Heterogeneous grain structure precipitation strengthening Ni-based alloy and preparation method thereof

By introducing a large and small heterograin structure and nanoscale precipitation phase into Ni-based alloy, combined with liquid nitrogen cold rolling and short-term annealing treatment, the problem of difficulty in taking into account strength and plasticity in the existing technology is solved, and the problem of strength and plasticity is realized High-strength and high-plastic Ni-based alloys simplify the preparation process and improve high-temperature performance.

CN118756002APending Publication Date: 2024-10-11HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410836047.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The prior art is difficult to maintain its plasticity while increasing the strength of Ni-based alloys, and the method of introducing heterostructures and precipitation phases is complex and time-consuming.

Method used

By introducing heterogeneous grain structures of one large and one small sizes and nanoscale precipitation phase Ni3 (Al,Ti) in Ni-based alloys, and using liquid nitrogen cold rolling and short-term annealing treatment, alternately distributed grains are formed Structural and uniformly distributed precipitation phases achieve synergistic effects between strength and plasticity.

Benefits of technology

It significantly improves the strength and plasticity of Ni-based alloys, simplifies the preparation process, shortens the process cycle, is suitable for industrial production, and improves high-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756002A_ABST
    Figure CN118756002A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of high-strength and high-plasticity Ni-based alloys, and discloses a heterogeneous grain structure precipitation strengthening Ni-based alloy and a preparation method thereof.The alloy comprises the Ni element, the Al element and the Ti element and is composed of heterogeneous grains with the large size and the small size, the size of the small-size grains is 1-10 microns, and the volume fraction ratio is 50%-70%; the size of the large-size crystal grains is 20-30 [mu] m, and the volume fraction accounts for 30-50%; a plurality of small-size crystal grains are gathered, a plurality of large-size crystal grains are gathered, the areas of the small-size crystal grains and the areas of the large-size crystal grains are alternately distributed, and meanwhile precipitated phases Ni3 (Al and Ti) are further distributed in the small-size crystal grains and the large-size crystal grains in a dispersed mode. The microstructure in the alloy is improved, and meanwhile, a heterogeneous grain structure and a precipitated phase are introduced, so that the alloy has more excellent plasticity while having high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of high-strength and high-plasticity Ni-based alloys, and more specifically, relates to a heterogeneous grain structure precipitation-strengthened Ni-based alloy and a preparation method thereof, wherein the obtained alloy has both a heterogeneous (i.e., inhomogeneous) grain structure and a precipitation phase. Background Art

[0002] As a widely used structural material, Ni-based alloys show excellent properties such as excellent strength, corrosion resistance and high temperature resistance. However, with the rapid development of industries such as aerospace, automobiles, and electronics, the demand for high-performance materials is increasing. Traditional methods such as deformation strengthening, precipitation strengthening, and grain refinement easily increase the strength of the alloy while sacrificing plasticity, which greatly limits its application.

[0003] The introduction of heterogeneous structure strategy can improve the strength of the material while maintaining the most excellent plasticity. This is mainly because the heterogeneous structure produces geometrically required dislocations in order to coordinate the interface strain gradient, adding heterogeneous plastic deformation based on geometrically required dislocations and causing additional strain hardening and additional strengthening. For example, the design of the heterogeneity of the martensite phase can enable the medium-entropy alloy to obtain an ultimate tensile strength of 1.88GPa and a uniform elongation of 14% (scripta materialia.2023,235,115617). However, the introduction of heterogeneous structures is one of the most difficult problems in current applications. Existing technologies often use different crystal structures or compositions to highlight heterogeneity, such as martensite-ferrite dual-phase steel, which requires more time to design the material structure.

[0004] In addition, when introducing heterogeneous structures, introducing additional precipitation phase strengthening and making it play a role at the same time is also one of the issues worth considering at present.

