Anti-pollution flashover coating
By optimizing the anti-fouling flashover coating formula, the mechanical properties and aging resistance of the coating are improved, the aging problem caused by ultraviolet radiation in the existing technology is solved, the service life is extended and the flame retardant performance is enhanced, and the stable operation of the power system is ensured. and safety.
Patent Information
- Application Number
- CN202410940581.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-11
AI Technical Summary
Existing RTV anti-pollution flashover coatings are prone to aging under long-term ultraviolet radiation, resulting in weakened hydrophobicity, increasing the risk of pollution flashover accidents in the power system, and insufficient mechanical properties, affecting the stable operation of the power system.
Uses include dihydroxypolymethylvinylsiloxane, organic tin, mica powder, nano-polytetrafluoroethylene micropowder, titanium dioxide, styrene-butadiene-styrene block copolymer, powdered aluminum hydroxide, resist The anti-fouling flashover coating formula of fuel and catalyst improves the mechanical properties and aging resistance of the coating by optimizing the component ratio and selecting the preferred components.
Significantly improve the mechanical properties and aging resistance of the coating, extend the service life, reduce the risk of power system failure, ensure the continuity and stability of power supply, and enhance the flame retardant performance, reduce the risk of flame spread, reduce Maintenance costs.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an anti-fouling flashover coating. Background Art
[0002] Natural dirt accumulation on the surface of insulators is inevitable for outdoor equipment in power systems, especially in today's increasingly serious air pollution. This dirt accumulation can cause flashover on the surface of insulators under humid conditions, which in turn causes flashover accidents in power systems, posing a threat to the stable operation of power supply systems. Anti-flashover coating is a coating used for the external insulation of insulators or electrical equipment in power systems, mainly used to prevent flashover.
[0003] Anti-pollution flashover coatings are mainly divided into two types: RTV (room temperature vulcanized silicone rubber) and PRTV (long-term anti-pollution flashover coatings). These coatings have been widely used in power systems and have excellent hydrophobicity and electrical properties. The hydrophobicity and hydrophobic migration of the coating are the key to improving the pollution flashover voltage level. The coating forms a layer of film on the surface of the electric porcelain, which has good hydrophobicity under clean conditions. When the surface of the film is covered with dirt, the small molecular hydrophobic groups contained in it can quickly migrate to the surface of the dirt layer to maintain its hydrophobicity. In this way, under humid climatic conditions, the surface of the dirt layer is difficult to wet, which effectively increases the pollution flashover voltage of the insulator.
[0004] Existing RTV anti-pollution flashover coatings are prone to aging under long-term ultraviolet radiation, resulting in reduced hydrophobicity and increasing the risk of flashover accidents in power systems. Therefore, improving the anti-aging performance of coatings is an important technical challenge. Summary of the invention
[0005] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide an anti-pollution flashover coating, which improves the mechanical properties and aging resistance of the coating, can ensure that the coating maintains its anti-pollution flashover function during long-term use, and reduce power system failures caused by degradation of coating performance, thereby ensuring the continuity and stability of power supply.
[0006] The technical solution of the present invention is:
[0007] The anti-pollution flashover coating comprises the following components in parts by mass: 3-10 parts of dihydroxy polymethylvinylsiloxane, 12-20 parts of dihydroxy polydimethylsiloxane, 20-40 parts of organic tin, 10-25 parts of mica powder, 10-30 parts of nano polytetrafluoroethylene powder, 2-4 parts of titanium dioxide, 30-50 parts of styrene-butadiene-styrene block copolymer, 1-2 parts of powdered aluminum hydroxide, 25-35 parts of flame retardant, 1-2 parts of catalyst and 70-100 parts of solvent.
[0008] Preferably, the flame retardant is magnesium hydroxide.
[0009] Preferably, the catalyst is dibutyltin dilaurate, stannous octoate or aluminum acetylacetonate.
[0010] Preferably, the solvent is a mixture of toluene, ethyl acetate and trichloroethane in a mass ratio of 1:(1-2):(1-3).
