Preparation method and application of embedded aluminum-based biomass material with strong electron transfer effect
By coupling zero-valent aluminum with pyrolytic biochar through mechanical ball milling technology, a mosaic aluminum-based biochar material with strong electron transfer effect is prepared, which solves the problem of high adsorbent consumption and cost in the treatment of high-concentration chromium-containing wastewater, and achieves Efficient, low-cost Cr(VI) removal and renewable utilization of materials.
Patent Information
- Application Number
- CN202410846750.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
AI Technical Summary
When existing adsorption methods treat high-concentration chromium-containing wastewater, the amount of adsorbent and treatment cost are high, and the regeneration process may cause environmental pollution. There is a lack of efficient, stable, low-cost, and renewable adsorption materials.
Micron zero-valent aluminum is coupled with pyrolytic biochar through mechanical ball milling technology to prepare a mosaic aluminum-based biochar material with strong electron transfer effect. The potential difference between the zero-valent metal and the carbon material is used to form a galvanic cell effect and strengthen the electron transfer process. , and reduce Cr(VI) to low-toxic Cr(III) through chemical adsorption.
It achieves efficient, low-cost, short-cycle Cr(VI) removal, the material can be reused, reduces the risk of environmental pollution, and converts waste biomass into high value-added adsorption materials.
Smart Images

Figure CN118755979A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional composite materials, and specifically relates to a preparation method and application of an embedded aluminum-based biomass material with strong electron transfer effect. Background Art
[0002] Chromium is a metal element that is toxic to humans and other animals. Its reserves in the earth's crust rank tenth. It mainly exists in three oxidation states (+2, +3, +6), of which trivalent chromium (Cr(III)) and hexavalent chromium (Cr(VI)) can exist stably in water and can be converted into each other under certain conditions. It is generally believed that Cr(III) is less toxic to the human body, while Cr(VI) is very harmful to the human body. Hexavalent chromium (Cr(VI)) exists in large quantities in the natural environment. It is highly toxic, strongly oxidizing, difficult to degrade and environmentally cumulative, and is listed as one of the typical heavy metal pollutants. With the development of industrial production, the pollution control of Cr(VI) has attracted widespread attention. Cr(VI) is mostly present in industrial wastewater, such as the electroplating industry, leather tanning industry, textile industry, chromium salt manufacturing, etc. If people are in an environment contaminated by Cr(VI) for a long time, human health will be seriously threatened, and it is very easy to cause a series of diseases, such as skin inflammation, respiratory diseases, lung cancer and bone marrow suppression. The presence of Cr(VI) can also have a serious impact on the ecosystem. Cr(VI) in wastewater can cause water pollution and have a direct toxic effect on aquatic organisms. It can also undergo complex chemical reactions with other elements to form difficult-to-degrade organic and inorganic matter, further aggravating water pollution.
[0003] Therefore, the treatment of chromium-containing wastewater is of great significance to human health and the ecological environment. The main methods for treating chromium-containing wastewater are: adsorption method, membrane separation method, ion exchange method, electrochemical method, etc. Among them, the adsorption method is widely used due to its simple operation, high removal efficiency, and less environmental pollution. The core principle of the adsorption method is to use solid substances with porous structures or high specific surface areas as adsorbents. Under the action of physical adsorption or chemical reaction, heavy metal ions in wastewater are adsorbed on their solid surfaces, thereby achieving wastewater purification. When treating chromium-containing wastewater, the adsorption method shows its unique advantages. This process mainly relies on the interaction between the adsorbent and the chromium ions to ensure the efficient removal of chromium ions. At present, there are many types of adsorbents reported, among which inorganic adsorption materials such as activated carbon, zeolite, and diatomaceous earth have attracted much attention due to their high efficiency and stability. These adsorption materials have rich pore structures and large specific surface areas, and can provide a large number of adsorption sites, thereby achieving efficient adsorption of chromium ions. In addition, some natural organic biomass adsorption materials also show good application prospects in the treatment of chromium-containing wastewater due to their unique surface groups and adsorption properties. However, the adsorption method also faces some challenges and limitations in the treatment of chromium-containing wastewater. Especially when treating high-concentration chromium-containing wastewater, the amount of adsorbent and the treatment cost are often high, and a large amount of adsorbent is required to achieve the ideal treatment effect. In addition, the regeneration and treatment process of the adsorbent may also bring new environmental problems, such as the generation of secondary pollution. Therefore, the adsorption treatment technology for chromium-containing wastewater still needs to develop efficient, stable, low-cost and renewable adsorption materials.
[0004] The present invention uses mechanical ball milling technology to couple micron zero-valent aluminum with pyrolytic biochar, and successfully prepares a mosaic aluminum-based biochar material with strong electron transfer. Theoretical research and practical application prove that the developed material has the advantages of high efficiency, low cost, short cycle, and secondary utilization for adsorption and removal of Cr(VI). Moreover, the preparation process can convert low-priced and widely available waste biomass into a mosaic aluminum-based biochar adsorption material with high added value, realizing the diversification and high-value utilization of waste biomass under the dual-carbon background. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a preparation method and application of a mosaic aluminum-based biomass material with strong electron transfer effect.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a mosaic aluminum-based biomass material with strong electron transfer effect comprises the following steps:
[0008] S1. Preparation of biomass powder: Cut banana peel into pieces, wash with ultrapure water, dry and grind into powder, and pass through a 100-mesh sieve for later use;
[0009] S2. Preparation of pyrolytic biochar: Weigh the biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the air tightness test, introduce N2 into the tube furnace for 30 min. Restart the pyrolysis process and control the heating rate to 10 °C min. - 1. When the temperature in the furnace reaches 500°C, maintain this temperature for 2 hours; finally, wait for the tube furnace to drop to room temperature and take out the crucible to obtain pyrolysis biochar;
[0010] S3. Preparation of embedded aluminum-based biochar material: zero-valent nano-aluminum powder and pyrolysis biochar are mixed evenly and placed in a stainless steel ball mill with a volume of 50 mL. The ball mill is then sealed and pressed tightly to start mechanical ball milling. The material synthesis process is in an air atmosphere at room temperature. The rotation direction of the ball mill is alternately forward and reverse, and the direction change frequency is 15 minutes to obtain aluminum-based biomass material.