[0005] Therefore, how to effectively introduce heterogeneous structures into Ni alloys and introduce precipitation strengthening while ensuring the heterogeneity of the alloy is an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0006] In view of the above defects or improvement needs of the prior art, the object of the present invention is to provide a heterogeneous grain structure precipitation strengthened Ni-based alloy and a preparation method thereof, wherein by improving the microstructure inside the alloy and introducing a heterogeneous grain structure (involving two different sizes of grains, one large and one small) and a precipitated phase, a synergistic effect of strength and plasticity of the Ni-based alloy is achieved compared to the conventional heat-treated Ni-based alloy (as illustrated in the embodiments below, compared to GH4698 obtained by the conventional heat treatment process, the modified alloy with a heterogeneous grain structure and a precipitated phase obtained in the embodiments of the present invention can achieve simultaneous improvement in strength and plasticity), so that the alloy has high strength and better plasticity.

[0007] To achieve the above-mentioned purpose, according to one aspect of the present invention, a heterogeneous grain structure precipitation strengthened Ni-based alloy is provided, characterized in that the alloy contains Ni, Al and Ti elements, and is composed of two sizes of heterogeneous grains, one large and one small, wherein the size of the small-sized grains is 1-10μm, and the volume fraction accounts for 50% to 70%; the size of the large-sized grains is 20-30μm, and the volume fraction accounts for 30% to 50%; a number of small-sized grains are aggregated, and a number of large-sized grains are aggregated, and the areas where these small-sized grains are aggregated and the areas where large-sized grains are aggregated are alternately distributed, and at the same time, the precipitated phase Ni3(Al,Ti) is also dispersed in these small-sized grains and large-sized grains.

[0008] As a further preferred embodiment of the present invention, the size of the precipitated phase Ni3(Al,Ti) is 10-45 nm, and the volume fraction in the alloy is 18% to 30%.

[0009] As a further preferred embodiment of the present invention, the alloy contains the following elements in percentage by mass: 1-5% Al, 2-7% Ti, 30-60% Ni;

[0010] Preferably, the alloy contains the following elements and their corresponding mass percentages: 13-16% Cr, 1.4-1.8% Al, 2.3-2.8% Ti, 1.8-2.2% Nb, 2.8-3.2% Mo, the balance being Ni, and other inevitable impurity elements.

[0011] According to another aspect of the present invention, the present invention provides a method for preparing the above-mentioned heterogeneous grain structure precipitation strengthened Ni-based alloy, characterized in that it comprises the following steps:

[0012] S1. According to the preset element types and corresponding mass percentages of the Ni-based alloy, raw materials are prepared, and the raw materials are placed in a smelting furnace and smelted under a protective atmosphere to obtain an alloy ingot; the element types contained in the Ni-based alloy include Ni, Al and Ti elements;

[0013] S2. The alloy ingot obtained in S1 is heated under a protective atmosphere, thereby free forging into a block to obtain a uniform equiaxed crystal structure;

[0014] S3. The block obtained in S2 is solution treated under a protective atmosphere to obtain a uniform supersaturated solid solution;

[0015] S4. The block obtained in S3 is subjected to liquid nitrogen cold rolling treatment to reduce the thickness by at least 60%, thereby obtaining a block of target thickness;

[0016] S5. The block obtained in S4 is annealed in a protective atmosphere to form heterogeneous grains of two sizes, one large and one small, in the alloy, wherein the size of the small-sized grains is 1-10 μm, and the volume fraction accounts for 50% to 70%; the size of the large-sized grains is 20-30 μm, and the volume fraction accounts for 30% to 50%;

[0017] S6. The block obtained in S5 is subjected to aging treatment under a protective atmosphere to generate a precipitated phase Ni3(Al,Ti) in the block, thereby obtaining a heterogeneous grain structure precipitation strengthened Ni-based alloy.

[0018] As a further preferred embodiment of the present invention, in step S5, the annealing treatment is performed at 1100-1150°C for 3-5.5 min;

[0019] Preferably, after the annealing treatment is completed, the block is cooled by air cooling.

[0020] As a further preferred embodiment of the present invention, in step S6, the aging treatment temperature is 700-800°C, and the aging treatment time is 30-120min;

[0021] Preferably, after the aging treatment is completed, cooling is performed by air cooling.

