Low-dielectric high-strength high-modulus fiber reinforced resin-based prepreg, composite material and method
By plasma pre-treating the composite of PBO fiber and modified fluorine-containing cyanate resin, a low-dielectric, high-strength and high-modulus fiber-reinforced resin-based composite material is prepared, which solves the problem of insufficient dielectric properties and mechanical properties of existing materials and achieves It improves the performance of radar radomes and high-frequency and high-speed copper-clad laminates, and provides materials and processes with excellent comprehensive properties such as high frequency, low dielectric, high temperature resistance, high strength, and high modulus.
Patent Information
- Application Number
- CN202410856053.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
AI Technical Summary
The dielectric and mechanical properties of fiber-reinforced resin-based composite materials used in existing radar radomes and high-frequency and high-speed copper-clad laminates cannot meet the improvement needs of the new generation of radar radomes and high-frequency and high-speed copper-clad laminates. The dielectric constant and loss tangent are relatively low. High, and the mechanical tensile modulus is insufficient.
The high-modulus PBO fiber fabric is composited with modified fluorine-containing cyanate resin by plasma pretreatment, and the low-dielectric, high-strength and high-modulus fiber-reinforced resin-based prepreg is prepared by hot melt method or solution impregnation method, combined with hot pressing or no Hot pressing molding process prepares composite materials with high frequency, low dielectric, high temperature resistance, high strength and high modulus.
It achieves the reduction of dielectric constant, loss tangent, improvement of tensile strength and modulus, and increase of glass transition temperature of composite materials, providing a material and process basis for improving the performance of radar radomes and high-frequency and high-speed copper-clad laminates. At the same time, It has excellent comprehensive performance.
Smart Images

Figure CN118755264A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wave-transmitting composite materials, and in particular to a high-frequency, low-dielectric, high-temperature-resistant, high-strength, high-modulus poly(p-phenylene benzobisoxazole) (PBO) fiber fabric-reinforced modified fluorinated cyanate resin prepreg, composite material and preparation method thereof for radar antenna covers and high-frequency and high-speed copper-clad laminates. Background Art
[0002] Radomes are generally made of high-frequency, low-dielectric, high-temperature-resistant, high-strength fiber-reinforced resin composite wave-transparent skin materials and sandwich materials through appropriate molding and processing processes. They are the most important electromagnetic wave-transparent windows for aircraft. The dielectric properties (dielectric constant and loss tangent) of the composite materials used to manufacture radar antenna covers directly affect their wave-transparent performance. The larger the dielectric loss tangent, the more energy the electromagnetic wave energy is converted into heat and lost during the process of passing through the radar cover. The larger the dielectric constant, the greater the reflection of the electromagnetic wave at the interface between the air and the dielectric cover wall, which will increase the mirror lobe level and reduce the transmission efficiency. Therefore, in order to achieve the purpose of maximum transmission and minimum reflection, the dielectric loss tangent of the radar cover composite material is required to be close to zero and the dielectric constant is as low as possible; as the aircraft develops towards high speed, the aerodynamic heating effect is stronger, which puts higher requirements on the heat resistance of the composite material; in addition, the higher mechanical strength and modulus of the composite material can ensure a higher damage tolerance of the structural parts and can design the skin to be thinner and lighter, so there is an urgent need to improve the strength and modulus of the composite material. In summary, the development of radar antenna covers urgently requires high-frequency, low-dielectric, high-temperature-resistant, high-strength and high-modulus fiber-reinforced resin-based composite materials. As printed circuit boards (PCBs) develop towards high frequency, high speed, high precision and high multi-layering, higher requirements are also placed on the dielectric, heat resistance and deformation resistance of fiber-reinforced resin substrates for high-frequency and high-speed copper-clad laminates.