[0011] Furthermore, in the step S3, the aluminum-based biomass material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls: mixture = 200:1, the particle sizes of the zirconia balls are 8 mm, 4 mm and 2 mm, and the mass ratio of the three is 2:3:5; the mixture is composed of zero-valent nano-aluminum and pyrolytic biochar in a ratio of 3:1, and the ball mill is operated at a speed of 450 rpm for 1.5 hours.
[0012] Furthermore, the mosaic aluminum-based biomass material with strong electron transfer effect is used to treat chromium mine leachate.
[0013] The beneficial effects of the present invention are:
[0014] 1. First, the original zero-valent nano-aluminum is very easy to passivate and agglomerate under natural conditions, making it lose its reactivity. Secondly, although the use of biochar materials can achieve the purpose of "waste treatment", the different preparation methods will lead to significant differences in physical and chemical properties, and its adsorption capacity for target substances is limited. Based on this, the present invention couples the two together through a mechanical ball milling process, utilizes the potential difference between the zero-valent metal and the carbon material, forms a primary cell effect during the reaction process, and strengthens the electron transfer process.
[0015] 2. Under the action of mechanical external force, the original zero-valent nano-aluminum is deformed into a plate-like structure and its surface passivation layer is destroyed. The pyrolytic biochar is evenly dispersed under the action of centrifugal force and combined with the zero-valent nano-aluminum. The surface roughness of the formed composite material is significantly increased, and the increase in specific surface area and pore structure parameters strengthens the physical adsorption of Cr(VI);
[0016] 3. During the preparation of the present invention, pyrolytic biochar is embedded on the surface of zero-valent nano-aluminum, which can slow down the rate of passivation and particle agglomeration, and play a certain protective role. On the other hand, it can also destroy the regularity of zero-valent nano-aluminum crystals, increase the lattice spacing, reduce the binding force of electron transfer, and accelerate the redox reaction. In addition, the aromatic structure and carbon defects of pyrolytic biochar enable it to promote the directional transfer of electrons in a "conductor-mediated" manner as an electron shuttle, and the corrosion current of the composite material is larger, the electron transfer impedance is smaller, and the energy required for transition is lower. Moreover, zero-valent nano-aluminum / pyrolytic biochar reacts with Cr(VI) mainly in the form of chemical adsorption, reducing it to low-toxic Cr(III), and as the alkalinity of the solution continues to increase during the reaction, it is further hydrolyzed in large quantities to generate hydroxides covering the surface of the material. In this process, substances such as Al(OH)3, Al2O3, and AlOOH with Cr(VI) adsorption capacity are also produced to effectively adsorb Cr(VI).
[0017] Other advantages, objectives and features of the present invention will be described in the following description and will be apparent to those skilled in the art to some extent, or those skilled in the art may be taught from the practice of the present invention. The objectives and other advantages of the present invention may be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to make the purpose, technical solution and beneficial effects of the invention clearer, the present invention provides the following drawings for illustration:
[0019] Figure 1 This is a diagram showing the mechanism of enhanced Cr(VI) removal by mZVAl / BC500 of the present invention.
[0020] Figure 2 The effects of the finished products of different mixing methods of the present invention on the Cr(VI) removal filtrate;
[0021] Figure 3 The performance of mZVAl / BC500 in treating chromium ore leachate;
[0022] Figure 4 This is an experiment of removing Cr(VI) from mZVAl / BC500 of the present invention.
[0023] Figure 5 The Raman spectra of different biochar materials of the present invention are shown;
[0024] Figure 6 The effect of the ball-to-material ratio on the removal of Cr(VI) in the present invention;
[0025] Figure 7 The effect of the material ratio on the removal of Cr(VI) in the present invention;
[0026] Figure 8 The effect of the ball milling speed on the removal of Cr(VI) in the present invention;
[0027] Fig. 9 The effect of ball milling time on the removal of Cr(VI) in the present invention;
[0028] Fig.10 (ab) are scanning electron microscope images of mZVAl0 of the present invention;
[0029] Fig.10 (cd) are scanning electron microscope images of mZVA1 / BC50 of the present invention;
[0030] Fig.10 (eg) is the element distribution diagram of Al, C and O in mZVAl / BC500 of the present invention;
[0031] Fig.11 This is a high-resolution transmission electron microscope image of mZVAl / BC500 of the present invention;
[0032] Fig.12 This is a metallographic microscope image of mZVAl / BC500 of the present invention;
[0033] Fig.13 It is the X-ray photoelectron spectrum of mZVAl and mZVAl / BC500 of the present invention. DETAILED DESCRIPTION
[0034] 1. A method for preparing an inlaid aluminum-based biomass material with strong electron transfer effect.
[0035] Example 1
[0036] S1. Preparation of biomass powder: using discarded banana peels as biomass, cutting them into small pieces, washing them with ultrapure water, drying them at 60° C., and then crushing them into powder, passing them through a 100-mesh sieve for later use;
[0037] S2. Preparation of pyrolytic biochar (BC500): Weigh 5 g of biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the airtightness test, N2 was introduced into the tube furnace for 30 min to ensure that the furnace reached an oxygen-free or oxygen-limited state. Subsequently, the pyrolysis process was started and the heating rate was controlled to be 10 °C min. -1 When the temperature in the furnace reaches 500°C, keep this temperature for 2 hours to ensure that the pyrolysis process is fully carried out; finally, wait for the tubular furnace to drop to room temperature and take out the crucible. The black substance obtained is the pyrolysis biochar;
[0038] S3. Preparation of embedded aluminum-based biochar materials: After zero-valent nano-aluminum powder (mZVAl) and pyrolytic biochar are mixed evenly, they are placed in a stainless steel ball mill with a volume of 50 mL, and then the ball mill is sealed and pressed to start mechanical ball milling; the material synthesis process is an air atmosphere at room temperature, and the rotation direction of the ball mill is forward and reverse alternately, and the direction change frequency is 15 minutes; after ball milling for 1.5 hours, aluminum-based biomass materials are obtained. (The material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls (8mm, 4mm and 2mm, mass ratio of 2:3:5): mixture = 200:1, the mixture consists of zero-valent nano-aluminum and pyrolytic biochar in a ratio of 3:1, and the ball milling speed is 450rpm for 1.5 hours).