[0022] As a further preferred embodiment of the present invention, in step S1, the smelting furnace is specifically a vacuum induction smelting furnace;

[0023] Accordingly, melting is performed under a protective atmosphere, specifically vacuum melting is performed under a protective atmosphere;

[0024] Preferably, after the raw materials are placed in the vacuum induction melting furnace, the vacuum degree in the furnace is first evacuated to <9Pa, and then electric heating is supplied. When the vacuum degree continues to reach 1.2-0.6Pa, a protective atmosphere is then filled into the furnace.

[0025] As a further preferred embodiment of the present invention, in step S2, the alloy ingot obtained in S1 is heated under a protective atmosphere, specifically, at a temperature of 1100-1150° C. for 150-210 min;

[0026] Preferably, after free forging is completed, cooling is performed by air cooling.

[0027] As a further preferred embodiment of the present invention, in step S3, the solution treatment temperature used in the solution treatment is 1100-1120° C., the holding time is 90-120 min, and then the solution is cooled by water.

[0028] As a further preferred embodiment of the present invention, in step S4, the cold rolling treatment is to first immerse the block in liquid nitrogen for at least 3 minutes to completely cool the block, and then perform rolling, and this is repeated multiple times until the block reaches the target thickness;

[0029] Preferably, the rolling speed is 4-6 m / min;

[0030] More preferably, in steps S1, S2, S3, S5, and S6, the protective gas is independently selected from argon or nitrogen.

[0031] Through the above technical scheme conceived by the present invention, compared with the prior art, the heterogeneous grain structure precipitation strengthened Ni-based alloy in the present invention is composed of two sizes of heterogeneous grains, one large and one small (wherein the size of the small-sized grains is 1-10μm, and the volume fraction accounts for 50% to 70%; the size of the large-sized grains is 20-30μm, and the volume fraction accounts for 30% to 50%), a number of small-sized grains are gathered to form a small-sized grain population, and a number of large-sized grains are gathered to form a large-sized grain population. The areas where these small-sized grains are gathered and the areas where the large-sized grains are gathered are alternately distributed, and the precipitated phase Ni3 (Al, Ti) is also dispersed in these small-sized grains and large-sized grains. In the alloy obtained by the present invention, the large grain population and the small grain population are alternately distributed, the large grains provide higher ductility, and the small grains have higher strength. The mutual cooperation between the two realizes the synergistic effect of strength and plasticity of the Ni-based alloy, so that the alloy has better plasticity while having high strength. The present invention can effectively improve plasticity. As shown in Comparative Example 1 below, the plasticity of GH4698 obtained by conventional heat treatment is 26%, while the plasticity of the precipitation-strengthened nickel-based alloy with a heterogeneous structure obtained by the present invention can be improved to more than 33%.

[0032] The corresponding preparation method can be to subject the sample prepared by conventional smelting operation to solution treatment to obtain a supersaturated solid solution, and then to rolling at liquid nitrogen temperature to reduce the thickness by at least 60% to achieve a specific deformation amount, and then to annealing treatment and controlled annealing treatment to form a heterogeneous grain structure in the alloy, and the subsequent aging treatment retains the heterogeneous grain structure while obtaining a uniformly distributed Ni3 (Al, Ti) precipitation phase; the precipitation phase introduced by the aging treatment does not destroy the heterogeneity of the grain structure, so that the alloy has a better strength. The Ni-based alloy combined with the heterogeneous grain structure and precipitation obtained by the present invention has the characteristics of high strength and high ductility, and good plasticity.

[0033] Different from the prior art that uses different crystal structures or components to highlight heterogeneity, the present invention uses two types of grains, one large and one small, to form a heterogeneous grain structure, highlighting the heterogeneity of the same structure but different grain sizes, making it possible to achieve heterogeneity of single-element materials, and simple liquid nitrogen cold rolling and subsequent short-time annealing also shorten the preparation time of heterogeneous structure materials. Specifically, the following beneficial effects can be achieved:

