containing a hydrophobic side chain shown in Formula II is 5 to 100 wt %, for example, 10 to 100 wt %, 20 to 100 wt %, 30 to 100 wt %, 40 to 100 wt %, 50 to 100 wt %, 60 to 100 wt %, 70 to 100 wt %, 80 to 100 wt %, 90 to 100 wt % of the total amount of the dibasic acid.

[0037] In some preferred embodiments, the content of the dibasic acid containing a hydrophobic side chain represented by Formula II is 30-100 wt % of the total amount of the dibasic acid. When the amount of the dibasic acid represented by Formula II is within the above range, the transparency, temperature resistance and mechanical properties of the polyamide polyester can be significantly improved.

[0038] In some embodiments, the molar ratio of the dibasic acid to the diol is 1:1.1 to 1:1.5, preferably 1:1.1 to 1:1.2.

[0039] The third aspect of the present invention is to provide a bio-based polyamide polyester obtained according to any one of the preparation methods described above.

[0040] The fourth aspect of the present invention is to provide the use of the bio-based polyamide polyester in the preparation of packaging materials or solar panels.

[0041] Compared with the prior art, this application has at least the following beneficial effects:

[0042] 1) The polyamide polyester provided by the present invention is an ordered copolymer of alternating amide bonds and ester bonds, and there is no phase separation phenomenon. Due to the presence of hydrophobic side chain groups, the hydrolysis resistance of the material is improved, the crystallinity of the polymer is reduced, and the transparency of the polymer is improved; at the same time, due to the presence of amide bonds, the temperature resistance of the polymer is improved.

[0043] 2) The present invention uses the dibasic acid shown in formula II to prepare polyamide polyester, which can be a semi-biobased source, and the synthesized polyamide polyester has certain biocompatibility and degradability; and the dibasic acid shown in formula II contains an amide bond, which can improve the mechanical strength and temperature resistance of the synthesized polyamide polyester, and at the same time, the hydrophobic side chain contained in it can improve the transparency of the polyamide polyester;

[0044] 3) The present invention adopts an in-situ melt polymerization method to synthesize polyamide polyester, which has a simple preparation process, is easy to operate, is convenient for mass production, and is conducive to industrialization; the use of a gradual heating method can prevent the decarboxylation / decomposition of the dibasic acid from affecting the polymerization degree and chromaticity of the polymer, thereby obtaining a polyamide polyester with high optical transparency. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is the DSC curve chart of the polyamide polyester in Example 3 of the present invention. DETAILED DESCRIPTION

[0046] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.

[0047] Example 1

[0048] Preparation of dibasic acid of formula II:

[0049] Weigh 60 g of terephthaloyl chloride and dissolve it in dichloromethane, weigh 105 g of 2-amino-3-methylbutyric acid and dissolve it in an aqueous solution with a pH of 7.5 to 8.5, slowly drop the terephthaloyl chloride solution into the 2-amino-3-methylbutyric acid aqueous solution, and react for 2 hours. During the reaction, the pH is controlled to be 7.5 to 9 and the reaction temperature is 15±5°C. After the reaction, use hydrochloric acid to adjust the pH to between 1 and 2, filter and wash with water to obtain a dibasic acid with a structure of formula II.

[0050] Weigh 30 g of the prepared dibasic acid of formula II structure, 10.72 g of hexanediol, and 0.01 g of ethylene glycol antimony and place them in a flask. Under nitrogen protection, first heat the temperature to 100 ° C. and react for 3 h, then heat the temperature to 160 ° C. and react for 1 h. Slowly reduce the vacuum degree until the vacuum degree drops to 400 ± 20 Pa, slowly heat the temperature to 230 ° C. and react for 5 h. After the reaction, cool down to obtain polyamide polyester.

[0051] According to the GB / T 1632-93 test method, the intrinsic viscosity of the prepared polyamide polyester was measured to be 0.62 dL / g; the crystallinity was measured to be 1.8% by differential scanning calorimetry; the transparency was measured to be 94% by the GB / T 2410 test method; and the glass transition temperature was measured to be 113°C by the GB / T19466.2-2004 test method.

