Spraying-free PP material and preparation method thereof
By using technical means such as hyperbranched resin and glycidyl maleic anhydride in spray-free PP materials, the problem of poor dispersion of glossy materials in spray-free PP materials has been solved, high gloss and uniform surface effects have been achieved, and the Impact resistance of materials.
Patent Information
- Application Number
- CN202410960377.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
AI Technical Summary
Existing spray-free PP materials have shear sensitivity and orientation problems when adding gloss materials, resulting in uneven surface color and unable to achieve the gloss effect of spray materials.
Hyperbranched resin and glycidyl maleopimaric anhydride are used to prepare spray-free pigment masterbatch, which is combined with metallocene-catalyzed polyethylene wax and compatibilizer to improve the dispersion of pearlescent pigments through chemical and physical bonding and cross-linking reactions. and compatibility, reduce flow marks and weld marks, and enhance the gloss and impact resistance of the material.
It improves the surface metallic gloss effect, reduces flow marks and weld marks, improves the gloss and impact resistance of the material, and improves the surface quality.
Smart Images

Figure BDA0004950084080000041 
Figure BDA0004950084080000051 
Figure BDA0004950084080000063
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of spray-free materials, and in particular to a spray-free PP material and a preparation method thereof. Background Art
[0002] Polypropylene materials are widely used in the automotive and home appliance fields due to their light weight, good chemical resistance, heat resistance and excellent processability. As national environmental protection requirements become increasingly stringent, ABS, which was previously used for electroplating or painting, has gradually been replaced by spray-free PP materials due to its disadvantages such as large environmental pollution and easy scrap rate. Spray-free PP materials are often used to prepare home appliance exterior parts due to their good appearance and high gloss. With the introduction of the automotive ELV decree, more thermoplastic materials are needed that can be directly recycled without the need to separate the thermosetting paint film. Therefore, it is of great significance to research and develop spray-free materials.
[0003] The main way to achieve a high gloss effect without spraying on plastic products is to add gloss pigments to the material. However, adding gloss materials, such as metallic pigments and pearlescent pigments, has problems of shear sensitivity, orientation and accumulation. The problem of pigment accumulation in places where the product has many structural features and where the flow converges causes uneven surface color, resulting in the final surface quality of the spray-free product being far inferior to that of the spray-free material. Therefore, it is of great significance to the development of spray-free materials to study a high-gloss spray-free PP material to improve the appearance of flow marks and weld lines. Summary of the invention
[0004] In order to solve the above technical problems, a spray-free PP material with good surface metallic gloss effect and less prone to flow marks is developed. The present application provides a spray-free PP material and a preparation method.
[0005] In the first aspect, the present application provides a spray-free PP material, wherein the content of each component in the spray-free PP material is: 2-5 parts of spray-free pigment masterbatch, 90-120 parts of polypropylene, 3-10 parts of compatibilizer, 0.2-0.8 parts of lubricant, 6-10 parts of inorganic filler, and 0.3-0.6 parts of antioxidant; the content of each component in the spray-free pigment masterbatch is: 60-80 parts of spray-free pearlescent pigment, 3-8 parts of hyperbranched resin, and 20-30 parts of dispersant.
[0006] Furthermore, the dispersant is a metallocene-catalyzed polyethylene wax with a number average molecular weight of 2000-4000.
[0007] Furthermore, the hyperbranched resin includes one or more of hyperbranched polyester, hyperbranched polyamide, hyperbranched polyester amide, hyperbranched polyimide ester or hyperbranched polysiloxane, and the branching degree of the hyperbranched resin is 0.3-1.
[0008] By adopting the above technical scheme, by using hyperbranched resin to prepare spray-free pigment masterbatch, a large number of active groups such as hydroxyl, carboxyl, amino, etc. may exist on the surface of the hyperbranched polymer, which can form certain chemical and physical bonds with the spray-free pearlescent pigment during the mixing process, thereby making the spray-free pearlescent pigment better dispersed and more compatible with the resin, which can reduce the flipping of the spray-free effect pigment, thereby reducing weld marks and flow marks and optimizing the appearance effect.