[0034] 1. The Ni-based alloy with heterogeneous grain structure and precipitation prepared by the present invention obtains two heterogeneous grain structures with obvious differences in grain size through high-temperature vacuum melting, and simple and easy-to-industrial cold rolling and annealing processes. In addition, while ensuring the heterogeneity of the grains, an aging process is adopted to obtain a uniformly distributed L12-Ni3 (Al, Ti) precipitation phase (as illustrated in the examples below, the volume fraction of the precipitation phase can be as high as 25%, with the characteristics of high density; while the traditional GH4698 has only 20%). The present invention introduces a heterogeneous grain structure of large and small grains and a nanoscale L12-Ni3 (Al, Ti) precipitation phase into the Ni-based alloy, and the two structures coexist, so that the alloy obtains an excellent combination of strength and plasticity. As illustrated in the embodiments below, the Ni-based alloy obtained based on the heterogeneous grain structure and precipitation obtained by the present invention has a tensile strength of more than 1500 MPa at room temperature, a yield strength of more than 1050 MPa, an elongation of more than 32%, and good plasticity; at a high temperature of 700°C, the tensile strength can reach more than 1050 MPa, the yield strength can reach more than 800 MPa, and the elongation can reach more than 20%. It has excellent comprehensive performance and has good application prospects.

[0035] 2. The Ni-based alloy with heterogeneous grain structure and precipitation combination prepared by the present invention accumulates higher energy at the alloy grain boundary or shear band through liquid nitrogen cold rolling, so that the subsequent annealing treatment forms two parts of grains of different sizes, and the high-energy grain boundary and shear band form large grains of 20-30μm, and the other matrix parts form small grains of 1-10μm, which together constitute the heterogeneous structure of the grains. The interaction between small grains and large grains causes additional strain hardening and additional strengthening, thereby obtaining an excellent combination of strength and plasticity.

[0036] 3. The Ni-based alloy with heterogeneous grain structure and precipitation prepared in the present invention is obtained by introducing a heterogeneous grain structure (i.e., large and small grain structure) through annealing treatment, and then obtaining a uniformly distributed L12-Ni3 (Al, Ti) precipitation phase through aging treatment. The introduction of the precipitation phase does not destroy the heterogeneity of the grain structure, which enables the heterogeneous structure strengthening and precipitation strengthening to give the alloy excellent performance to the greatest extent.

[0037] 4. The Ni-based alloy with heterogeneous grain structure and precipitation prepared by the present invention, wherein the precipitated phase L12-Ni3 (Al, Ti) is obtained by aging treatment after the heterogeneous grain structure is introduced by annealing treatment, and the aging treatment can be aging treatment at a temperature of 700-800°C for 30-120 minutes, which is short in time; compared with the traditional heat treatment process of introducing precipitation phase, the time required is shorter (the traditional process often requires more than 28 hours), shortening the process cycle and greatly saving costs. In addition, the strengthening of the precipitation phase is not reduced due to the short-cycle heat treatment process.

[0038] 5. The Ni-based alloy with heterogeneous grain structure and precipitation prepared by the present invention has a higher synergistic effect of strength and plasticity compared with the traditional heat treatment process. Taking Example 4 as an example, while the tensile strength is greater than 1500MPa, the elongation is about 30%, and the plasticity is good.

[0039] 6. The present invention is simple and convenient to operate, has good controllability, is clean and pollution-free, and is suitable for large-scale industrialization.

[0040] 7. The Ni-based alloy with heterogeneous grain structure and precipitation prepared by the present invention can be preferably annealed at a temperature between 1100-1150°C and a time between 3.0-5.5 minutes, which can most effectively introduce heterogeneous grain structure. The volume fraction of small grains is 50% to 70%, and the volume fraction of large grains is 30% to 50%.

[0041] In summary, the present invention obtains a heterogeneous structure Ni-based precipitation strengthening alloy with strong plasticity synergistic effect, adopts a simple and easy industrial rolling and heat treatment method, effectively combines the heterogeneous structure of the grains and the precipitated phase, and the heat treatment time is short, which can minimize environmental pollution. The combination of the two structures gives the Ni alloy a higher strength and plasticity synergistic effect, so that the alloy has excellent strength and also obtains a better elongation, and the high temperature performance is improved simultaneously. The present invention simultaneously introduces a heterogeneous grain structure and a precipitated phase into the Ni-based alloy, and provides a high-strength and high-plastic nickel-based alloy block that can be oriented to engineering applications, and has high practical application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of the preparation process of Ni-based alloy with heterogeneous grain structure and precipitation combination according to Example 4 of the present invention.