[0039] In order to demonstrate the superiority of the materials and parameters of the present invention in removing Cr(VI) filtrate, Comparative Examples 1 to 4 are set up.
[0040] Comparative Example 1
[0041] S1. Preparation of biomass powder: using discarded banana peels as biomass, cutting them into small pieces, washing them with ultrapure water, drying them at 60° C., and then crushing them into powder, passing them through a 100-mesh sieve for later use;
[0042] S2. Preparation of pyrolytic biochar (BC500): Weigh 5 g of biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the airtightness test, N2 was introduced into the tube furnace for 30 min to ensure that the furnace reached an oxygen-free or oxygen-limited state. Subsequently, the pyrolysis process was started and the heating rate was controlled to be 10 °C min. -1 When the temperature in the furnace reaches 500°C, keep this temperature for 2 hours to ensure that the pyrolysis process is fully carried out; finally, wait for the tubular furnace to drop to room temperature and take out the crucible. The black substance obtained is the pyrolysis biochar;
[0043] S3. After mixing the nano zero-valent iron and pyrolytic biochar evenly, put them into a stainless steel ball mill with a volume of 50mL, then seal the ball mill, press it and start mechanical ball milling; the material synthesis process is an air atmosphere at room temperature, the rotation direction of the ball mill is forward and reverse alternately, and the direction change frequency is 15 minutes; after ball milling for 1.5h, aluminum-based biomass materials are obtained. (The material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls (8mm, 4mm and 2mm, mass ratio is 2:3:5): mixture = 200:1, the mixture consists of zero-valent nano aluminum and pyrolytic biochar in a ratio of 3:1, and the ball milling speed is 450rpm for 1.5h).
[0044] The difference between this comparative example and Example 1 is that the nano-zero-valent aluminum in step S3 is replaced by nano-zero-valent iron.
[0045] Comparative Example 2
[0046] S1. Preparation of biomass powder: using discarded grapefruit peel as biomass, cutting it into small pieces, washing it with ultrapure water, drying it at 60° C., and then crushing it into powder, passing it through a 100-mesh sieve for later use;
[0047] S2. Preparation of pyrolytic biochar (BC500): Weigh 5 g of biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the airtightness test, N2 was introduced into the tube furnace for 30 min to ensure that the furnace reached an oxygen-free or oxygen-limited state. Subsequently, the pyrolysis process was started and the heating rate was controlled to be 10 °C min. -1 When the temperature in the furnace reaches 500°C, keep this temperature for 2 hours to ensure that the pyrolysis process is fully carried out; finally, wait for the tubular furnace to drop to room temperature and take out the crucible. The black substance obtained is the pyrolysis biochar;
[0048] S3. Preparation of embedded aluminum-based biochar materials: After zero-valent nano-aluminum powder (mZVAl) and pyrolytic biochar are mixed evenly, they are placed in a stainless steel ball mill with a volume of 50 mL, and then the ball mill is sealed and pressed to start mechanical ball milling; the material synthesis process is an air atmosphere at room temperature, and the rotation direction of the ball mill is forward and reverse alternately, and the direction change frequency is 15 minutes; after ball milling for 1.5 hours, aluminum-based biomass materials are obtained. (The material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls (8mm, 4mm and 2mm, mass ratio of 2:3:5): mixture = 200:1, the mixture consists of zero-valent nano-aluminum and pyrolytic biochar in a ratio of 3:1, and the ball milling speed is 450rpm for 1.5 hours).
[0049] The difference between this comparative example and Example 1 is that the biomass raw material in step S1 is grapefruit peel.
[0050] Comparative Example 3
[0051] S1. Preparation of biomass powder: using discarded banana peels as biomass, cutting them into small pieces, washing them with ultrapure water, drying them at 60° C., and then crushing them into powder, passing them through a 100-mesh sieve for later use;
[0052] S2. Preparation of pyrolytic biochar (BC300): Weigh 5 g of biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the air tightness test, N2 was introduced into the tube furnace for 30 min to ensure that the furnace reached an oxygen-free or oxygen-limited state. Subsequently, the pyrolysis process was started and the heating rate was controlled to be 10 °C min. -1When the temperature in the furnace reaches 300°C, keep this temperature for 2 hours to ensure that the pyrolysis process is fully carried out; finally, wait for the tubular furnace to drop to room temperature and take out the crucible. The black substance obtained is the pyrolysis biochar;
[0053] S3. Preparation of embedded aluminum-based biochar materials: After zero-valent nano-aluminum powder (mZVAl) and pyrolytic biochar are mixed evenly, they are placed in a stainless steel ball mill with a volume of 50 mL, and then the ball mill is sealed and pressed to start mechanical ball milling; the material synthesis process is an air atmosphere at room temperature, and the rotation direction of the ball mill is forward and reverse alternately, and the direction change frequency is 15 minutes; after ball milling for 1.5 hours, aluminum-based biomass materials are obtained. (The material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls (8mm, 4mm and 2mm, mass ratio of 2:3:5): mixture = 200:1, the mixture consists of zero-valent nano-aluminum and pyrolytic biochar in a ratio of 3:1, and the ball milling speed is 450rpm for 1.5 hours).