[0009] Furthermore, the melt index of the polypropylene is 60-150 g / 10 min.
[0010] Furthermore, the inorganic filler includes one or more of talc, calcium carbonate, barium sulfate, and silica.
[0011] Preferably, the inorganic filler comprises barium sulfate and talc in a weight ratio of 5:3.
[0012] Furthermore, the particle size of the inorganic filler is 2500-4000 mesh.
[0013] By adopting the above technical scheme, barium sulfate as an inorganic filler is fine, uniform, high in whiteness, and has good optical properties, which can enhance the rigidity, toughness and gloss retention of the material; the main component of talcum powder is talcum powder containing hydrated magnesium silicate, which has the advantages of good lubricity and strong insulation, and can reduce the thermal expansion of the material; compounding the two as an inorganic filler and adding them to the PP material is beneficial to enhancing the strength and chemical stability of the material while maintaining its surface optical effect.
[0014] Further, the compatibilizer includes a first compatibilizer and a second compatibilizer in a weight ratio of 1-2:2-4, the first compatibilizer includes one or more of polypropylene grafted maleic anhydride, ethylene-vinyl acetate grafted maleic anhydride, polyethylene grafted maleic anhydride, and ethylene-octene copolymer grafted maleic anhydride; the second compatibilizer includes one or more of ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-propyl acrylate copolymer, ethylene-propyl methacrylate copolymer, ethylene-n-butyl acrylate copolymer and ethylene-n-butyl methacrylate copolymer.
[0015] Preferably, the compatibilizer includes a first compatibilizer and a second compatibilizer in a weight ratio of 1.5:2.5.
[0016] Preferably, the compatibilizer comprises a first compatibilizer and a second compatibilizer in a weight ratio of 1.5:2.5, the first compatibilizer is selected from polypropylene grafted maleic anhydride, and the second compatibilizer is selected from ethylene-methacrylic acid copolymer.
[0017] By adopting the above technical solution, if metal pigments or pearlescent pigments are directly added to the PP substrate, the notched impact strength thereof will be greatly reduced relative to that of pure PP materials, thereby increasing the risk of cracking or breaking of parts made of spray-free PP materials when subjected to strong external impact. Pearlescent pigments are inorganic pigments and generally have poor compatibility with plastics. In this application, two compatibilizers are compounded and used, wherein the second compatibilizer has a strong polarity and good compatibility with pearlescent pigments. The first compatibilizer cross-links with the polypropylene molecular chain during heating to improve the strength of the polypropylene matrix material, thereby achieving the technical effect of promoting the dispersibility of pearlescent pigments in the polypropylene matrix material and improving the impact resistance of the spray-free PP material.
[0018] Furthermore, the spray-free pigment masterbatch further comprises 9-15 parts by weight of maleopimaric anhydride glycidyl ester and 5-10 parts by weight of polyvinyl alcohol.
[0019] Preferably, the spray-free pigment masterbatch further comprises 14 parts by weight of glycidyl maleopimaric anhydride and 8 parts by weight of polyvinyl alcohol.
[0020] By adopting the above technical scheme, the spray-free pearlescent pigment is coated and modified with maleopimaric anhydride glycidyl ester and polyvinyl alcohol, and the epoxy group is opened under heating conditions to cross-link with polyvinyl alcohol, thereby improving the dispersibility of the spray-free pearlescent pigment in the PP material. Maleopimaric anhydride glycidyl ester, as an epoxy resin, will copolymerize with the hyperbranched resin in the masterbatch under heating conditions to generate macromolecules with a highly cross-linked network structure, so that the maleopimaric anhydride glycidyl ester coated modified spray-free pearlescent pigment is uniformly dispersed in the spray-free pigment masterbatch. Maleopimaric anhydride glycidyl ester can be well combined with the compatibilizer, so that when the masterbatch is melt-mixed with the polypropylene matrix material, the modified spray-free pearlescent pigment in the maleopimaric anhydride glycidyl ester coated state can be well dispersed in the polypropylene matrix material under the action of the second compatibilizer and reduce the agglomeration effect under the cross-linking action of the first compatibilizer and the polypropylene molecular chain, thereby improving the dispersion speed of the spray-free pearlescent pigment in the polypropylene matrix and promoting the uniform distribution of the spray-free pearlescent pigment in the polypropylene matrix. In addition, maleopimaric anhydride glycidyl ester has good optical properties. Adding it to the spray-free PP material can increase the coloring rate of the material, so that adding the same amount of spray-free pearlescent pigment to the material can obtain higher gloss and stronger metallic texture, enhance the dispersibility of the spray-free pearlescent pigment in the material, thereby weakening the covering effect of inorganic fillers on the spray-free pearlescent pigment.