[0043] Figure 2 This is a microstructure diagram of the alloy after cold rolling in Example 1 of the present invention; wherein, Figure 2 The a in corresponds to the inverse pole figure, Figure 2 b in the figure corresponds to the bottom plate. Figure 2 The c in the figure corresponds to the geometric dislocation density map.

[0044] Figure 3 This is a microstructure diagram of the alloy heterogeneous grains after annealing treatment in Example 2 of the present invention; wherein, Figure 3 The a in corresponds to the inverse pole figure, Figure 3 The b in corresponds to the bottom plate image.

[0045] Figure 4 This is the distribution diagram of the precipitated phase after aging treatment in Example 4 of the present invention.

[0046] Figure 5The figure is a schematic flow chart of the preparation method of the heterogeneous grain structure precipitation strengthened Ni-based alloy of the present invention.

[0047] Figure 6 This is the homogeneous microstructure organization diagram obtained in Example 3 of the present invention. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0049] The present invention can obtain a Ni-based alloy with a heterogeneous grain structure and precipitation. The Ni-based alloy with a heterogeneous grain structure and precipitation has two grain size populations, wherein the small grain size is 1-10 μm, the volume fraction is 50% to 70% (such as 60%), the large grain size is 20-30 μm, and the volume fraction is 30% to 50% (such as 40%); the Ni3 (Al, Ti) precipitation phase is dispersed in the small grains and the large grains, the distribution is uniform, the size is 10-45 nm, and the volume fraction is 18% to 30%.

[0050] Taking the high temperature alloy GH4698 as an example (the mass percentage of the elements is: 15% Cr, 1.8% Al, 2.5% Ti, 2.0% Nb, 3.1% Mo, the balance is Ni, and other inevitable impurity elements; each embodiment below uses this formula, and the percentage sign is omitted), based on the present invention, Figure 5 As shown, you can follow the steps below ( Figure 5 The “introduction of heterogeneous grain structure” may include first rolling treatment and then annealing treatment):

[0051] Step 1: Ni-based alloy smelting

[0052] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace, and the vacuum is pumped to <9Pa and then electric heating is sent. When the vacuum is further pumped to 1.2-0.6Pa, argon gas is filled into the furnace as a protective gas; the smelted material is annealed, and after descaling, smelting is carried out in a vacuum consumable furnace, and the vacuum process is consistent with the above (that is, the vacuum degree of the vacuum consumable furnace is first pumped to <9Pa and then electric heating is sent. When the vacuum is further pumped to 1.2-0.6Pa, argon gas is filled into the furnace as a protective gas), and finally the material ingot required for smelting is obtained for standby use;

[0053] Step 2: Free Forging

[0054] The alloy ingot obtained in step 1 is heated to 1100-1150°C, and heat-treated for 150-210 minutes under an inert gas, and then hot-forged into a block sample for standby use; this step of free forging can break up the coarse grains to obtain a uniform equiaxed grain structure;

[0055] Step 3: Solution treatment

[0056] Under the protection of inert gas argon, the block sample obtained in step 2 is solution treated in an environment of 1100-1120°C for 90-120 minutes (the cooling method can be water quenching); this solution treatment can dissolve carbides and precipitates in the matrix to obtain a uniform supersaturated solid solution, which is convenient for re-precipitation of fine-grained and evenly distributed precipitates during aging, and at the same time eliminates the stress caused by hot and cold processing.

[0057] The term "solution treatment" used in the present invention is the same as the conventional definition, and refers to a process in which the equilibrium transformation is suppressed during the solidification of the solid solution to obtain a metastable supersaturated solid solution single-phase structure.