[0003] At present, the relatively mature low-dielectric reinforcement fibers in the fields of radar antenna covers and high-frequency and high-speed copper-clad laminates are mainly low-dielectric quartz / glass fibers, whose mechanical tensile modulus is less than 80GPa, and the dielectric constant of quartz / glass fibers is ≥3.7, and the tensile modulus of the composite materials manufactured is less than 25GPa; the relatively mature resin matrices are mainly multifunctional epoxy resin systems, modified bismaleimide resin systems, and cyanate resins, and the dielectric constant is limited to the level of 2.85-4.0 (10GHz), and the dielectric properties of the composite materials prepared therefrom (dielectric constant ≥3.2, loss factor <10 -2 ) is relatively high, which can no longer meet the requirements of the new generation of radar antenna covers, high-frequency and high-speed copper-clad laminates for the dielectric and mechanical properties of composite materials. Summary of the invention
[0004] The purpose of the present invention is to provide a low-dielectric, high-strength, high-modulus fiber-reinforced resin-based prepreg, composite material and method. The present invention has the characteristics of high frequency, low dielectric, high temperature resistance, high strength, high modulus, etc., showing excellent comprehensive performance, and provides a material and process basis for improving the performance of radar antenna cover and high-frequency and high-speed copper cladding.
[0005] Technical solution: A low dielectric high strength high modulus fiber reinforced resin based prepreg is made from the following raw materials:
[0006] Fluorinated cyanate resin: 100 parts, epoxy resin: 1 to 10 parts,
[0007] Active hydrogen catalyst: 1 to 5 parts; Plasma pretreated high modulus PBO fiber fabric: several parts;
[0008] The glue content of the prepared prepreg is 30% to 50%.
[0009] In the aforementioned low-dielectric high-strength high-modulus fiber-reinforced resin-based prepreg, the fluorine-containing cyanate resin includes one or more of bisphenol D cyanate, bisphenol H cyanate and bisphenol T cyanate.
[0010] In the aforementioned low-dielectric high-strength high-modulus fiber-reinforced resin-based prepreg, the epoxy resin includes one or more of TDE85, TTA21P and E-51 epoxy resins.
[0011] In the aforementioned low-dielectric high-strength high-modulus fiber-reinforced resin-based prepreg, the active hydrogen catalyst includes one or more of triethylenediamine, p-hydroxybiphenyl, nonylphenol, phenol and p-tert-butylphenol.
[0012] The method for preparing the aforementioned low dielectric high strength high modulus fiber reinforced resin based prepreg comprises the following steps:
[0013] S1. Preparing a number of plasma pretreated high modulus PBO fiber fabrics;
[0014] S2. Adding epoxy resin to the molten fluorine-containing cyanate resin, followed by adding an active hydrogen catalyst, prepolymerizing at 120 ℃ ~ 150 ℃ for 5min ~ 60min to obtain a modified cyanate resin;
[0015] S3. A prepreg with a glue content of 30% to 50% is prepared by pretreating high modulus PBO fiber fabric with modified cyanate resin and plasma.
[0016] In the aforementioned method for preparing low dielectric high strength high modulus fiber reinforced resin-based prepreg, step S3 is specifically as follows: using hot melt prepreg manufacturing technology, plasma pretreated high modulus PBO fiber fabric and modified cyanate ester resin are compounded to prepare a hot melt prepreg with a glue content of 30% to 50%.
[0017] In the aforementioned method for preparing low-dielectric, high-strength, high-modulus fiber-reinforced resin-based prepreg, step S3 is specifically as follows: dissolving the modified cyanate ester resin in acetone, butanone or dichloroethane solvent to prepare a solution with a solid content of 50% to 80%, and manufacturing a prepreg with a glue content of 30% to 50% by solution impregnation prepreg manufacturing technology.
[0018] The composite material prepared based on the aforementioned low-dielectric high-strength high-modulus fiber-reinforced resin-based prepreg is prepared by curing and molding the low-dielectric high-strength high-modulus fiber-reinforced resin-based prepreg.
[0019] In the aforementioned composite material, the curing molding adopts a hot pressing curing molding process, and the process parameters are as follows: vacuum degree is 0.05MPa~0.09MPa, external pressure is 0.1MPa~0.5MPa, and curing temperature parameters are (130℃~150℃)×(2h~4h)+(180℃~210℃)×(6h~12h).
[0020] In the aforementioned composite material, the process parameters for curing molding are as follows: the vacuum degree is 0.05MPa~0.09MPa, and the curing temperature parameters are (130℃~150℃)×(2h~4h)+(180℃~210℃)×(6h~12h).