[0021] In a second aspect, the present application provides a method for preparing the above-mentioned spray-free PP material, comprising the following steps: S1, adding the spray-free pearlescent pigment, the hyperbranched resin and the dispersant into a mixer and mixing to obtain a first premix, and performing extrusion granulation to obtain a spray-free pigment masterbatch; S2, adding polypropylene, lubricant, inorganic filler, antioxidant and the spray-free pigment masterbatch prepared in step S1 into a mixer and mixing to prepare a second premix, and extruding and granulating to prepare a spray-free PP material.
[0022] Furthermore, in the step S1, when preparing the first premix, the mixer speed is 150-200 r / min, the mixing time is 10-15 min, and the extrusion temperature is 200-230°C; in the step S2, when preparing the second premix, the mixer speed is 350-500 r / min, the mixing time is 20-30 min, and the extrusion temperature is 220-250°C.
[0023] Furthermore, the method for preparing the spray-free PP material comprises the following steps: S1. In a reaction container, maleopimaric anhydride glycidyl ester, polyethylene glycol and water in a weight ratio of 1:1:4 are mixed, heated to 70-85°C and stirred for 30-50 minutes, and cooled to obtain a premixed solution; tetraethyl orthosilicate and water in a weight ratio of 1:6 are added to another reaction container, the pH is adjusted to 2-3, and stirred at 35°C until the liquid is clear and transparent to obtain a hydrolyzate; the spray-free pearlescent pigment is added to the premixed solution, ultrasonicated, the hydrolyzate is added, stirred to obtain a suspension, filtered to obtain a residue, and dried to obtain a modified spray-free pearlescent pigment; S2, adding the hyperbranched resin, the dispersant and the modified spray-free pearlescent pigment prepared in step S1 into a mixer, mixing to prepare a first premix, and performing extrusion granulation to prepare a spray-free pigment masterbatch; S3, adding polypropylene, lubricant, inorganic filler, antioxidant and the spray-free pigment masterbatch prepared in step S2 into a mixer and mixing to prepare a second premix, and then extruding and granulating to prepare a spray-free PP material.
[0024] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The spray-free PP material prepared in the present application is used to prepare the spray-free pigment masterbatch by compounding hyperbranched resin, metallocene polyethylene wax and glycidyl maleopimaric anhydride, and two compatibilizers are used to enhance the dispersibility of the pearlescent pigment in the PP material. The glycidyl maleopimaric anhydride has low crystallinity and has a good dispersion effect when coating the spray-free pigment, thereby reducing the risk of the spray-free pearlescent pigment being sheared and agglomerated, and improving the metallic gloss of the product; 2. The preparation method of the spray-free PP material in this application is simple, easy and low-cost. DETAILED DESCRIPTION
[0025] The present application designs a spray-free PP material, in which the contents of the components are: 2-5 parts of spray-free pigment masterbatch, 90-120 parts of polypropylene, 3-10 parts of compatibilizer, 0.2-0.8 parts of lubricant, 6-10 parts of inorganic filler, and 0.3-0.6 parts of antioxidant; the contents of the components in the spray-free pigment masterbatch are: 60-80 parts of spray-free pearlescent pigment, 3-8 parts of hyperbranched resin, and 20-30 parts of dispersant.
