Ion selective electrode sensitive membrane and preparation method thereof
By coating the polymer substrate film with a coating of sensitive substances, combined with the hot melt method and the solvent evaporation method, the problems of high organic solvent consumption and uneven film thickness in the existing technology are solved, and an environmentally friendly ion-selective electrode sensitivity is achieved. Membrane preparation improves the electrochemical response performance and stability of the electrode.
Patent Information
- Application Number
- CN202410738011.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing preparation method of ion-selective electrode sensitive membrane, the use of organic solvents consumes a lot of money, causes serious environmental pollution, slow film formation speed and uneven film thickness distribution, which affects the stability and response performance of the electrode.
The polymer substrate film is used as the basis, and the surface is coated with a coating containing sensitive substances. The ion-selective electrode sensitive film is prepared by combining the hot melt method and the solvent evaporation method to reduce the use of solvents, increase the film formation speed, and ensure Film thickness uniformity.
The use of harmful solvents is significantly reduced, the preparation time is shortened, the uniformity of film thickness and the electrochemical response performance of the electrode are improved, and the stability and response performance of the electrode are ensured.
Smart Images

Figure BDA0004882357760000061 
Figure BDA0004882357760000071 
Figure BDA0004882357760000072
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrode sensitive membranes, and specifically relates to an ion selective electrode sensitive membrane and a preparation method thereof. Background Art
[0002] Ion selective electrode (ISE) is an analytical test tool that can quickly, accurately, conveniently and selectively determine the content of a certain ion in a complex sample. Its detection principle is that the relationship between the response potential of the sensitive membrane and the activity of the analyte ion conforms to the Nernst equation. It is widely used in biomedical testing, chemical production and geological testing. The sensitive membrane is the core of the ion selective electrode. Glass membrane, crystal membrane, liquid membrane and polymer membrane have been developed successively. Since polymer sensitive membranes are easy to make and process, they are increasingly widely used in ion selective electrodes. The preparation of polymer membranes generally adopts solvent evaporation and hot melt methods. In the former, the polymer is in a dissolved state in the solvent. When the solvent evaporates, the strong interaction between the polymer chains causes the polymer to form a film with substances such as plasticizers and ion carriers. In the latter, the polymer particles are in a dispersed accumulation state and need to be heated above the softening temperature to be molten together with the plasticizer and ion carrier, so that the polymer chains of different particles penetrate each other and form a film after cooling.
[0003] In the prior art, most of the ion-selective electrode sensitive membranes are prepared by the organic solvent volatilization method. This method uses a large amount of organic solvents, which causes great environmental pollution and is not conducive to environmental protection. The volatilization process generally lasts 24 to 48 hours, which is time-consuming. During the membrane preparation process, due to the volatilization of organic solvents, more pores will be generated on the membrane surface, and long-term immersion in aqueous solution will cause rapid erosion and deterioration. At the same time, the inconsistency of the volatilization rate of the solution surface and the surface tension of the wall make the membrane uniform and inconsistent, affecting the stability of the membrane.
[0004] The patented technology of "A dripping film sensing membrane ion selective electrode" (CN201210459460) directly drips the prepared membrane solution into the electrode chamber to volatilize into a film; the patented technology of "A solid contact potassium ion selective electrode and its preparation and application" (CN106198676A) drips the membrane solution on the solid layer and dries it at room temperature to form an ion selective electrode. The multiple dripping methods in the above two patented technologies are cumbersome and time-consuming, and the thickness, shape, size and uniformity of the sensitive membrane are not easy to control, and are suitable for preparing micron-level thin films. There are still some shortcomings if you want to prepare a thicker and evenly distributed sensitive membrane.
[0005] The patented technology of "Organic Ion Selective Membrane" (CN1302223A) uses hot melt extrusion to prepare ion selective membranes. The prepared membranes are less porous, inert to water, have a longer storage period, and are suitable for mass production. However, the hot melt method promotes the mutual penetration of substances by heating. Excessively high temperatures will decompose ion carrier sensitive substances, which hinders the application of the hot melt method.