[0054] The difference between this comparative example and Example 1 is that the temperature in the furnace is 300° C. when preparing pyrolysis biochar in step S2.
[0055] Comparative Example 4
[0056] S1. Preparation of biomass powder: using discarded banana peels as biomass, cutting them into small pieces, washing them with ultrapure water, drying them at 60° C., and then crushing them into powder, passing them through a 100-mesh sieve for later use;
[0057] S2. Preparation of pyrolytic biochar (BC700): Weigh 5 g of biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the air tightness test, N2 was introduced into the tube furnace for 30 min to ensure that the furnace reached an oxygen-free or oxygen-limited state. Subsequently, the pyrolysis process was started and the heating rate was controlled to be 10 °C min. -1 When the temperature in the furnace reaches 700°C, keep this temperature for 2 hours to ensure that the pyrolysis process is fully carried out; finally, wait for the tubular furnace to drop to room temperature and take out the crucible. The black substance obtained is the pyrolysis biochar;
[0058] S3. Preparation of embedded aluminum-based biochar materials: After zero-valent nano-aluminum powder (mZVAl) and pyrolytic biochar are mixed evenly, they are placed in a stainless steel ball mill with a volume of 50 mL, and then the ball mill is sealed and pressed to start mechanical ball milling; the material synthesis process is an air atmosphere at room temperature, and the rotation direction of the ball mill is forward and reverse alternately, and the direction change frequency is 15 minutes; after ball milling for 1.5 hours, aluminum-based biomass materials are obtained. (The material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls (8mm, 4mm and 2mm, mass ratio of 2:3:5): mixture = 200:1, the mixture consists of zero-valent nano-aluminum and pyrolytic biochar in a ratio of 3:1, and the ball milling speed is 450rpm for 1.5 hours).
[0059] The difference between this comparative example and Example 1 is that when preparing pyrolysis biochar in step S2, the temperature in the furnace is 700°C.
[0060] In order to demonstrate the superiority of the ball milling method of the present invention in removing Cr(VI) filtrate, comparative examples 5 to 9 are set up.
[0061] Comparative Example 5
[0062] S1. Preparation of biomass powder: using discarded banana peels as biomass, cutting them into small pieces, washing them with ultrapure water, drying them at 60° C., and then crushing them into powder, passing them through a 100-mesh sieve for later use;
[0063] S2. Preparation of pyrolytic biochar (BC500): Weigh 5 g of biomass powder into a crucible and place it in a tube furnace for carbonization. After completing the airtightness test, N2 was introduced into the tube furnace for 30 min to ensure that the furnace reached an oxygen-free or oxygen-limited state. Subsequently, the pyrolysis process was started and the heating rate was controlled to be 10 °C min. -1 When the temperature in the furnace reaches 500°C, keep this temperature for 2 hours to ensure that the pyrolysis process is fully carried out; finally, wait for the tubular furnace to drop to room temperature and take out the crucible. The black substance obtained is the pyrolysis biochar;
[0064] S3. Directly mix the zero-valent nano aluminum powder (mZVAl) and pyrolyzed biochar evenly.
[0065] In order to demonstrate the important role of the mechanical external force generated by the ball milling process on material coupling and the influence of the unique geometric configuration on the Cr(VI) removal efficiency, comparative example 5 was set up without using the ball milling method, and the pyrolysis biochar was directly mixed with the zero-valent nano-aluminum powder.
[0066] Comparative Example 6
[0067] S1. Directly use zero-valent nano-aluminum powder for Cr(VI) filtrate treatment.
[0068] Comparative Example 7
[0069] S1. The ball-milled zero-valent nano-aluminum powder is directly used for Cr(VI) filtrate treatment.
[0070] Comparative Example 8
[0071] S1. The pyrolysis biochar powder is directly used for Cr(VI) filtrate treatment.
[0072] Comparative Example 9
[0073] S1. The ball-milled pyrolysis biochar powder is directly used for Cr(VI) filtrate treatment.
[0074] The aluminum-based biomass material prepared in Example 1 and the comparative materials prepared in Comparative Examples 1 to 9 were added to the Cr(VI) solution respectively. The removal effects of the nine groups of products after 30 minutes are shown in Table 1:
[0075] Table 1 Effect of different finished products on removal of Cr(VI) solution
[0076]
[0077] As can be seen from the table above, the removal capacity of mZVAl / BC500 for Cr(VI) is significantly improved through the ball milling composite process, and complete adsorption and removal is basically achieved within 30 minutes, which greatly reflects the synergistic effect. Considering that under the strong centrifugal force, BC500 and mZVAl are successfully coupled, which not only increases the specific surface area of the material and strengthens the physical adsorption effect, but also protects mZVAl and slows down its re-oxidation and agglomeration rate. More importantly, the change in the lattice structure of mZVAl accelerates the electron transfer process, thereby achieving the purpose of efficient removal of Cr(VI).
[0078] At the same time, the present invention can not only slow down the rate of passivation and particle agglomeration of zero-valent nano-aluminum, but also play a certain protective role, and can also destroy the regularity of zero-valent nano-aluminum crystals, increase the lattice spacing, reduce the restraining force on electron transfer, and accelerate the redox reaction. Figure 1As shown in the figure, the aromatic structure and carbon defects of pyrolytic biochar enable it to act as an electron shuttle to promote the directional transfer of electrons in a "conductor-mediated" manner. The corrosion current of the composite material is larger, the electron transfer impedance is smaller, and the energy required for the transition is lower. In addition, zero-valent nano-aluminum / pyrolytic biochar reacts with Cr(VI) mainly in the form of chemical adsorption, reducing it to low-toxic Cr(III). As the alkalinity of the solution continues to increase during the reaction, it is further hydrolyzed in large quantities to generate hydroxides that cover the surface of the material. In this process, substances such as Al(OH)3, Al2O3, and AlOOH with Cr(VI) adsorption capacity are also produced to effectively adsorb Cr(VI).