[0052] Example 2

[0053] In the process of preparing the dibasic acid of formula II, the difference between Example 2 and Example 1 is that 2-amino-3-methylbutyric acid is replaced by 2-amino-4-methylpentanoic acid, and the rest is the same as Example 1.

[0054] Weigh 30 g of a dibasic acid of formula II, 15 g of adipic acid, 17.1 g of butanediol, and 0.02 g of tetrabutyl titanate and place them in a reaction kettle. Under nitrogen protection, first heat the temperature to 120°C for reaction for 1.5 h, then heat the temperature to 180°C for reaction for 1 h, then slowly reduce the vacuum degree to 500±20 Pa, continue to heat the temperature to 250°C for reaction for 3 h, and cool down after the reaction to obtain polyamide polyester.

[0055] According to the same testing method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 0.89 dL / g, the crystallinity was 3.1%, the Tg was 108° C., and the transparency was 93%.

[0056] Example 3

[0057] In the preparation process of the dibasic acid of formula II, the difference between Example 3 and Example 1 is that 2-amino-3-methylbutyric acid is replaced by 2-amino-3-indolylpropionic acid, terephthalic acid is replaced by isophthalic acid, and the rest is implemented in the same way as in Example 1.

[0058] Weigh 10 g of a dibasic acid of formula II structure, 90 g of adipic acid, 89.9 g of hexanediol, and 0.05 g of germanium dioxide and place them in a reactor. First, heat the temperature to 130°C for reaction for 1 h, then heat the temperature to 180°C for reaction for 1 h, then slowly reduce the vacuum degree to 100±10 Pa, continue to heat the temperature to 270°C for reaction for 2 h, and cool down after the reaction to obtain polyamide polyester. Figure 1 It is the DSC curve chart of the polyamide polyester of this Example 3.

[0059] According to the same testing method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 1.08 dL / g, the crystallinity was 9.6%, the Tg was 93° C., and the transparency was 87%.

[0060] Example 4

[0061] In the preparation process of the dibasic acid of formula II structure, the difference between Example 4 and Example 1 is that 2-amino-3-methylbutyric acid is replaced by 2-amino-4-(methylmercapto)butyric acid, and terephthalic acid is replaced by isophthalic acid, and the rest is the same as Example 1.

[0062] Weigh 40 g of the prepared dibasic acid of formula II structure, 20 g of sebacic acid, 39.8 g of decanediol, and 0.04 g of tetrabutyl titanate into a reactor, first react at 100°C for 2 h, then heat to 170°C for 1 h, slowly evacuate to 300±10 Pa, continue to heat to 220°C for 6 h, and cool after the reaction to obtain polyamide polyester.

[0063] According to the same testing method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 0.52 dL / g, the crystallinity was 4.2%, the Tg was 95° C., and the transparency was 91%.

[0064] Example 5

[0065] In the process of preparing the dibasic acid of formula II structure, the difference between Example 5 and Example 1 is that 2-amino-3-methylbutyric acid is replaced by 2-amino-3-phenylpropionic acid, and terephthalic acid is replaced by isophthalic acid, and the rest is the same as Example 1.

[0066] Weigh 50 g of the prepared dibasic acid of formula II structure, 30 g of succinic acid, 107.1 g of hydrogenated bisphenol A, and 0.06 g of germanium dioxide and place them in a reaction kettle. Under nitrogen protection, first heat the temperature to 110° C. for reaction for 2 h, then heat the temperature to 160° C. for reaction for 1 h, slowly reduce the vacuum degree to 100±10 Pa, continue to heat the temperature to 240° C. for reaction for 3 h, and cool down after the reaction to obtain polyamide polyester.

[0067] According to the same testing method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 0.83 dL / g, the crystallinity was 3.6%, the Tg was 115° C., and the transparency was 93%.