[0058] Step 4: Rolling treatment

[0059] The block obtained in step three is immersed in liquid nitrogen, and after being completely cooled, it is rolled for multiple times. Before each rolling, the sample is cooled with liquid nitrogen for 5 minutes (of course, it can also be longer, as short as 3 minutes). The thickness of the block sample is reduced by 67-70% after rolling (of course, it can also be other target thicknesses). The present invention adopts liquid nitrogen cold rolling in order to store higher energy in the Ni-based alloy matrix, which is conducive to the preferential rapid growth of some grains, thereby obtaining the desired heterogeneous grain structure, so it is generally required that the thickness is reduced by at least 60% after rolling.

[0060] Step 5: Annealing

[0061] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100-1150° C. for 3-5.5 min (the cooling method may be air cooling). This process can obtain the desired heterogeneous grain structure. Of course, the annealing time for obtaining the heterogeneous grain structure may be different at different annealing temperatures. The heterogeneous grain structure can be ensured by controlling the annealing temperature and time.

[0062] Step 6: Aging Process

[0063] Under the protection of inert gas argon, the annealed sample obtained in step 5 is subjected to aging treatment in an environment of 700-800° C. for 30-120 min (the cooling method may be air cooling). This process can obtain the desired precipitated phase structure.

[0064] Through the above six steps, a Ni-based alloy with heterogeneous grain structure and precipitation bonding can be obtained.

[0065] The following are specific embodiments:

[0066] Example 1

[0067] In this embodiment, only rolling at liquid nitrogen temperature is performed in the Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0068] The specific preparation method is:

[0069] Step 1: Ni-based alloy smelting

[0070] According to the above mass percentage ratio of Cr single substance material, Al single substance material, Ti single substance material, Nb single substance material, Mo single substance material and Ni single substance material, each element is selected and placed in a vacuum induction melting furnace, and after the vacuum degree is evacuated to 9Pa, electric heating is sent, and when the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby use;

[0071] Step 2: Free Forging

[0072] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0073] Step 3: Solution treatment

[0074] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0075] Step 4: Rolling treatment

[0076] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0077] At room temperature, the microstructure and performance tests of the rolled Ni-based alloy prepared in this embodiment are as follows:

[0078] The microstructure of the cold-rolled Ni-based alloy obtained in this embodiment was observed using a scanning electron microscope. Figure 2 As shown, the morphology and geometry of the grains after cold rolling must be seen. The finished Ni-based alloy obtained in this embodiment has a tensile strength of 1700 MPa, a yield strength of 1600 MPa, an elongation of 4%, and very poor plasticity (see Table 1 below).

[0079] Example 2

[0080] In this embodiment, a heterogeneous grain structure is prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0081] The specific preparation method is:

[0082] Step 1: Ni-based alloy smelting

[0083] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0084] Step 2: Free Forging

[0085] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0086] Step 3: Solution treatment

[0087] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0088] Step 4: Rolling treatment

[0089] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling;

[0090] Step 5: Annealing

[0091] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100° C. for 5.5 min and air-cooled. This process can obtain the desired heterogeneous grain structure.

[0092] At room temperature, the microstructure and performance tests of the heterogeneous grain structure Ni-based alloy prepared in this embodiment are as follows:

[0093] The microstructure of the heterogeneous grain structure Ni-based alloy prepared in this embodiment was observed by scanning electron microscope. Figure 3 As shown, the morphology of the heterogeneous grain structure can be seen. And, Figure 3It can be clearly seen that there are two grain size populations (i.e., two grain size aggregation areas), the small grain size is 1-10μm, the volume fraction is ~60%; the large grain size is 20-30μm, the volume fraction is ~40%; the large grain population and the small grain population are not arranged separately, but are alternately distributed, and the large and small grains coexist in the form of stacked communities. The tensile strength of the finished Ni-based alloy obtained in this embodiment is 1230MPa, the yield strength is 760MPa, and the elongation is 45% (see Table 1 below).

[0094] Example 3 (this example is a comparative example)

[0095] In this embodiment, a homogeneous grain structure is prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0096] The specific preparation method is:

[0097] Step 1: Ni-based alloy smelting

[0098] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0099] Step 2: Free Forging

[0100] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0101] Step 3: Solution treatment

[0102] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0103] Step 4: Rolling treatment

[0104] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0105] Step 5: Annealing

[0106] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100° C. for 6 minutes and air-cooled. This process can obtain the desired homogeneous grain structure.