[0079] As for the other comparative examples, due to the changes in parameters such as raw materials, temperature, mixing method, etc., the effects of the finished products are not as good as the finished products prepared by the present invention. It can be seen that only when the raw materials, temperature and mixing method of the present invention are coordinated, the removal effect of the finished product on the Cr(VI) solution can be optimal.
[0080] In addition, the effects of different mixing methods on the finished product are discussed. Figure 2 As shown in the figure, compared with mZVAl, BC500 has a larger specific surface area, which enhances the removal ability of Cr(VI). Within a reaction time of 30 minutes, 27.48% of Cr(VI) was adsorbed and removed. For BM-BC500, the ball milling process reduces its particle size and enhances the physical adsorption force, and the removal efficiency increases to 32.08%. However, both mZVAl and BC500 have very limited ability to remove Cr(VI) in a short period of time. The composite material formed by coupling the two through mechanical ball milling can enhance the removal of Cr(VI) in the solution.
[0081] When mZVAl and BC500 were mixed by mass and directly added to the solution containing Cr(VI), the removal rate of Cr(VI) did not increase, and was only 12.03% in 30 minutes, indicating that there was no synergistic effect between the two. This is because simple mixing did not achieve the removal of the passivation layer on the surface of mZVAl, the regularity of its crystal structure was not affected, the electron transfer process was severely inhibited, and the microscopic galvanic cell effect could not be formed. mZVAl and BC500 played a role alone.
[0082] The specific surface area and pore structure parameters of different biochar materials are shown in Table 2:
[0083] Table 2 Specific surface area and pore structure parameters of different biochar materials
[0084] sample <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Average pore volume (cm 3 ·g -1 )]]> Average pore size (nm) 160℃ pyrolysis biochar 29.8104 0.0039 32.8838 200℃ pyrolysis biochar 55.6724 0.0110 23.0007 240℃ pyrolysis biochar 58.5783 0.0115 24.8286 300℃ pyrolysis biochar 19.9836 0.0051 79.9253 500℃ pyrolysis biochar 47.5499 0.0101 29.7564 700℃ pyrolysis biochar 33.1457 0.0043 37.8704
[0085] 2. Mosaic aluminum-based biomass materials with strong electron transfer function are used to treat leaching in chromium mines.
[0086] Chromium-containing wastewater generated in industrial production activities usually has the characteristics of complex treatment conditions and contains more coexisting ions, which brings many challenges to conventional treatment processes. In order to further evaluate the application potential of ball-milled composite material mZVAl / BC500 in the actual treatment of chromium-containing wastewater, the removal ability in water bodies with more complex components was investigated. This experiment selected the leachate from a chromium mine in Chongqing as the actual treatment object. Its basic water quality parameters are shown in Table 3. The pH value is 6.10 and the concentration of Cr(VI) is 67.83 mg·L -1 , and contains 836.35mg·L -1 Na + and 778.55 mg·L -1 Cl - , and a small amount of SO4 2- and trace amounts of NO3 - . Add 2.5g·L -1 The composite material reacts, and the result Figure 3 shown.
[0087] Table 3 Water quality indicators of chromium ore leachate
[0088]
[0089] Table 4m ZVAl Specific surface area and pore structure parameters of mZVAl / BC500
[0090] sample <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Average pore volume (cm 3 ·g -1 )]]> Average pore size (nm) VtL 1.857 0.009 4.879 mZVAl / BC500 23.389 0.054 19.285
[0091] When the reaction reaches equilibrium, 79.44% of Cr(VI) and 76.51% of total Cr in the solution are removed, indicating that the ball-milled composite material can not only be used to treat industrial wastewater containing Cr(VI) with complex components, but also enhance the adsorption and fixation of its reaction products. Further calculations show that the equilibrium adsorption capacity of mZVAl / BC500 for Cr(VI) is 21.56 mg·g -1 , which is comparable to the adsorption capacity in laboratory prepared solution.
[0092] In summary, mZVAl / BC500 prepared by ball milling can be used as a new type of material with excellent performance, safety and reliability for the treatment of actual acidic chromium-containing wastewater. Its specific dosage should be selected according to the initial concentration of Cr(VI) and the removal efficiency to be achieved.
[0093] 3. Reuse Experiment
[0094] In order to understand the application prospects of mZVAl / BC500, its recycling performance was evaluated. Figure 4 As shown, at room temperature, when the initial concentration of Cr(VI) was 10.0 mg·L -1 Add 0.8 g·L -1 The composite material was reacted, and no Cr(VI) was detected in the solution after 30 minutes, and the total Cr removal rate was as high as 98.08%. The reacted materials were separated, washed and dried, and then reacted for the second time under the same conditions. The results showed that only 45.92% of Cr(VI) in the solution was removed, and the total Cr removal rate dropped to 37.79%. It is considered that after the first reaction, the hydroxide generated by the hydrolysis of Cr(Ⅲ) covered the surface of the mZVAl / BC500 material, covering the active sites, and all the reactions and material collection steps were carried out in the air atmosphere, which caused the mZVAl to be secondary passivated, weakening the electron transfer efficiency. It can be seen that the presence of the precipitation layer on the surface of mZVAl / BC500 will have a certain impact on the Cr(VI) removal performance of the composite material.
[0095] Based on this, the reacted material was ball-milled for a second time to restore its activity. As shown in Table 5, the reaction performance of the material after the second ball-milling was significantly improved, and the nearly simultaneous removal of Cr(VI) and total Cr was achieved within a reaction time of 30 min, with the removal rates of 99.17% and 95.67%, respectively.
[0096] The above results indicate that the mechanical ball milling process can not only successfully couple mZVAl and BC500 to form a composite material, but also restore the reactivity of the passivated material. The process is convenient and economical.