[0021] Beneficial effects: In view of the urgent need for high-frequency, low-dielectric, high-temperature-resistant, high-strength and high-modulus fiber-reinforced resin-based composite materials for radar antenna covers and high-frequency and high-speed copper-clad laminates, the present invention provides a PBO fiber-reinforced modified fluorine-containing cyanate resin prepreg, a composite material and a preparation method thereof. The high-modulus PBO fiber fabric pretreated with plasma is used as a reinforcement, and a modified fluorine-containing low-dielectric cyanate resin is used as a resin matrix. The reinforcement and the resin matrix are compounded by a hot melt method or a solution impregnation method prepreg manufacturing technology to prepare a prepreg, and the composite material is cured and formed by an autoclave or an autoclave-free molding (OOA) process. The composite material has the characteristics of high-frequency, low-dielectric, high-temperature resistance, high strength, high modulus and the like, and exhibits excellent comprehensive performance. The technical problems of high dielectric constant, low strength and low modulus of glass fiber / quartz fiber reinforced epoxy / BT / cyanate resin wave-transparent composite materials commonly used in radar antenna covers and high-frequency and high-speed copper-clad laminates at this stage are solved, and the material and process basis are provided for improving the performance of radar antenna covers and high-frequency and high-speed copper-clad laminates.
[0022] The invention is based on plasma pretreatment of high modulus PBO fiber fabrics and three fluorine-containing cyanate resin matrices. The modified low-dielectric fluorine-containing cyanate resin matrix is manufactured by toughening and low-temperature catalytic curing modification of epoxy resin and nonylphenol to fluorine-containing cyanate. The high modulus, high strength and low dielectric properties of the composite material are achieved by means of the low dielectric and high modulus of the PBO fiber. The low molecular polarization density, high temperature resistance and low dielectric properties of the modified fluorine-containing cyanate resin are utilized to give the composite material high strength, high temperature resistance and high strength properties. In addition, the PBO fiber fabric is plasma pretreated, and a large number of polar active groups are introduced on the surface, thereby ensuring a good interface bonding effect between the fiber and the resin matrix. The reinforcement and the modified resin matrix are compounded by hot melt or solution impregnation prepreg manufacturing technology to prepare a prepreg, which is then cured and formed into a composite material through an autoclave or out-of-autoclave molding (OOA) process. The prepared composite material has a dielectric constant of 2.80-2.90, a loss tangent of 0.004-0.007, a tensile strength of 775MPa-695MPa, a tensile modulus of 58GPa-69GPa, an interlaminar shear strength of 35MPa-43MPa, and a glass transition temperature of 210°C-240°C, showing excellent comprehensive properties such as high frequency and low dielectric, high temperature resistance, high strength and high modulus. This material can provide a material and process basis for improving the performance of radar antenna covers and high-frequency and high-speed copper clad laminates, and has broad application prospects in the fields of 5G communications and packaging substrates. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is the molecular structure of PBO fiber;
[0024] Figure 2 It is the molecular structure of bisphenol D, bisphenol H and bisphenol T cyanate resin;
[0025] Figure 3 It is the molecular structure of TDE85, TTA21P and E-51 epoxy resin;
[0026] Figure 4 Molecular structures of active hydrogen catalysts triethylenediamine, p-hydroxybiphenyl, nonylphenol, phenol and p-tert-butylphenol. DETAILED DESCRIPTION
[0027] Example 1
[0028] Prepare plasma pretreated high modulus PBO fiber fabrics; use 100 molecular structures such as Figure 2 The bisphenol D cyanate resin shown is melted and then added as Figure 3 1 part of E-51 epoxy resin and 5 parts of TTA21P epoxy resin were added. Figure 41 part of triethylenediamine and 5 parts of nonylphenol are prepolymerized at 120°C for 15 minutes to obtain a modified cyanate ester resin; a plasma pretreated high modulus PBO fiber fabric and a modified cyanate ester resin are compounded by hot melt prepreg manufacturing technology to prepare a prepreg with a glue content of 30%; a composite material is obtained by curing and molding through a hot autoclave molding process with a vacuum degree of 0.05MPa, an external pressure of 0.1MPa, and a curing temperature parameter of 130°C×2h+180°C×12h.