[0026] The spray-free PP material in this application is prepared by the following method, including the following steps: S1, adding the spray-free pearlescent pigment, the hyperbranched resin and the dispersant into a mixer and mixing to obtain a first premix, and performing extrusion granulation to obtain a spray-free pigment masterbatch; S2, adding polypropylene, lubricant, inorganic filler, antioxidant and the spray-free pigment masterbatch prepared in step S1 into a mixer and mixing to prepare a second premix, and extruding and granulating to prepare a spray-free PP material.
[0027] The technical problem solved by the present application is to achieve a spray-free and high-gloss effect on plastic products, which is mainly achieved by adding gloss pigments to the material. However, when adding gloss materials, such as metallic pigments and pearlescent pigments, there are problems of shear sensitivity, orientation and accumulation. The problem of pigment accumulation in places where the product has many structural features and where the flow converges causes the surface color to be uneven, resulting in the surface quality of the final spray-free product being far inferior to that of the spray-coated material. The present application uses a hyperbranched resin, metallocene polyethylene wax and maleopimaric anhydride glycidyl ester in the preparation of spray-free pigment masterbatch. The two compatibilizers are used in combination to enhance the dispersibility of pearlescent pigments in PP materials. Maleopimaric anhydride glycidyl ester has low crystallinity and has a good dispersion effect when coated with spray-free pigments. At the same time, it can also reduce the risk of spray-free pearlescent pigments being sheared and agglomerated, thereby improving the metallic gloss of the product.
[0028] The present application is further described in detail below in conjunction with embodiments.
[0029] Preparation Example 1-5 Preparation Examples 1-5 are spray-free pigment masterbatches prepared with different raw material ratios. The specific raw material ratios are shown in Table 1.
[0030] Table 1 Among them, the spray-free pearlescent pigment uses aluminum silver powder surface treated with silane coupling agent KH-550.
[0031] The hyperbranched resin is a model of HyPer HPN 202 purchased from Wuhan Hyperbranched Resin Technology Co., Ltd., with a molecular weight of about 2700 g / mol and 12 moles of hydroxyl groups per mole. It is a high molecular weight, highly active terminal hydroxyl hyperbranched polymer with an aromatic polyamide hyperbranched polymer as the skeleton, and a branching degree of 0.5.
[0032] The dispersant is polyethylene wax catalyzed by metallocene with a number average molecular weight of 3,000.
[0033] The preparation method of Preparation Example 1-5 comprises the following steps: The spray-free pearlescent pigment, hyperbranched resin and dispersant are added into a mixer and mixed to obtain a first premix, which is then extruded and granulated to obtain a spray-free pigment masterbatch; wherein the mixer speed is set to 160 r / min, the mixing time is set to 15 min, and the extrusion temperature is set to 220°C.
[0034] Preparation Example 6 Preparation Example 6 is based on Preparation Example 2, except that Preparation Example 6 further includes 14 parts by weight of glycidyl maleopimaric anhydride and 8 parts by weight of polyvinyl alcohol.
[0035] The preparation method of Preparation Example 6 comprises the following steps: In a reaction container, glycidyl maleopimaric anhydride, polyvinyl alcohol and a spray-free pearlescent pigment are mixed, heated to 80°C and stirred for 40 minutes to obtain a modified spray-free pearlescent pigment; then, the modified spray-free pearlescent pigment, a hyperbranched resin and a dispersant are added to a mixer and mixed to obtain a first premix, which is then extruded and granulated to obtain a spray-free pigment masterbatch; wherein the mixer speed is set to 160 r / min, the mixing time is set to 15 minutes, and the extrusion temperature is set to 220°C.
[0036] Examples 1-6 Examples 1-6 include the following raw materials in parts by weight: 4 parts of spray-free pigment masterbatch, 100 parts of polypropylene, 8 parts of compatibilizer, 0.3 parts of lubricant, 8 parts of inorganic filler, and 0.4 parts of antioxidant.
[0037] The difference between Examples 1-6 is that different spray-free pigment masterbatches are used. The spray-free pigment masterbatches used in Examples 1-6 correspond to Preparation Examples 1-6 in sequence: The spray-free pigment masterbatch used in Example 1 is Preparation Example 1; The spray-free pigment masterbatch used in Example 2 is Preparation Example 2; The spray-free pigment masterbatch used in Example 3 is Preparation Example 3; The spray-free pigment masterbatch used in Example 4 is Preparation Example 4; The spray-free pigment masterbatch used in Example 5 is Preparation Example 5; The spray-free pigment masterbatch used in Example 6 is Preparation Example 6.