[0097] Table 5 Removal of Cr(VI) and total Cr in the reuse experiment
[0098] sample Cr(Ⅵ) Total Cr 1st 100.00% 98.08% 2nd 45.92% 39.79% Ball milling again 99.17% 95.67%
[0099] 4. Selection of optimal experimental conditions
[0100] The hydrothermal biochar materials obtained by hydrothermal reaction at 160℃, 200℃ and 240℃ for 4h were recorded as HC160, HC200 and HC240. When the temperature of the tube furnace was 300℃, 500℃ and 700℃, the pyrolysis biochar materials obtained by pyrolysis for 2h were abbreviated as BC300, BC500 and BC700. The physicochemical properties of the six biochar materials were comprehensively compared under the same experimental conditions, and BC500 was finally selected as the optimal biochar for coupling with mZVAl.
[0101] (1) Physical characterization
[0102] The specific surface area, average pore volume and pore size of different materials were measured in detail using a fully automatic specific surface area and pore size analyzer. The results are shown in Table 1. The results show that for hydrothermal biochar, its specific surface area and pore structure parameters are proportional to the hydrothermal temperature. When the hydrothermal temperature increases from 160°C to 200°C, the specific surface area of the carbon material increases from 29.8104m 2 ·g -1 Increased to 55.6724m 2 ·g -1 , while the difference between HC200 and HC240 is not much. For pyrolytic biochar, when the temperature in the tube furnace increases from 300℃ to 700℃, the specific surface area and average pore volume of the pyrolytic biochar first increase and then decrease. It is considered that the excessively high temperature causes the collapse of the pore structure. Porosity and a larger specific surface area are more conducive to the adsorption of the target substance on the surface of the material or inside the pores. This physical adsorption mainly relies on the van der Waals force between molecules. Among them, BC500 has a larger specific surface area among the three pyrolytic carbons, which enhances the physical adsorption of Cr(VI).
[0103] (2) Chemical structure
[0104] The carbon structure of different biochar materials was analyzed by Raman spectroscopy. Figure 5 As shown. Located at 1350cm -1 The D peak near 1580 cm-1 is related to the crystal defects of carbon atoms, while -1 The nearby G peak is attributed to the stretching vibration of the in-plane bond of carbon atoms, which is related to the regular graphite sheet structure. The ratio of the two (ID / IG) is usually used to reflect the degree of defects in the carbon structure. When the pyrolysis temperature continues to increase, the ID / IG values of BC500 and BC700 are 1.28 and 1.32, respectively. It is considered that the increase in pyrolysis temperature causes more aromatic ring conjugated structures to form, which not only enhances the stability of the material, but also helps to improve the electrical conductivity of the material. Compared with hydrothermal carbon, the carbon structure of pyrolyzed biochar has a greater degree of defects, which will lead to significant differences in the subsequent Cr(VI) removal performance of the mZVAl / biochar composite material.
[0105] After comprehensive consideration, BC500 was selected as the optimal biochar for coupling with mZVAl.
[0106] Taking the removal rate of Cr(VI) as an indicator, the effects of ball-to-material ratio, material ratio, ball milling speed and ball milling time on the removal performance of mZVAl / BC500 were investigated, and the optimal preparation parameters of the composite material were optimized.
[0107] (1) Ball to material ratio
[0108] During the mechanical ball milling process, the centrifugal force generated by high-speed rotation causes the grinding balls to fall and collide continuously, forming severe friction and impact force, which in turn breaks the material or deforms it. In the ball mill, the grinding balls occupy a large amount of space, so in order to avoid the influence of filling degree, the total mass of the zirconia balls is determined to be 48g, and the ball-to-material ratio parameters are selected as 50:1, 100:1, 200:1 and 300:1. Figure 6 As shown in the test results, the removal rate of Cr(VI) is proportional to the ball-to-material ratio. When the mass ratio of zirconia ball to material is 50:1 and 100:1, the removal rates of Cr(VI) are 43.25% and 51.90% respectively. This is because when the mass of the grinding ball is constant, the smaller the ball-to-material ratio, the more raw materials to be processed. At the same ball milling speed and time, the number of times the powder particles are collided is reduced, and the mechanical damage to mZVAl and the coupling effect between raw materials are weakened. When the ball-to-material ratio is greater than 200, the synthesized composite material can achieve complete removal of Cr(VI) within 30 minutes, indicating that the number of effective collisions between the grinding ball and the material per unit time increases, the energy transferred to the powder particles is higher, and the synthesized mZVAl / BC500 has excellent performance. However, when the ball-to-material ratio continues to increase from 200:1 to 300:1, the removal rate of Cr(VI) by the composite material increases slowly. Considering the removal efficiency and the yield of the composite material, the preferred ball-to-material ratio is 200:1.
[0109] (2) Material ratio
[0110] The effect of the mass ratio of mZVAl and BC500 (i.e. material ratio) on the properties of composite materials was studied, and the experimental parameters selected were mZVAl:BC500 of 5:1, 4:1, 3:1, 2:1 and 1:1.
[0111] like Figure 7 As shown in the figure, when the mass of BC500 gradually increases, the removal of Cr(VI) first increases and then decreases, increasing from 81.65% to 100.00% and then decreasing to 59.65%. The removal effect is best when mZVAl:BC500=3:1. This is because when the ratio of the two is high, the mZVAl content is high and BC500 is lacking. The freshly exposed zero-valent aluminum after ball milling cannot couple with sufficient biochar material, which not only reduces the protective effect on the mZVAl surface, but also reduces the number of microscopic galvanic cells, which weakens the removal effect of Cr(VI).
[0112] (3) Ball mill speed
[0113] Changes in the ball mill speed will produce different collisions, frictions, and shearing behaviors, which in turn affect the motion state of the grinding balls and materials in the ball mill, resulting in the input and accumulation of different energies in the system. Under the premise that other conditions remain constant, four parameters of 250rpm, 350rpm, 450rpm, and 550rpm were set to explore the effect of ball mill speed on the coupling performance of composite materials. Figure 8 As shown in the figure, with the increase of the rotation speed, the removal of Cr(VI) by the synthetic material first increased and then decreased. Under the conditions of 250rpm and 350rpm, 50.30% and 55.75% of Cr(VI) were removed, and when the rotation speed reached 450rpm, mZVAl / BC500 achieved enhanced removal of the target pollutant within 30min, so the ball milling speed of 450rpm was selected.