[0011] Preferably, the following components are included in parts by mass: 5 parts of dihydroxypolymethylvinylsiloxane, 15 parts of dihydroxypolydimethylsiloxane, 20 parts of organic tin, 10 parts of mica powder, 20 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 35 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 25 parts of flame retardant, 2 parts of catalyst, and 100 parts of solvent.
[0012] Preferably, the following components are included in parts by mass: 3 parts of dihydroxypolymethylvinylsiloxane, 20 parts of dihydroxypolydimethylsiloxane, 25 parts of organic tin, 15 parts of mica powder, 25 parts of nano polytetrafluoroethylene powder, 3 parts of titanium dioxide, 40 parts of styrene-butadiene-styrene block copolymer, 2 parts of powdered aluminum hydroxide, 30 parts of flame retardant, 1 part of catalyst, and 80 parts of solvent.
[0013] Preferably, the following components are included in parts by mass: 8 parts of dihydroxypolymethylvinylsiloxane, 12 parts of dihydroxypolydimethylsiloxane, 25 parts of organic tin, 25 parts of mica powder, 30 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 30 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 25 parts of flame retardant, 1 part of catalyst, and 100 parts of solvent.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] The anti-pollution flashover coating of the present invention can improve the mechanical properties and aging resistance of the coating, and by adding flame retardants, the resistance to leakage tracking and flame retardant properties of the coating can be improved, thereby extending the service life of the coating. The improved aging resistance of the coating means that it can better resist the influence of environmental factors such as ultraviolet rays, ozone, and temperature changes. Extending the service life of the coating can ensure that the coating maintains its anti-pollution flashover function during long-term use, and reduce power system failures caused by the degradation of coating performance, thereby ensuring the continuity and stability of power supply. The improvement of flame retardant properties can reduce the spread of flames when a fire occurs, providing additional protection for personnel and equipment. This is particularly important for power systems, because electrical failures are a common cause of fires. In addition, the extension of the service life of the coating and the improvement of its flame retardant properties can reduce the number of equipment maintenance and replacements, thereby reducing long-term maintenance costs. In short, the anti-pollution flashover coating of the present invention not only improves the performance of the product itself, but also provides a strong guarantee for the safe, reliable and efficient operation of the power system. DETAILED DESCRIPTION
[0016] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0017] Example 1
[0018] The anti-pollution flashover coating of this embodiment includes the following components in parts by mass: 5 parts of dihydroxypolymethylvinylsiloxane, 15 parts of dihydroxypolydimethylsiloxane, 20 parts of organic tin, 10 parts of mica powder, 20 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 35 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 25 parts of magnesium hydroxide, 2 parts of dibutyltin dilaurate, and 100 parts of solvent, wherein the solvent is a mixture of toluene, ethyl acetate, and trichloroethane in a mass ratio of 1:2:2.
[0019] Example 2
[0020] The anti-pollution flashover coating of this embodiment includes the following components in parts by mass: 3 parts of dihydroxypolymethylvinylsiloxane, 20 parts of dihydroxypolydimethylsiloxane, 25 parts of organic tin, 15 parts of mica powder, 25 parts of nano polytetrafluoroethylene powder, 3 parts of titanium dioxide, 40 parts of styrene-butadiene-styrene block copolymer, 2 parts of powdered aluminum hydroxide, 30 parts of magnesium hydroxide, 1 part of stannous octoate, and 80 parts of solvent, wherein the solvent is a mixture of toluene, ethyl acetate, and trichloroethane in a mass ratio of 1:2:3.
[0021] Example 3
[0022] The anti-pollution flashover coating of this embodiment includes the following components in parts by mass: 8 parts of dihydroxypolymethylvinylsiloxane, 12 parts of dihydroxypolydimethylsiloxane, 25 parts of organic tin, 25 parts of mica powder, 30 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 30 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 25 parts of magnesium hydroxide, 1 part of aluminum acetylacetonate, and 100 parts of solvent, wherein the solvent is a mixture of toluene, ethyl acetate, and trichloroethane in a mass ratio of 1:1:1.