[0038] The compatibilizers used in Examples 1-6 are the first compatibilizer and the second compatibilizer in a weight ratio of 1.5:2.5, wherein the first compatibilizer is polypropylene grafted with maleic anhydride (purchased from Clariant Chemicals, model PP MA 6452, viscosity at 170°C is about 1200 mPa·s, softening point is 146°C), the second compatibilizer is ethylene-methacrylic acid copolymer (DuPont 0609HSA, containing 6.5 wt% MAA), that is, the compatibilizer used in Examples 1-6 includes 3 parts by weight of polypropylene grafted maleic anhydride and 5 parts by weight of ethylene-methacrylic acid copolymer.
[0039] The lubricant used in Examples 1 to 6 was Kao lubricant EBS-FF.
[0040] The inorganic filler used in Examples 1-6 is barium sulfate and talc in a weight ratio of 5:3.
[0041] The antioxidant used in Examples 1-6 is a mixture of 0.2 parts by weight of antioxidant 1010 and 0.2 parts by weight of antioxidant 168.
[0042] The melt index of the polypropylene used in Examples 1 to 6 was 120 g / 10 min.
[0043] The preparation process of Examples 1-6 comprises the following steps: Polypropylene, lubricant, inorganic filler, antioxidant and spray-free pigment masterbatch are added into a mixer to mix to obtain a second premix, which is then extruded and granulated to obtain a spray-free PP material. When preparing the second premix, the mixer speed is 450 r / min, the mixing time is 25 min, and the extrusion temperature is 240°C.
[0044] Examples 7-10 Examples 7-10 are spray-free PP materials made with different raw material ratios, which are based on Example 6, except that the raw material ratios are different, as shown in Table 2.
[0045] Table 2 Examples 11-12 Example 11 is based on Example 6, except that the melt index of the polypropylene in Example 11 is 60 g / 10 min.
[0046] Example 12 is based on Example 6, except that the melt index of the polypropylene in Example 12 is 150 g / 10 min.
[0047] Embodiment 13 Example 13 is based on Example 6, except that the inorganic filler in Example 13 is changed to calcium carbonate and talc in a weight ratio of 5:3.
[0048] Examples 14-17 Example 14 is based on Example 6, except that the compatibilizer in Example 14 uses 3 parts by weight of ethylene-octene copolymer grafted with maleic anhydride (purchased from Shanghai Jiayirong Polymer, model number CMG5805) and 5 parts by weight of ethylene-methacrylic acid copolymer.
[0049] Example 15 is based on Example 6, except that the compatibilizer in Example 15 uses 3 parts by weight of polypropylene grafted maleic anhydride and 5 parts by weight of ethylene-methyl methacrylate copolymer (purchased from Sumitomo Chemical of Japan, model number SWA330).
[0050] Example 16 is based on Example 6, except that the compatibilizer in Example 16 uses 3 parts by weight of polypropylene grafted maleic anhydride, 2 parts by weight of ethylene-methacrylic acid copolymer and 3 parts by weight of ethylene-methyl methacrylate copolymer.
[0051] Example 17 is based on Example 6, except that the compatibilizer in Example 17 uses 3 parts by weight of polypropylene grafted maleic anhydride, 2 parts by weight of ethylene-methacrylic acid copolymer and 3 parts by weight of ethylene-acrylic acid copolymer (purchased from DuPont, model number Nucrel EAA 3990, melt index: 10 g / 10 min, acrylic acid content of 9.5wt%).
[0052] Embodiment 18 Example 18 is based on Example 6, except that the glycidyl maleopimaric anhydride in the spray-free pigment masterbatch is replaced with epoxy resin (the epoxy resin is bisphenol A epoxy resin, model E-55).