[0029] In this embodiment, the dielectric constant of the modified cyanate ester resin matrix is 2.54, the loss tangent is 0.004 (GB / T5597), the dielectric constant and loss tangent of the PBO fiber fabric reinforced modified cyanate ester resin are 2.89 and 0.006 (GB / T5597, 10GHz), respectively, the tensile strength is 760MPa, the tensile modulus is 66GPa (ASTM D3039), the interlaminar shear strength is 39MPa (ASTMD2344), and the glass transition temperature is 220°C (GB / T40396).
[0030] Example 2
[0031] Prepare plasma pretreated high modulus PBO fiber fabrics; use 100 molecular structures such as Figure 2 The bisphenol T cyanate ester resin shown is melted and then added as Figure 3 2 parts of TDE85 epoxy resin and 2 parts of TTA21P epoxy resin as shown, then add Figure 4 1 part of triethylenediamine and 2 parts of nonylphenol are prepolymerized at 150°C for 6 minutes to obtain a modified cyanate ester resin; the modified cyanate ester resin is dissolved in a mixed solvent of acetone and butanone to prepare a solution with a solid content of 50%, and a prepreg with a glue content of 50% is manufactured by a solution impregnation prepreg manufacturing technology; a composite material is obtained by curing and molding through a non-autoclave molding process with a vacuum degree of 0.09 MPa and a curing temperature parameter of 130°C×2h+200°C×8h.
[0032] In this embodiment, the dielectric constant of the modified cyanate ester resin matrix is 2.55, and the loss tangent is 0.003 (GB / T5597, 10GHz), the dielectric constant and loss tangent of the PBO fiber fabric reinforced modified cyanate ester resin are 2.85 and 0.004 (GB / T 5597, 10GHz), respectively, the tensile strength is 705MPa, the tensile modulus is 62GPa (ASTM D3039), the interlaminar shear strength is 35MPa (ASTM D2344), and the glass transition temperature is 210°C (GB / T 40396).
[0033] Example 3
[0034] Prepare plasma pretreated high modulus PBO fiber fabrics; use 100 molecular structures such as Figure 2 The bisphenol H cyanate resin shown is melted and then added as Figure 3 2 parts of TDE85 epoxy resin, 2 parts of TTA21P epoxy resin, 2 parts of E-51 epoxy resin, and then add Figure 4 1 part of p-hydroxyphenol and 2 parts of nonylphenol are prepolymerized at 130°C for 30 minutes to obtain a modified cyanate ester resin; the modified cyanate ester resin is dissolved in a mixed solvent of acetone and butanone to prepare a solution with a solid content of 80%, and a prepreg with a glue content of 45% is manufactured by a solution impregnation prepreg manufacturing technology; a composite material is obtained by curing and molding through a non-autoclave molding process with a vacuum degree of 0.09 MPa and a curing temperature parameter of 130°C×2h+210°C×10h.
[0035] In this embodiment, the dielectric constant of the modified cyanate ester resin matrix is 2.65, the loss tangent is 0.004 (GB / T5597, 10GHz), the dielectric constant and loss tangent of the PBO fiber fabric reinforced modified cyanate ester resin are 2.90 and 0.006 (GB / T 5597, 10GHz), respectively, the tensile strength is 775MPa, the tensile modulus is 69GPa (ASTM D3039), the interlaminar shear strength is 42MPa (ASTM D2344), and the glass transition temperature is 239°C (GB / T 40396).
[0036] Example 4
[0037] Prepare plasma pretreated high modulus PBO fiber fabrics; use 95 parts of molecular structure such as Figure 2 The bisphenol D cyanate resin shown and 5 parts of Figure 2 The bisphenol T cyanate ester resin shown is melted and then added as Figure 3 3 parts of TDE85 epoxy resin and 2 parts of TTA21P epoxy resin are added as shown. Figure 4 3 parts of nonylphenol and 1 part of p-tert-butylphenol are prepolymerized at 120°C for 60 minutes to obtain a modified cyanate ester resin; a plasma pretreated high modulus PBO fiber fabric and a modified cyanate ester resin are compounded by hot melt prepreg manufacturing technology to prepare a prepreg with a glue content of 42%; a composite material is obtained by curing and molding through a hot autoclave molding process with a vacuum degree of 0.09MPa, an external pressure of 0.1MPa, and a curing temperature parameter of 150°C×2h+200°C×10h.