[0006] In summary, the current technology of preparing ion-selective electrode sensitive membranes by organic solvent volatilization has the defects of large organic solvent consumption, environmental pollution, slow film formation speed and uneven film thickness distribution. Summary of the invention
[0007] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing an ion-selective electrode sensitive membrane which consumes less solvent, is environmentally friendly and has a fast film-forming speed. The ion-selective electrode sensitive membrane prepared by the method has a uniform film thickness and the electrode prepared by the ion-selective electrode sensitive membrane has good electrochemical response performance.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is:
[0009] The method comprises taking 25-50 wt% of polyvinyl chloride, 45-73.5 wt% of plasticizer, 1-4 wt% of ion carrier and 0.5-1 wt% of ion exchanger as raw materials, dissolving the raw materials in tetrahydrofuran at a mass ratio of 1:50-100 under normal temperature and pressure conditions, and obtaining a coating containing sensitive substances.
[0010] 33-50 wt% of polymer particles and 50-67 wt% of plasticizer are mixed at room temperature and normal pressure to obtain a mixed solution; the mixed solution is then heated at 0.02-0.06 mL / cm 2 The mixture is added to the bottom of a flat plate, kept warm at 80 to 120° C. for 10 to 30 minutes, and cooled naturally to obtain a polymer substrate film.
[0011] The plasticizer in the raw material is the same as the plasticizer in the mixed solution.
[0012] The polymer substrate film is cut into a rectangular plane, and then the coating containing the sensitive substance is applied to the surface of the polymer substrate film of the rectangular plane, and left to stand at room temperature for 5 to 10 minutes to obtain an ion selective electrode sensitive membrane with a thickness of 0.1 to 0.3 mm.
[0013] The plasticizer is one of o-nitrophenyl octyl ether, dioctyl phthalate and dioctyl sebacate.
[0014] The ion carrier is a potassium ion carrier or a sodium ion carrier.
[0015] The ion exchanger is one of potassium tetrakis(4-chlorophenyl)borate and sodium tetrakis(4-chlorophenyl)borate.
[0016] The polymer particles are one of polyvinyl chloride, cellulose acetate and polyurethane.
[0017] The coating method is one of brushing, dipping and spraying; brushing each plane 3 to 5 times, spraying each plane 3 to 4 times; after the solvent evaporates to form a coating, turn over and brush or spray. Dipping is 2 to 3 times, and each dipping time is 1 to 2 seconds.
[0018] The length×width of the rectangle is 5-8×6-9 mm.
[0019] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0020] 1. The existing polymer solution volatilization method is used to prepare ion-selective electrode sensitive membranes, which uses a large amount of organic solvents such as THF / cyclohexanone. The solvent must be completely volatilized during membrane preparation, which causes heavy pollution. The present invention prepares ion-selective electrode sensitive membranes by coating a coating containing sensitive substances on a polymer substrate membrane, and the solvent consumption is about 1-2% of the former, which greatly reduces the volatilization of harmful organic solvents and is environmentally friendly. At the same time, the film forming speed is fast. The preparation of the polymer substrate membrane only takes about half an hour, and the coating solution coating and solvent volatilization film forming also only take half an hour, which is less than 1 hour in total. The solvent volatilization film forming takes 24-48 hours, which greatly saves the preparation time and has a fast film forming speed.
[0021] 2. The present invention combines the advantages of hot melt method and solvent volatilization method for preparing polymer membrane. The polymer substrate membrane prepared by the hot melt method adopted by the present invention has uniform film thickness distribution, a small amount of coating solution containing sensitive substances is attached to the polymer substrate membrane by coating, and then the solvent evaporates quickly to form an ion selective electrode sensitive membrane, and the prepared ion selective electrode membrane has uniform thickness and uniform material distribution.