[0053] Comparative Example 1 Comparative Example 1 is based on Example 6, except that no hyperbranched resin is added to the spray-free pigment masterbatch in Comparative Example 1.
[0054] Accordingly, the spray-free PP material in Comparative Example 1 includes the following raw materials in parts by weight: 4 parts by weight of spray-free pigment masterbatch, 100 parts by weight of polypropylene, 8 parts by weight of compatibilizer, 0.3 parts by weight of lubricant, 8 parts by weight of inorganic filler, and 0.4 parts by weight of antioxidant; wherein, the raw materials in the spray-free pigment masterbatch include: 75 parts by weight of spray-free pearlescent pigment, 25 parts by weight of metallocene-catalyzed polyethylene wax, 14 parts by weight of maleopimaric anhydride glycidyl ester, and 8 parts by weight of polyvinyl alcohol.
[0055] The preparation method of the spray-free pigment masterbatch in Comparative Example 1 comprises the following steps: In a reaction container, glycidyl maleopimaric anhydride, polyvinyl alcohol and a spray-free pearlescent pigment are mixed, heated to 80°C and stirred for 40 minutes to obtain a modified spray-free pearlescent pigment; then, the modified spray-free pearlescent pigment and metallocene-catalyzed polyethylene wax are added to a mixer and mixed to obtain a first premix, which is then extruded and granulated to obtain a spray-free pigment masterbatch; wherein the mixer speed is set to 160 r / min, the mixing time is set to 15 minutes, and the extrusion temperature is set to 280°C.
[0056] Comparative Example 2 Comparative Example 2 is based on Example 6, except that the hyperbranched resin in the spray-free pigment masterbatch in Comparative Example 2 is replaced by bisphenol A epoxy resin.
[0057] Accordingly, the spray-free PP material in Comparative Example 1 includes the following raw materials in parts by weight: 4 parts by weight of spray-free pigment masterbatch, 100 parts by weight of polypropylene, 8 parts by weight of compatibilizer, 0.3 parts by weight of lubricant, 8 parts by weight of inorganic filler, and 0.4 parts by weight of antioxidant; wherein, the raw materials in the spray-free pigment masterbatch include: 75 parts by weight of spray-free pearlescent pigment, 5 parts by weight of bisphenol A type epoxy resin, 25 parts by weight of metallocene-catalyzed polyethylene wax, 14 parts by weight of maleopimaric anhydride glycidyl ester, and 8 parts by weight of polyvinyl alcohol.
[0058] The preparation method of the spray-free pigment masterbatch in Comparative Example 2 comprises the following steps: In a reaction container, glycidyl maleopimaric anhydride, polyvinyl alcohol and a spray-free pearlescent pigment are mixed, heated to 80°C and stirred for 40 minutes to obtain a modified spray-free pearlescent pigment; then, the modified spray-free pearlescent pigment, bisphenol A epoxy resin and metallocene-catalyzed polyethylene wax are added to a mixer and mixed to obtain a first premix, which is then extruded and granulated to obtain a spray-free pigment masterbatch; wherein the mixer speed is set to 160 r / min, the mixing time is set to 15 minutes, and the extrusion temperature is set to 280°C.
[0059] Performance Testing 1. The spray-free PP materials prepared in Examples 1-18 and Comparative Examples 1-2 were injection molded into test pieces with a length*width of 1m*1m and a thickness of 3mm. The glossiness of the test pieces was tested using a universal 60° mirror gloss tester. Referring to the standard ASTM D2457-13, 10 test points were evenly selected on the surface of the test pieces to test the glossiness and gloss uniformity. The average glossiness and variance were calculated. The variance reflects the gloss uniformity. The test results are shown in Table 3.