[0068] Example 6

[0069] In the preparation process of the dibasic acid of formula II, the difference between Example 5 and Example 1 is that 2-amino-3-methylbutyric acid is replaced by 3-aminopropionic acid, terephthalic acid is replaced by isophthalic acid, and the rest is the same as Example 1.

[0070] Weigh 80 g of the prepared dibasic acid of formula II structure, 32.4 g of neopentyl glycol, and 0.04 g of tetrabutyl titanate and place them in a reaction kettle. Under nitrogen protection, first react at 100° C. for 2 h, then heat to 170° C. for 1 h, slowly evacuate to 50±5 Pa, continue to heat to 250° C. for 3 h, and cool after the reaction to obtain polyamide polyester.

[0071] According to the same test method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 0.97 dL / g, the crystallinity was 1.6%, the Tg was 116° C., and the transparency was 96%.

[0072] Example 7

[0073] The only difference between Example 7 and Example 1 is that, during the preparation of polyamide polyester, 10.72 g of hexanediol in Example 1 is replaced by 13.05 g of 1,4-cyclohexanedimethanol, and the rest is the same as Example 1 to obtain polyamide polyester.

[0074] According to the same test method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be -0.61 dL / g, the crystallinity was 2.3%, the transparency was 92%, and the glass transition temperature was 114°C.

[0075] Example 8

[0076] The only difference between Example 8 and Example 1 is that, during the preparation of polyamide polyester, 10.72 g of hexanediol in Example 1 is replaced by 17.95 g of hydroquinone bis(hydroxyethyl) ether, and the rest is carried out in the same manner as Example 1 to obtain polyamide polyester.

[0077] According to the same testing method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 0.65 dL / g, the crystallinity was 3.2%, the transparency was 89%, and the glass transition temperature was 118°C.

[0078] Example 9

[0079] The only difference between Example 9 and Example 2 is that, during the preparation of polyamide polyester, 2.25 g of dibasic acid of formula II, 42.75 g of adipic acid, 29.76 g of butanediol, and 0.02 g of tetrabutyl titanate are placed in a reactor for reaction, and the rest is carried out in the same manner as in Example 2 to obtain polyamide polyester.

[0080] According to the same testing method as in Example 1, the intrinsic viscosity of the prepared polyamide polyester was measured to be 0.87 dL / g, the crystallinity was 21.8%, the Tg of the synthesized polyamide polyester was 25° C., and the transparency was 81%.

[0081] Example 10

[0082] The only difference between Example 10 and Example 2 is that, during the preparation of polyamide polyester, 4.5 g of dibasic acid of formula II, 40.5 g of adipic acid, 28.62 g of butanediol, and 0.02 g of tetrabutyl titanate are placed in a reactor for reaction, and the rest is carried out in the same manner as in Example 2 to obtain polyamide polyester.

[0083] According to the same testing method as in Example 1, the intrinsic viscosity of the prepared polyamide polyester was measured to be 0.82 dL / g, the Tg of the synthesized polyamide polyester was 36° C., the crystallinity was 10.5%, and the transparency was 82%.

[0084] Comparative Example 1

[0085] The difference between Comparative Example 1 and Example 2 is that the dibasic acid of formula II is not pre-synthesized, and terephthalic acid and 2-amino-4-methylvaleric acid are directly used for polymerization reaction, as follows:

[0086] Take 12.7g of terephthalic acid, 20.1g of 2-amino-4-methylvaleric acid, 15g of adipic acid, 17.1g of butanediol, and 0.02g of tetrabutyl titanate and put them in a reactor. Under nitrogen protection, first heat the temperature to 120°C for reaction for 1.5h, then heat the temperature to 180°C for reaction for 1h, then slowly reduce the vacuum degree to 500±20Pa, continue to heat the temperature to 250°C for reaction for 3h, and cool down after the reaction to obtain polyamide polyester.

[0087] According to the same test method as in Example 1, the intrinsic viscosity of the polyamide polyester was measured to be 0.55 dL / g, its Tg was measured by DSC to be 92° C., its crystallinity was 8.6%, and its transparency was 56%.