[0022] 3. The electrode assembled from the ion-selective electrode sensitive membrane prepared by the present invention has been tested: the CV value is less than 1%, and the stability is good; the slope is 48-53mV; and after being washed and treated with heat and humidity changes, it still has a good response.
[0023] Therefore, the present invention has the characteristics of less solvent consumption, environmental friendliness and fast film forming speed. The prepared ion selective electrode sensitive membrane has uniform film thickness and the electrode prepared with the ion selective electrode sensitive membrane has good electrochemical response performance. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with specific embodiments, but is not intended to limit the scope of protection thereof:
[0025] An ion selective electrode sensitive membrane and a preparation method thereof. The preparation method described in this specific embodiment is:
[0026] The method comprises taking 25-50 wt% of polyvinyl chloride, 45-73.5 wt% of plasticizer, 1-4 wt% of ion carrier and 0.5-1 wt% of ion exchanger as raw materials, dissolving the raw materials in tetrahydrofuran at a mass ratio of 1:50-100 under normal temperature and pressure conditions, and obtaining a coating containing sensitive substances.
[0027] 33-50 wt% of polymer particles and 50-67 wt% of plasticizer are mixed at room temperature and normal pressure to obtain a mixed solution; the mixed solution is then heated at 0.02-0.06 mL / cm 2 The mixture is added to the bottom of a flat plate, kept warm at 80 to 120° C. for 10 to 30 minutes, and cooled naturally to obtain a polymer substrate film.
[0028] The plasticizer in the raw material is the same as the plasticizer in the mixed solution.
[0029] The polymer substrate film is cut into a rectangular plane, and then the coating containing the sensitive substance is applied to the surface of the polymer substrate film of the rectangular plane, and left to stand at room temperature for 5 to 10 minutes to obtain an ion selective electrode sensitive membrane with a thickness of 0.1 to 0.3 mm.
[0030] The plasticizer is one of o-nitrophenyl octyl ether, dioctyl phthalate and dioctyl sebacate.
[0031] The ion carrier is a potassium ion carrier or a sodium ion carrier.
[0032] The ion exchanger is one of potassium tetrakis(4-chlorophenyl)borate and sodium tetrakis(4-chlorophenyl)borate.
[0033] The polymer particles are one of polyvinyl chloride, cellulose acetate and polyurethane.
[0034] The coating method is one of brushing, dipping and spraying; each plane is brushed 3 to 5 times, and each plane is sprayed 3 to 4 times. After the solvent evaporates to form a coating, it is turned over and brushed or sprayed; the number of dipping is 2 to 3 times, and the time of each dipping is 1 to 2 seconds.
[0035] The length×width of the rectangle is 5~8×6~9mm.
[0036] Example 1
[0037] An ion selective electrode sensitive membrane and a preparation method thereof. The preparation method described in this embodiment is:
[0038] 25 wt% of polyvinyl chloride, 73.5 wt% of plasticizer, 1 wt% of ion carrier and 0.5 wt% of ion exchanger are used as raw materials, and the raw materials are dissolved in tetrahydrofuran at a mass ratio of 1:50 under normal temperature and pressure to obtain a coating containing sensitive substances.
[0039] 33 wt% of polymer particles and 67 wt% of plasticizer were mixed at room temperature and pressure to obtain a mixed solution; the mixed solution was then heated at 0.02 mL / cm 2 The mixture was added to the bottom of a flat plate, kept at 80° C. for 30 min, and cooled naturally to obtain a polymer substrate film.
[0040] The plasticizer in the raw material is the same as the plasticizer in the mixed solution.
[0041] The polymer substrate film was cut into a rectangular plane of 5×6 mm, and then the coating containing the sensitive substance was applied to the surface of the polymer substrate film of the rectangular plane and allowed to stand at room temperature for 5 minutes to obtain an ion-selective electrode sensitive membrane with a thickness of 0.1 mm.
[0042] The plasticizer is o-nitrophenyl octyl ether.
[0043] The ion carrier is a potassium ion carrier.