[0038] In this embodiment, the dielectric constant of the modified cyanate resin matrix is 2.54, the loss tangent is 0.004 (GB / T5597), the dielectric constant and loss tangent of the PBO fiber fabric reinforced modified cyanate resin are 2.82 and 0.006 (GB / T5597, 10GHz), respectively, the tensile strength is 710MPa, the tensile modulus is 66GPa (ASTM D3039), the interlaminar shear strength is 43MPa (ASTMD2344), and the glass transition temperature is 240°C (GB / T40396).
[0039] Example 5
[0040] Prepare plasma pretreated high modulus PBO fiber fabrics; use 90 parts of molecular structure such as Figure 2 bisphenol D cyanate resin, 5 parts Figure 2 The bisphenol T cyanate resin shown and 5 parts of Figure 2 The bisphenol H cyanate resin shown in the figure is melted and then added as Figure 3 3 parts of E-51 epoxy resin and 2 parts of TTA21P epoxy resin are added. Figure 4 1 part of nonylphenol, 1 part of p-tert-butylphenol and 1 part of phenol as shown are prepolymerized at 130°C for 50 minutes to obtain a modified cyanate ester resin; a plasma pretreated high modulus PBO fiber fabric and a modified cyanate ester resin are compounded by hot melt prepreg manufacturing technology to prepare a prepreg with a glue content of 50%; a composite material is obtained by curing and molding through a hot autoclave molding process with a vacuum degree of 0.09MPa, an external pressure of 0.1MPa, and a curing temperature parameter of 150°C×2h+210°C×12h.
[0041] In this embodiment, the dielectric constant of the modified cyanate resin matrix is 2.59, the loss tangent is 0.005 (GB / T5597), the dielectric constant and loss tangent of the PBO fiber fabric reinforced modified cyanate resin are 2.80 and 0.006 respectively (GB / T5597, 10GHz), the tensile strength is 720MPa, the tensile modulus is 65GPa (ASTM D3039), the interlaminar shear strength is 40MPa (ASTMD2344), and the glass transition temperature is 235°C (GB / T40396).
[0042] Example 6
[0043] Prepare plasma pretreated high modulus PBO fiber fabrics; use 50 parts of molecular structure such as Figure 2 The bisphenol T cyanate resin shown and 50 parts of the molecular structure as Figure 2 The bisphenol H cyanate resin shown is melted and then added as Figure 32 parts of TDE85 epoxy resin, 2 parts of TTA21P epoxy resin and 2 parts of E51 epoxy resin as shown, then add Figure 4 1 part of triethylenediamine and 2 parts of nonylphenol are prepolymerized at 150°C for 40 minutes to obtain a modified cyanate ester resin; the modified cyanate ester resin is dissolved in dichloroethane solvent to prepare a solution with a solid content of 50%, and a prepreg with a glue content of 40% is manufactured by a solution impregnation prepreg manufacturing technology; a composite material is obtained by curing and molding through a hot autoclave molding process with a vacuum degree of 0.09MPa, a pressure of 0.30MPa, and a curing temperature parameter of 150°C×4h+200°C×8h.
[0044] In this embodiment, the dielectric constant of the modified cyanate ester resin matrix is 2.60, and the loss tangent is 0.005 (GB / T5597, 10GHz), the dielectric constant and loss tangent of the PBO fiber fabric reinforced modified cyanate ester resin are 2.90 and 0.007 (GB / T 5597, 10GHz), respectively, the tensile strength is 695MPa, the tensile modulus is 58GPa (ASTM D3039), the interlaminar shear strength is 35MPa (ASTM D2344), and the glass transition temperature is 221°C (GB / T 40396).
[0045] Example 7
[0046] A low dielectric, high strength and high modulus fiber reinforced resin prepreg, composite material and preparation method thereof, the steps are as follows:
[0047] 1. Prepare some plasma pretreated high modulus PBO fiber fabrics. The molecular structure of PBO fiber is as follows: Figure 1 As shown;
[0048] 2. Use 100 molecular structures such as Figure 2 The fluorinated cyanate resin shown in the figure is melted and then added with Figure 3 1 to 10 parts of epoxy resin as shown, then add Figure 4 1 to 5 parts of the active hydrogen catalyst shown above are prepolymerized at 120° C. to 150° C. for 5 to 60 minutes to obtain a modified cyanate ester resin;
[0049] 3. Using hot melt prepreg manufacturing technology, plasma pretreated high modulus PBO fiber fabric and modified cyanate resin are compounded to prepare hot melt prepreg with a glue content of 30% to 50%; or the modified cyanate resin is dissolved in acetone, butanone or dichloroethane solvent to prepare a solution with a solid content of 50% to 80%, and a prepreg with a glue content of 30% to 50% is manufactured by solution impregnation prepreg manufacturing technology.