[0060] Table 3 By analyzing the data of Table 3, it can be obtained that the gloss of the spray-free PP material prepared in Examples 1-18 of the present application is good, and the gloss of multiple sampling points is uniform, and the gloss uniformity of the test piece surface is good. Comparing Example 6 with Example 1-5, it can be obtained that after the spray-free pearlescent pigment is coated and modified by maleopimaric anhydride glycidyl ester and polyvinyl alcohol, the gloss of the test piece surface and the uniformity of the surface gloss are significantly improved. Comparing Example 6 with Comparative Examples 1-2, it can be obtained that the addition of hyperbranched resin has an important effect on the gloss and uniformity of the prepared spray-free PP material. Comparing Example 6 with Examples 14-17, it can be obtained that the type selection and specific ratio of the compatibilizer have a significant effect on the gloss and gloss uniformity of the spray-free PP material prepared in the present application. It can be seen that the addition of the compatibilizer is conducive to improving the problem of pigment accumulation and uneven surface color of the final product when the spray-free PP material is injected.
[0061] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A spray-free PP material, characterized in that: The content of each component in the spray-free PP material is: 2-5 parts of spray-free pigment masterbatch, 90-120 parts of polypropylene, 3-10 parts of compatibilizer, 0.2-0.8 parts of lubricant, 6-10 parts of inorganic filler, 0.3-0.6 parts of antioxidant; The contents of the components in the spray-free pigment masterbatch are: 60-80 parts of the spray-free pearlescent pigment, 3-8 parts of the hyperbranched resin, and 20-30 parts of the dispersant.
2. The spray-free PP material according to claim 1, characterized in that: The dispersant is a metallocene-catalyzed polyethylene wax with a number average molecular weight of 2000-4000.
3. The spray-free PP material according to claim 1, characterized in that: The hyperbranched resin includes one or more of hyperbranched polyester, hyperbranched polyamide, hyperbranched polyesteramide, hyperbranched polyimide ester or hyperbranched polysiloxane, and the branching degree of the hyperbranched resin is 0.3-1.
4. The spray-free PP material according to claim 1, characterized in that: The melt index of the polypropylene is 60-150 g / 10 min.
5. The spray-free PP material according to claim 1, characterized in that: The inorganic filler includes one or more of talc, calcium carbonate, barium sulfate and silica.
6. The spray-free PP material according to claim 5, characterized in that: The particle size of the inorganic filler is 2500-4000 mesh.
7. The spray-free PP material according to claim 1, characterized in that: The compatibilizer includes a first compatibilizer and a second compatibilizer in a weight ratio of 1-2:2-4, wherein the first compatibilizer includes one or more of polypropylene grafted maleic anhydride, ethylene-vinyl acetate grafted maleic anhydride, polyethylene grafted maleic anhydride, and ethylene-octene copolymer grafted maleic anhydride; the second compatibilizer includes one or more of ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-propyl acrylate copolymer, ethylene-propyl methacrylate copolymer, ethylene-n-butyl acrylate copolymer and ethylene-n-butyl methacrylate copolymer.
8. The spray-free PP material according to claim 1, characterized in that: The spray-free pigment masterbatch further comprises 9-15 parts by weight of glycidyl maleopimaric anhydride and 5-10 parts by weight of polyvinyl alcohol.
9. A method for preparing the spray-free PP material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, adding the spray-free pearlescent pigment, the hyperbranched resin and the dispersant into a mixer and mixing to obtain a first premix, and performing extrusion granulation to obtain a spray-free pigment masterbatch; S2, adding polypropylene, lubricant, inorganic filler, antioxidant and the spray-free pigment masterbatch prepared in step S1 into a mixer and mixing to prepare a second premix, and extruding and granulating to prepare a spray-free PP material.
10. The method for preparing the spray-free PP material according to claim 9, characterized in that: The following steps are involved: S1. In a reaction vessel, maleopimaric anhydride glycidyl ester, polyvinyl alcohol and a spray-free pearlescent pigment are mixed, heated to 70-85° C. and stirred for 30-50 minutes to prepare a modified spray-free pearlescent pigment; S2, adding the hyperbranched resin, the dispersant and the modified spray-free pearlescent pigment prepared in step S1 into a mixer, mixing to prepare a first premix, and performing extrusion granulation to prepare a spray-free pigment masterbatch; S3, adding polypropylene, lubricant, inorganic filler, antioxidant and the spray-free pigment masterbatch prepared in step S2 into a mixer and mixing to prepare a second premix, and then extruding and granulating to prepare a spray-free PP material.