[0044] The ion exchanger is potassium tetrakis (4-chlorophenyl) borate.
[0045] The polymer particles are polyvinyl chloride.
[0046] The coating method is brushing, and each plane is brushed 3 times; after the solvent evaporates to form a coating, it is turned over and brushed.
[0047] Example 2
[0048] An ion selective electrode sensitive membrane and a preparation method thereof. The preparation method described in this embodiment is:
[0049] 35 wt% of polyvinyl chloride, 62.2 wt% of plasticizer, 2 wt% of ion carrier and 0.8 wt% of ion exchanger are used as raw materials, and the raw materials are dissolved in tetrahydrofuran at a mass ratio of 1:65 under normal temperature and pressure to obtain a coating containing sensitive substances.
[0050] 40 wt% of polymer particles and 60 wt% of plasticizer were mixed at room temperature and pressure to obtain a mixed solution; the mixed solution was then heated at 0.04 mL / cm 2 The mixture was added to the bottom of a flat plate, kept at 100° C. for 25 min, and cooled naturally to obtain a polymer substrate film.
[0051] The plasticizer in the raw material is the same as the plasticizer in the mixed solution.
[0052] The polymer substrate film was cut into a rectangular plane of 6×7 mm, and then the coating containing the sensitive substance was applied to the surface of the polymer substrate film of the rectangular plane and allowed to stand at room temperature for 7 minutes to obtain an ion-selective electrode sensitive membrane with a thickness of 0.2 mm.
[0053] The plasticizer is dioctyl phthalate.
[0054] The ion carrier is a potassium ion carrier.
[0055] The ion exchanger is potassium tetrakis (4-chlorophenyl) borate.
[0056] The polymer particles are cellulose acetate.
[0057] The coating method is dipping; the dipping times are 3 times, and the dipping time for each time is 1 second.
[0058] Example 3
[0059] An ion selective electrode sensitive membrane and a preparation method thereof. The preparation method described in this embodiment is:
[0060] 45 wt% of polyvinyl chloride, 51 wt% of plasticizer, 3 wt% of ion carrier and 1 wt% of ion exchanger are used as raw materials, and the raw materials are dissolved in tetrahydrofuran at a mass ratio of 1:80 under normal temperature and pressure to obtain a coating containing sensitive substances.
[0061] 50 wt% of polymer particles and 50 wt% of plasticizer were mixed at room temperature and normal pressure to obtain a mixed solution; the mixed solution was then heated at 0.06 mL / cm 2 The mixture was added to the bottom of a flat plate, kept at 110° C. for 20 min, and cooled naturally to obtain a polymer substrate film.
[0062] The plasticizer in the raw material is the same as the plasticizer in the mixed solution.
[0063] The polymer substrate film was cut into a rectangular plane of 7×8 mm, and then the coating containing the sensitive substance was applied to the surface of the polymer substrate film of the rectangular plane and allowed to stand at room temperature for 9 minutes to obtain an ion-selective electrode sensitive membrane with a thickness of 0.3 mm.
[0064] The plasticizer is dioctyl sebacate.
[0065] The ion carrier is a potassium ion carrier.
[0066] The ion exchanger is potassium tetrakis (4-chlorophenyl) borate.
[0067] The polymer particles are polyurethane.
[0068] The coating method is spraying, and each plane is sprayed 4 times; after the solvent evaporates to form a coating, it is turned over and sprayed again.
[0069] Example 4
[0070] An ion selective electrode sensitive membrane and a preparation method thereof. The preparation method described in this embodiment is:
[0071] 50 wt% of polyvinyl chloride, 45 wt% of plasticizer, 4 wt% of ion carrier and 1 wt% of ion exchanger are used as raw materials, and the raw materials are dissolved in tetrahydrofuran at a mass ratio of 1:100 under normal temperature and pressure to obtain a coating containing sensitive substances.