[0114] (4) Ball milling time
[0115] The difference in ball milling time will directly lead to the difference in the accumulated energy in the ball mill, which will in turn affect the synthesis process of the material. The experiment explored the removal effect of Cr(VI) on the composite material synthesized when the ball milling time was 0.5h, 1.0h, 1.5h and 2.0h.
[0116] like Fig. 9 As shown in the figure, when the ball milling time is 0.5h, the removal rate of Cr(VI) by mZVAl / BC500 is low, which is 62.10%. When the ball milling time is further increased to 1.0h, the removal rate increases to 72.75%, and the change rate is not large, indicating that the coupling and activity enhancement of mZVAl and BC500 require a certain amount of time during the mechanical ball milling process. When the ball milling time is greater than 1.5h, the removal efficiency of the composite material for Cr(VI) is significantly improved, and it is completely removed within about 15min. This may be because the material is evenly dispersed at the beginning to prepare for the subsequent coupling. With the extension of the ball milling time, the collision and bonding between the particles intensify, and the mZVAl is deformed into plate-like particles with defects such as cracks and depressions on its surface. BC500 is loaded on it and forms a partially embedded embedding structure. The change in the microstructure affects the change in the electron transfer performance and promotes the occurrence of redox reactions.
[0117] 5. Performance analysis of materials under optimal preparation conditions
[0118] The composite material mZVAl / BC500 was prepared and its physical and chemical properties were analyzed under the conditions of a zirconia ball to mixed powder mass ratio (mballs:mpowders) of 200, a mZVAl to BC500 mass ratio (mAl:mBC500) of 3, and a ball milling speed of 450 rpm for 1.5 h.
[0119] Firstly, the microstructure of the original mZVAl and the ball-milled composite mZVAl / BC500 and the composition distribution of the surface elements of the samples were determined in detail by using a scanning electron microscope and an energy dispersive spectrometer. Fig.10 As shown in (ab), the original mZVAl is a spherical particle with a diameter of about 25μm, and its surface is covered with a passivation layer. Considering that the zero-valent metal has a strong reactivity, it is inevitable to react with oxygen or water in the natural environment. In addition, the particles are very likely to agglomerate, reducing their contact area with the target pollutant. The scanning electron microscope image of mZVAl / BC500 is shown in Fig.10 As shown in (cd), there are significant differences in the morphology of the two compared with the original mZVAl. Due to the soft texture of ZVAl, under the centrifugal force generated by high-speed rotation, the collision between the substances causes it to be deformed into flaky aluminum particles. There are a large number of gaps on the edge of the material, and the overall shape is irregular. Secondly, there are defects and many small particles on the surface of the mZVAl / BC500 material. This is because during the rotation and collision, the mechanical force destroys the passivation layer on the surface of the mZVAl, and cracks and concave structures are generated on its surface. BC500 is evenly dispersed and embedded in the surface of the mZVAl, which significantly increases its roughness, which has a great influence on the specific surface area and pore structure parameters of the material. Attached Fig.10 (eg) The signals of Al, C, and O elements were detected in the energy dispersive scanning results, indicating that the composite material was successfully prepared. The appearance of O element indicates that the mechanical ball milling process destroyed the passivation layer on the surface of mZVAl rather than completely removed it. At the same time, obvious Al element signals were found, indicating that BC500 did not completely cover mZVAl.
[0120] Table 4 shows the comparison of the specific surface area and pore structure parameters of the two. The specific surface area, average pore volume and pore diameter of the original mZVAl are 1.857 m2·g -1 , 0.009cm 3 ·g -1 and 4.879nm. After ball milling, the specific surface area of the composite material increased significantly to 23.389m 2 ·g -1 On the one hand, it is due to the introduction of BC500 with a larger specific surface area, and on the other hand, the shear force generated during the mechanical ball milling process has a certain crushing effect on the material, resulting in a decrease in its particle size and an increase in its specific surface area. In addition, the average pore volume and pore size of mZVAl / BC500 also increased significantly, which is consistent with the results of scanning electron microscopy. In summary, after the mechanical ball milling process, biochar was successfully loaded on the surface of mZVAl, resulting in changes in its morphology and structure. The increase in specific surface area and pore structure parameters enriched the active sites on the surface of the material, strengthened the adsorption of the target substance, and was conducive to the Cr(VI) degradation chemical reaction.
[0121] High-resolution transmission electron microscopy is used to characterize the microstructure of materials to analyze their micro-region composition, lattice fringes, structural defects, etc. Fig.11 (a) shows that the amorphous carbon material BC500 is evenly dispersed on the mZVAl matrix, indicating that the two are successfully coupled under the mechanical ball milling process. Through the analysis of lattice fringes, we have a deeper understanding of the changes in the crystal structure of mZVAl before and after ball milling, and the mechanism of strengthening the removal of Cr(VI) by the coupling material is clarified. According to the standard PDF card of aluminum (PDF#85-1327), the Al(111) plane has the largest interplanar spacing. After ball milling, Fig.11 (bd) show the presence of The lattice spacing. It is known that if the density of a single crystal is certain, the number of atoms per unit volume is certain. The larger the interplanar spacing, the more atoms per unit area, which also means that the atoms are arranged more closely, which is conducive to strengthening the conductivity of metal materials. And the larger the lattice spacing of the material, the smaller the restraint effect on the electron transfer process, and the easier it is to escape. Fig.11 (d) shows a structure where BC500 is embedded in mZVAl. The microstructure of this structure is analyzed and found to exist This indicates that under the action of external mechanical force, the crystal plane spacing of mZVAl increases to varying degrees. The embedding structure of biochar material directly embedded in the ball milling process has the most significant effect on its crystal regularity. The significant increase in crystal spacing reduces the binding effect of atomic nuclei on electrons, accelerates the transfer of electrons between mZVAl and target pollutants, and strengthens the redox reaction.