[0088] By comparing Comparative Example 1 and Example 2, it can be seen that the Tg of the polyamide polyester synthesized in Example 2 is 108°C and the transparency is 93%. This is because the use of the dibasic acid of the formula II structure in Example 2 can make the formed polyamide polyester an ordered homopolymer of alternating amide bonds and ester bonds, and the obtained polyamide polyester has a higher molecular weight (for example, the number average molecular weight reaches more than 20,000) and exhibits a higher glass transition temperature; while in Comparative Example 1, due to the use of three monomers for polymerization, the segment structure is not uniform during the polymerization process, showing a block copolymer, and the glass transition temperature of the obtained polymer is low. At the same time, since 2-amino-4-methylpentanoic acid has poor stability, it is easy to self-polymerize or deaminate during the polymerization process, resulting in a decrease in the molecular weight of the polymer and a deepening of the color. The present invention uses the dibasic acid of the formula II structure with better stability and better reaction activity to prepare polyamide polyester, so that the obtained polyamide polyester has higher transparency, lower chroma, and higher viscosity.

[0089] Comparative Example 2

[0090] The difference between Comparative Example 2 and Example 2 is that the dibasic acid of Formula II is replaced with an equal molar amount of terephthalic acid to carry out the polymerization reaction, as follows:

[0091] Take 12.7g of terephthalic acid, 15g of adipic acid, 17.1g of butanediol, and 0.02g of tetrabutyl titanate and put them in a reactor. Under nitrogen protection, first heat it to 120℃ and react for 1.5h, then heat it to 180℃ and react for 1h, then slowly reduce the vacuum degree to 500±20Pa, continue to heat it to 250℃ and react for 3h, cool it after the reaction to obtain a polymer.

[0092] The test was carried out in the same manner as in Example 1, and the intrinsic viscosity was measured to be 0.49 dL / g. The Tg was measured by DSC to be 63° C., the crystallinity was 36%, and the transparency was 78%.

[0093] By comparing Comparative Example 2 and Example 2, it can be seen that the polyamide polyester synthesized in Example 2 has a Tg of 108°C and a transparency of 93%, which indicates that the presence of amide bonds can significantly improve the temperature resistance of the polymer, while the presence of side chains improves the transparency of the polyester.

[0094] Comparative Example 3

[0095] 10.2g of terephthalic acid and 4.5g of 4-aminobutyric acid were weighed, heated to 130°C for reaction for 2h, then 8.7g of hexanediol was added, the temperature was raised to 150°C for reaction for 3h, vacuumed to below 100Pa, and the temperature was raised to 230°C for reaction for 5h to obtain polyamide polyester. After testing, the viscosity was 0.83, the crystallinity was 26%, the Tg was 105°C, and the transparency was 68%. The polyamide polyester synthesized in this comparative example has a higher crystallinity and a significantly reduced transparency because it does not contain a side chain structure.

[0096] Table 1 Relevant properties of polymers prepared in the examples and comparative examples of the present invention

[0097]

[0098] In summary, the present invention uses a dibasic acid of formula II structure containing an amide bond, a hydrophobic side chain and a biological carbon atom to prepare polyamide polyester, wherein the hydrophobic side chain reduces the crystallinity of the polyamide-polyester and improves its optical transparency, the amide bond gives the product excellent temperature resistance, wear resistance and mechanical properties, and the ester bond gives it good impact resistance, high modulus and strength. Therefore, the polymer synthesized by the present invention has the advantages of both engineering plastic polyamide and general plastic polyester, and is a new type of bio-based polymer material, which has potential application value in the fields of packaging materials and films in the future.

[0099] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0100] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0101] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.

Claims

1. A bio-based polyamide polyester, characterized in that: The bio-based polyamide polyester comprises a structure shown in Formula I: Wherein, Y is selected from para-benzene or iso-benzene, R1, R2, and R3 are independently selected from substituted or unsubstituted alkyl or substituted or unsubstituted aryl, and n is an integer greater than 50.