[0072] 33 wt% of polymer particles and 67 wt% of plasticizer were mixed at room temperature and pressure to obtain a mixed solution; the mixed solution was then heated at 0.06 mL / cm 2 The mixture was added to the bottom of a flat plate, kept at 120° C. for 10 min, and cooled naturally to obtain a polymer substrate film.
[0073] The plasticizer in the raw material is the same as the plasticizer in the mixed solution.
[0074] The polymer substrate film was cut into a rectangular plane of 8×9 mm, and then the coating containing the sensitive substance was applied to the surface of the polymer substrate film of the rectangular plane and allowed to stand at room temperature for 10 minutes to obtain an ion-selective electrode sensitive membrane with a thickness of 0.3 mm.
[0075] The plasticizer is o-nitrophenyl octyl ether.
[0076] The ion carrier is a sodium ion carrier.
[0077] The ion exchanger is sodium tetrakis (4-chlorophenyl) borate.
[0078] The polymer particles are polyvinyl chloride.
[0079] The coating method is brushing, and each plane is brushed 5 times; after the solvent evaporates to form a coating, it is turned over and brushed.
[0080] Compared with the prior art, this specific implementation has the following positive effects:
[0081] 1. The existing polymer solution volatilization method is used to prepare ion-selective electrode sensitive membranes, which uses a large amount of organic solvents such as THF / cyclohexanone. The solvent must be completely volatilized during membrane preparation, which causes heavy pollution. This specific embodiment prepares an ion-selective electrode sensitive membrane by coating a coating containing sensitive substances on a polymer substrate membrane, and the solvent consumption is about 1-2% of the former, which greatly reduces the volatilization of harmful organic solvents and is environmentally friendly. At the same time, the film formation speed is fast. The preparation of the polymer substrate membrane only takes about half an hour, and the coating solution coating and solvent volatilization film formation also only take half an hour, less than 1 hour in total, while the solvent volatilization film formation takes 24-48 hours, which greatly saves the preparation time and has a fast film formation speed.
[0082] 2. This specific embodiment combines the advantages of the hot melt method and the solvent evaporation method for preparing the polymer substrate membrane. The polymer substrate membrane prepared by the hot melt method used in this specific embodiment has a uniform film thickness distribution, a small amount of coating solution containing sensitive substances is attached to the polymer substrate membrane by coating, and then the solvent evaporates quickly to form an ion-selective electrode sensitive membrane. The prepared ion-selective electrode membrane has a uniform thickness and uniform material distribution.
[0083] 3. Performance Testing
[0084] 3.1. Performance test of ion selective electrode sensitive membrane prepared in Examples 1 to 4
[0085] The prepared ion-selective electrode sensitive membrane was assembled into an electrode, activated for 2 hours, and then placed on an electrolyte analysis tester to measure the reference solution. The electrochemical properties of the prepared ion-selective electrode sensitive membrane are shown in Table 1, which are comparable to those of commercial K + Compared with the electrodes, the performance of the two is similar. The CV value during the measurement is less than 1%, and the stability is good.
[0086] Table 1 Electrochemical performance of the prepared ion selective electrode sensitive membrane
[0087]
[0088] *L CV , H CV They are the coefficient of variation values of low-concentration and high-concentration calibration solutions, which are used to measure the stability of data measurement. CV≤1% is considered to be good for data measurement stability.
[0089] 3.2. Stability test of the ion selective electrode sensitive membrane prepared in Examples 1 to 4
[0090] To simulate the working conditions of the electrode, the assembled electrode was placed on a pulse flushing device, and the ion-selective electrode sensitive membrane was flushed with a water flow of 60 ml / min. After 10 hours (about 100,000 times) of flushing, the measurement results of the electrochemical performance of the assembled electrode after flushing are shown in Table 2. Comparing Table 1 and Table 2, the slope of the assembled electrode after flushing remains good, with only a slight increase in the CV value, and it has appropriate stability.