[0023] Example 4
[0024] The anti-pollution flashover coating of this embodiment includes the following components in parts by mass: 7 parts of dihydroxypolymethylvinylsiloxane, 16 parts of dihydroxypolydimethylsiloxane, 24 parts of organic tin, 12 parts of mica powder, 18 parts of nano polytetrafluoroethylene powder, 3 parts of titanium dioxide, 38 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 26 parts of magnesium hydroxide, 2 parts of aluminum acetylacetonate, and 90 parts of solvent, wherein the solvent is a mixture of toluene, ethyl acetate, and trichloroethane in a mass ratio of 1:2:1.
[0025] Example 5
[0026] The anti-pollution flashover coating of this embodiment includes the following components in parts by mass: 10 parts of dihydroxypolymethylvinylsiloxane, 16 parts of dihydroxypolydimethylsiloxane, 35 parts of organic tin, 22 parts of mica powder, 14 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 33 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 26 parts of magnesium hydroxide, 2 parts of stannous octoate, and 100 parts of solvent, wherein the solvent is a mixture of toluene, ethyl acetate, and trichloroethane in a mass ratio of 1:1:3.
[0027] Example 6
[0028] The anti-pollution flashover coating of this embodiment includes the following components in parts by mass: 3 parts of dihydroxypolymethylvinylsiloxane, 20 parts of dihydroxypolydimethylsiloxane, 25 parts of organic tin, 12 parts of mica powder, 14 parts of nano polytetrafluoroethylene powder, 4 parts of titanium dioxide, 40 parts of styrene-butadiene-styrene block copolymer, 2 parts of powdered aluminum hydroxide, 29 parts of magnesium hydroxide, 1 part of dibutyltin dilaurate, and 70 parts of solvent, wherein the solvent is a mixture of toluene, ethyl acetate, and trichloroethane in a mass ratio of 1:2:2.
Claims
1. Anti-fouling flashover coating, characterized in that: The invention comprises the following components in parts by weight: 3-10 parts of dihydroxy polymethylvinylsiloxane, 12-20 parts of dihydroxy polydimethylsiloxane, 20-40 parts of organic tin, 10-25 parts of mica powder, 10-30 parts of nano polytetrafluoroethylene powder, 2-4 parts of titanium dioxide, 30-50 parts of styrene-butadiene-styrene block copolymer, 1-2 parts of powdered aluminum hydroxide, 25-35 parts of flame retardant, 1-2 parts of catalyst and 70-100 parts of solvent.
2. The anti-fouling flashover coating according to claim 1, characterized in that: The flame retardant is magnesium hydroxide.
3. The anti-fouling flashover coating according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate, stannous octoate or aluminum acetylacetonate.
4. The anti-fouling flashover coating according to claim 1, characterized in that: The solvent is a mixture of toluene, ethyl acetate and trichloroethane in a mass ratio of 1:(1-2):(1-3).
5. The anti-fouling flashover coating according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 5 parts of dihydroxy polymethylvinylsiloxane, 15 parts of dihydroxy polydimethylsiloxane, 20 parts of organic tin, 10 parts of mica powder, 20 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 35 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 25 parts of flame retardant, 2 parts of catalyst and 100 parts of solvent.
6. The anti-fouling flashover coating according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 3 parts of dihydroxy polymethylvinylsiloxane, 20 parts of dihydroxy polydimethylsiloxane, 25 parts of organic tin, 15 parts of mica powder, 25 parts of nano polytetrafluoroethylene powder, 3 parts of titanium dioxide, 40 parts of styrene-butadiene-styrene block copolymer, 2 parts of powdered aluminum hydroxide, 30 parts of flame retardant, 1 part of catalyst and 80 parts of solvent.
7. The anti-fouling flashover coating according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 8 parts of dihydroxy polymethylvinylsiloxane, 12 parts of dihydroxy polydimethylsiloxane, 25 parts of organic tin, 25 parts of mica powder, 30 parts of nano polytetrafluoroethylene powder, 2 parts of titanium dioxide, 30 parts of styrene-butadiene-styrene block copolymer, 1 part of powdered aluminum hydroxide, 25 parts of flame retardant, 1 part of catalyst and 100 parts of solvent.