[0050] 4. The composite material is obtained by a hot autoclave molding process with a vacuum degree of 0.05MPa to 0.09MPa, an external pressure of 0.1MPa to 0.5MPa, and a curing temperature parameter of (130°C to 150°C) × (2h to 4h) + (180°C to 210°C) × (6h to 12h); or the composite material is obtained by curing in an oven without a hot autoclave molding process with a vacuum degree of 0.05MPa to 0.09MPa and a curing temperature parameter of (130°C to 150°C) × (2h to 4h) + (180°C to 210°C) × (6h to 12h).
Claims
1. A low dielectric high strength high modulus fiber reinforced resin based prepreg, characterized in that: It is prepared from the following raw materials: Fluorinated cyanate resin: 100 parts, epoxy resin: 1 to 10 parts, Active hydrogen catalyst: 1 to 5 parts; Plasma pretreated high modulus PBO fiber fabric: several parts; The glue content of the prepared prepreg is 30% to 50%.
2. The low dielectric high strength high modulus fiber reinforced resin based prepreg according to claim 1, characterized in that: The fluorine-containing cyanate resin includes one or more of bisphenol D cyanate, bisphenol H cyanate and bisphenol T cyanate.
3. The low dielectric high strength high modulus fiber reinforced resin based prepreg according to claim 1, characterized in that: The epoxy resin includes one or more of TDE85, TTA21P and E-51 epoxy resins.
4. The low dielectric high strength high modulus fiber reinforced resin based prepreg according to claim 1, characterized in that: The active hydrogen catalyst includes one or more of triethylenediamine, p-hydroxybiphenyl, nonylphenol, phenol and p-tert-butylphenol.
5. A method for preparing a low dielectric high strength high modulus fiber reinforced resin based prepreg according to any one of claims 1 to 4, characterized in that: The steps include: S1. Preparing a number of plasma pretreated high modulus PBO fiber fabrics; S2. Adding epoxy resin to the molten fluorine-containing cyanate resin, followed by adding an active hydrogen catalyst, prepolymerizing at 120 ℃ ~ 150 ℃ for 5min ~ 60min to obtain a modified cyanate resin; S3. A prepreg with a glue content of 30% to 50% is prepared by pretreating high modulus PBO fiber fabric with modified cyanate resin and plasma.
6. The method for preparing the low dielectric high strength high modulus fiber reinforced resin based prepreg according to claim 5, characterized in that: Step S3 is specifically as follows: using hot melt prepreg manufacturing technology, the plasma pretreated high modulus PBO fiber fabric and the modified cyanate ester resin are compounded to prepare a hot melt prepreg with a glue content of 30% to 50%.
7. The method for preparing the low dielectric high strength high modulus fiber reinforced resin based prepreg according to claim 5, characterized in that: Step S3 is as follows: dissolving the modified cyanate ester resin in acetone, butanone or dichloroethane solvent to prepare a solution with a solid content of 50% to 80%, and manufacturing a prepreg with a glue content of 30% to 50% by solution impregnation prepreg manufacturing technology.
8. A composite material prepared based on the low dielectric high strength high modulus fiber reinforced resin based prepreg according to any one of claims 1 to 4, characterized in that: The invention is prepared by curing and molding the low-dielectric, high-strength and high-modulus fiber-reinforced resin-based prepreg.
9. The composite material according to claim 8, characterized in that The curing molding adopts a hot pressing curing molding process, and the process parameters are as follows: vacuum degree is 0.05MPa~0.09MPa, external pressure is 0.1MPa~0.5MPa, and curing temperature parameters are (130℃~150℃)×(2h~4h)+(180℃~210℃)×(6h~12h).
10. The composite material according to claim 8, characterized in that The process parameters of curing molding are as follows: vacuum degree is 0.05MPa~0.09MPa, and curing temperature parameters are (130℃~150℃)×(2h~4h)+(180℃~210℃)×(6h~12h).