[0091] Table 2 Electrochemical performance of the assembled electrodes after flushing
[0092]
[0093] 3.3. Electrochemical performance test of the ion-selective electrode sensitive membranes prepared in Examples 1 to 4 assembled into electrodes after storage at variable temperatures
[0094] With reference to the relevant requirements of GB / T 11606-2007, the ion selective electrode sensitive membrane was stored in alternating wet and hot conditions. The temperature range was 5-40°C, and one cycle was 24 hours. After two cycles, it was taken out and then the membrane was attached. The ion selective electrode sensitive membrane was assembled into an electrode. The electrochemical performance test of the electrode assembled after the ion selective electrode sensitive membrane was stored in alternating wet and hot conditions is shown in Table 3.
[0095] Table 3 Electrochemical performance of ion selective electrode sensitive membrane assembled into electrodes after storage at variable temperature
[0096]
[0097] The ion selective electrode sensitive membrane prepared in this specific embodiment is assembled into an electrode and tested: the CV value is less than 1%, and the stability is good; the slope is 48-53mV. After being washed and treated with heat and humidity changes, it still has a good response.
[0098] Therefore, this specific implementation has the characteristics of low solvent consumption, environmental friendliness, and fast film formation speed. The prepared ion-selective electrode sensitive membrane has uniform film thickness, and the electrode prepared with the ion-selective electrode sensitive membrane has good electrochemical response performance.
Claims
1. A method for preparing an ion-selective electrode sensitive membrane, Features The preparation method is: Using 25-50 wt% of polyvinyl chloride, 45-73.5 wt% of plasticizer, 1-4 wt% of ion carrier and 0.5-1 wt% of ion exchanger as raw materials, dissolving the raw materials in tetrahydrofuran at a mass ratio of 1:50-100 under normal temperature and pressure conditions to obtain a coating containing a sensitive substance; 33-50 wt% of polymer particles and 50-67 wt% of plasticizer are mixed at room temperature and normal pressure to obtain a mixed solution; the mixed solution is then heated at 0.02-0.06 mL / cm 2 Adding the bottom of a flat plate, keeping the temperature at 80-120° C. for 10-30 min, and cooling naturally to obtain a polymer substrate film; The plasticizer in the raw material is the same as the plasticizer in the mixed solution; The polymer substrate film is cut into a rectangular plane, and then the coating containing the sensitive substance is coated on the surface of the polymer substrate film of the rectangular plane, and left to stand at room temperature for 5 to 10 minutes to obtain an ion selective electrode sensitive membrane.
2. The method for preparing an ion-selective electrode sensitive membrane according to claim 1, It is characterized in that The plasticizer is one of o-nitrophenyl octyl ether, dioctyl phthalate and dioctyl sebacate.
3. The method for preparing an ion-selective electrode sensitive membrane according to claim 1, Features: The ion carrier is a potassium ion carrier or a sodium ion carrier.
4. The method for preparing an ion-selective electrode sensitive membrane according to claim 1, Features: The ion exchanger is one of potassium tetrakis(4-chlorophenyl)borate and sodium tetrakis(4-chlorophenyl)borate.
5. The method for preparing an ion-selective electrode sensitive membrane according to claim 1, Features: The polymer particles are one of polyvinyl chloride, cellulose acetate and polyurethane.
6. The method for preparing an ion-selective electrode sensitive membrane according to claim 1, Features: The coating method is one of brushing, dipping and spraying; each plane is brushed 3 to 5 times, and each plane is sprayed 3 to 4 times. After the solvent evaporates to form a coating, it is turned over and brushed or sprayed; the number of dipping is 2 to 3 times, and the time of each dipping is 1 to 2 seconds.
7. The method for preparing an ion-selective electrode sensitive membrane according to claim 1, Features: The length×width of the rectangle is 5-8×6-9 mm.
8. An ion selective electrode sensitive membrane, Features The ion selective electrode sensitive membrane is an ion selective electrode sensitive membrane prepared by the method for preparing an ion selective electrode sensitive membrane according to any one of claims 1 to 7; The thickness of the ion selective electrode sensitive membrane is 0.1-0.3 mm.