[0122] In order to further explore the coupling mode of composite materials, metallographic microscope was used to analyze its internal structure. This characterization technology combines optical microscopy, photoelectric conversion and computer image processing technology, and can reflect important information such as the grain structure, grain boundary characteristics, and defects of metal materials. Based on this, in this study, the surface defects, morphological changes, corrosion conditions, etc. of mZVAl / BC500 were analyzed through metallographic microscope testing to further illustrate the bonding of mZVAl and BC500 under mechanical external force. First, from Fig.12 (a) It can be seen that the ball milling process deforms the original mZVAl into plate-like particles with a length of about 20 μm. Its surface is no longer smooth, and many irregular broken structures appear, and the roughness increases significantly. Further magnification of it, the results are as follows Fig.12As shown in (b), a "sandwich" carbon material embedded grain structure appeared, with the Al0 part with regular crystal structure in the middle, many cracks on both sides, and the material surface was uneven. The biochar material was embedded in the rough surface of the mZVAl matrix, and the two were tightly combined. The characterization results of the metallographic microscope further demonstrated the influence of the ball milling process on the material geometry and the unique coupling mode of BC500 and mZVAl through the analysis of the material microstructure.
[0123] X-ray photoelectron spectroscopy can achieve qualitative and semi-quantitative analysis of samples by measuring the binding energy of electrons. The type and chemical state of the elements on the surface of the material can be obtained from the position and shape of the diffraction peaks in the spectrum, and the content of the elements on the surface of the material can be determined by the size of the peak intensity. The XPS characterization results of the original mZVAl and mZVAl / BC500 are shown in Figure 2. Fig.13 As shown in the figure, the diffraction peaks of aluminum oxide and zero-valent aluminum are observed in the Al2p spectrum, indicating that the mechanical ball milling process destroys the surface passivation layer of mZVAl instead of completely removing it. The Al0 content on the surface of the original mZVAl and the composite material is 12.59% and 19.23%, respectively. It is considered that the mechanical external force makes more Al0 exposed, and the loading effect of BC500 slows down the rate of its re-passivation, which is conducive to the subsequent redox reaction. ZVAl is a shell-core structure formed by the external (hydr) oxide layer wrapping the internal Al single substance. When the outer passivation layer film of this structure (its thickness is about 5nm) is effectively destroyed, the internal Al0 can fully play its role as an efficient "electron source", thereby promoting the relevant chemical reactions. Further analysis of its peak position shows that the binding energy corresponding to the Al0 signal peak in mZVAl / BC500 is 71.07eV, which is 0.65eV lower than that of the original mZVAl. The size of the binding energy can reflect the energy required for an electron at a specific energy level to transition to the Fermi level, so the electron transfer process can be explored by analyzing the displacement of the binding energy of a specific element. Generally, a relatively low binding energy means that the orbital electron is less bound by the nucleus, and the transfer process is easier to occur, which further confirms the better electron transfer performance of mZVAl / BC500.
[0124] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for preparing a mosaic aluminum-based biomass material with strong electron transfer effect, Features: The following steps are included: S1. Preparation of biomass powder: Cut banana peel into pieces, wash with ultrapure water, dry and grind into powder, and pass through a 100-mesh sieve for later use; S2. Preparation of pyrolytic biochar: Weigh biomass powder into a crucible and place it in a tube furnace for carbonization treatment; after completing the air tightness test, place N 2 The mixture was placed in a tube furnace and continued for 30 min. The pyrolysis process was restarted and the heating rate was controlled at 10 °C min. -1 When the temperature in the furnace reaches 500°C, maintain this temperature for 2 hours; finally, wait for the tube furnace to drop to room temperature and take out the crucible to obtain pyrolysis biochar; S3. Preparation of embedded aluminum-based biochar material: zero-valent nano-aluminum powder and pyrolysis biochar are mixed evenly and placed in a stainless steel ball mill with a volume of 50 mL. The ball mill is then sealed and pressed tightly to start mechanical ball milling. The material synthesis process is in an air atmosphere at room temperature. The rotation direction of the ball mill is alternately forward and reverse, and the direction change frequency is 15 minutes to obtain aluminum-based biomass material.
2. A method for preparing a mosaic aluminum-based biomass material with strong electron transfer according to claim 1, Features: In the step S3, the aluminum-based biomass material is prepared by a planetary ball mill, and the ball milling parameter values are set as follows: mixed zirconia balls: mixed material = 200:1, the particle sizes of the zirconia balls are 8 mm, 4 mm and 2 mm, and the mass ratio of the three is 2:3:5; the mixed material is composed of zero-valent nano-aluminum and pyrolytic biochar in a ratio of 3:1, and the ball mill is operated at a speed of 450 rpm for 1.5 hours.
3. A method for preparing a mosaic aluminum-based biomass material with strong electron transfer according to claim 1, Features: In step S1, after the banana peels are washed, they are dried at a temperature of 55-65°C.
4. A mosaic aluminum-based biomass material with strong electron transfer function according to any one of claims 1 to 3, used for treating chromium mine leachate.
Citation Information
Patent Citations
Porous carbon material capable of selectively absorbing gold ions, preparation method and application of porous carbon material
CN102895952A
Preparation method and application of LDH modified biomass charcoal material
CN114307944A
Preparation method and application of aluminum-copper-carbon composite material for efficiently reducing nitrate into nitrogen
CN116062870A
Preparation method and application of aluminum-iron-carbon composite material for realizing continuous activation of zero-valent aluminum
CN116409865A
Preparation method and application of zero-valent aluminum / iron-bearing clay composite for catalyzing persulfate to oxidize organics
US11534738B1