2. The bio-based polyamide polyester according to claim 1, characterized in that The bio-based polyamide polyester satisfies at least one of the following conditions ah: a. R1 and R2 are independently selected from substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted phenyl or substituted or unsubstituted aromatic heterocyclic group; b. R1 and R2 are independently selected from methyl, propyl, isopropyl, isobutyl, sec-butyl, ethyl methyl sulfide, benzyl or methyl indole groups; c. R3 is selected from substituted or unsubstituted C2 to C 10 an alkyl group or a substituted or unsubstituted phenyl group; d. R3 is selected from ethyl, butyl, hexyl, decyl, neopentyl, 1,4-cyclohexanedimethyl or 1,4-di(ethoxy)phenyl; e. The intrinsic viscosity of the bio-based polyamide polyester is 0.4 dL / g to 2.0 dL / g; f. The crystallinity of the bio-based polyamide polyester is less than 10%; g. The transparency of the bio-based polyamide polyester is greater than 85%; h. The glass transition temperature of the bio-based polyamide polyester is 90 to 120° C.; i. The number average molecular weight of the bio-based polyamide polyester is greater than 20,000.

3. A method for preparing bio-based polyamide polyester, characterized in that: include: A mixed reaction system containing a dibasic acid, a diol and a catalyst is subjected to a polymerization reaction to obtain a bio-based polyamide polyester; the dibasic acid comprises a dibasic acid having a hydrophobic side chain and having a structure shown in Formula II; Wherein, Y is selected from para-benzene or iso-benzene, and R1 and R2 are independently selected from substituted or unsubstituted alkyl or substituted or unsubstituted aryl.

4. The preparation method according to claim 3, characterized in that: The polymerization reaction specifically includes: under inert atmosphere conditions, the mixed reaction system is first subjected to a first-stage reaction at a temperature of 100-130° C., then the temperature is raised to 150-180° C. for a second-stage reaction, and then the vacuum degree is adjusted to below 500 Pa and the temperature is raised to 220-270° C. for a third-stage reaction.

5. The preparation method according to claim 4, characterized in that: The first stage reaction time is 1 to 3 hours, the second stage reaction time is 1 to 3 hours, and the third stage reaction time is 1 to 6 hours.

6. The preparation method according to claim 3, characterized in that: R1 and R2 are independently selected from substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted phenyl or substituted or unsubstituted aromatic heterocyclic group. Preferably, R1 and R2 are independently selected from methyl, propyl, isopropyl, isobutyl, sec-butyl, ethyl methyl sulfide, benzyl or methyl indole group.

7. The preparation method according to claim 3, characterized in that: The diol includes aliphatic diol and / or aromatic diol. Preferably, the diol includes one or more of ethylene glycol, butanediol, propylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, hydroquinone bis(hydroxyethyl) ether, resorcinol bis(hydroxyethyl) ether, hexanediol, and decanediol. And / or, the dibasic acid further comprises an aliphatic dibasic acid and / or an aromatic dibasic acid, preferably, the dibasic acid further comprises one or more of adipic acid, sebacic acid, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid; And / or, the catalyst includes one or more of antimony glycol, antimony trioxide, tetrabutyl titanate, stannous octoate, and germanium dioxide.

8. The preparation method according to claim 3, characterized in that: The content of the dibasic acid containing a hydrophobic side chain represented by formula II is 5 to 100 wt % of the total amount of the dibasic acid, preferably 30 to 100 wt %; And / or, the molar ratio of the dibasic acid to the diol is 1:1.1 to 1:1.

5.

9. The bio-based polyamide polyester obtained according to the preparation method according to any one of claims 3 to 7.

10. Use of the bio-based polyamide polyester according to any one of claims 1, 2 and 9 in the preparation of packaging materials or solar panels.

Citation Information

Patent Citations

  • Biodegradable alternate polyesteramide preparation method

    CN103881086A

  • Semi-aromatic polyesteramide and synthetic method thereof

    CN105295036A

  • Transparent polyamide as well as preparation method and application thereof

    CN117186343A

  • Polyester, polyesteramide, and polyamide compositions

    US20220325035A1