[0107] At room temperature, the microstructure of the Ni-based alloy prepared in this embodiment was tested. The microstructure of the Ni-based alloy prepared in this embodiment was observed using a scanning electron microscope. The results are as follows: Figure 6 As shown, the morphology of the homogeneous grain structure can be seen.

[0108] At room temperature, the homogeneous grain structure Ni-based alloy prepared in this embodiment is subjected to the following performance tests: The finished Ni-based alloy prepared in this embodiment has a tensile strength of 1100 MPa, a yield strength of 640 MPa, and an elongation of 46% (see Table 1 below).

[0109] Example 4

[0110] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0111] The specific preparation method is:

[0112] Step 1: Ni-based alloy smelting

[0113] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0114] Step 2: Free Forging

[0115] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0116] Step 3: Solution treatment

[0117] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0118] Step 4: Rolling treatment

[0119] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0120] Step 5: Annealing

[0121] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100°C for 5.5 minutes and air-cooled. This process can obtain the desired heterogeneous grain structure;

[0122] Step 6: Aging Process

[0123] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 750° C. for 60 min and air-cooled.

[0124] At room temperature, the microstructure and performance tests of the Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment are as follows:

[0125] The morphology of the precipitated phase of the Ni-based alloy with homogeneous grain structure and precipitation obtained in this embodiment was observed by transmission electron microscopy. Figure 4 As shown, the morphology of the precipitated phase can be seen, and these precipitated phases are L12-Ni3 (Al, Ti), which are dispersed in small grains and large grains, with a volume fraction of 25%. The tensile strength of the finished Ni-based alloy obtained in this embodiment is 1503MPa, the yield strength is 1100MPa, and the elongation is 33% (see Table 1 below).

[0126] Example 5

[0127] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0128] The method for preparing the Ni-based alloy combining heterogeneous grain structure and precipitation in this embodiment is the same as that in Embodiment 4, except that the aging treatment temperature and time of the heat treatment system in step 6 are changed to 700° C. / 120 min.

[0129] At room temperature, the performance of the Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment was tested as follows: The tensile strength of the finished Ni-based alloy prepared in this embodiment was 1350 MPa, the yield strength was 950 MPa, and the elongation was 39% (see Table 1 below).

[0130] Example 6

[0131] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0132] The method for preparing the Ni-based alloy combining heterogeneous grain structure and precipitation in this embodiment is the same as that in Embodiment 4, except that the aging treatment temperature and time of the heat treatment system in step 6 are changed to 800° C. / 30 min.

[0133] At room temperature, the performance of the Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment was tested as follows: The finished Ni-based alloy prepared in this embodiment had a tensile strength of 1380 MPa, a yield strength of 960 MPa, and an elongation of 37% (see Table 1 below).

[0134] Example 7 (this example is a comparative example)

[0135] In this embodiment, a homogeneous grain structure and a precipitated phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0136] The specific preparation method is:

[0137] Step 1: Ni-based alloy smelting

[0138] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0139] Step 2: Free Forging

[0140] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0141] Step 3: Solution treatment

[0142] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0143] Step 4: Rolling treatment

[0144] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0145] Step 5: Annealing

[0146] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100° C. for 6 minutes and air-cooled. This process can obtain the desired homogeneous grain structure.

[0147] Step 6: Aging Process

[0148] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 750° C. for 60 min and air-cooled.

[0149] At room temperature, the performance test of the Ni-based alloy combined with homogeneous grain structure precipitation prepared in this embodiment is as follows: The tensile strength of the finished Ni-based alloy prepared in this embodiment is 1360MPa, the yield strength is 800MPa, and the elongation is 31% (see Table 1 below).

[0150] Example 8

[0151] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0152] The method for preparing the Ni-based alloy combining heterogeneous grain structure and precipitation in this embodiment is the same as that in embodiment 4, except that the annealing treatment in a 1100° C. environment for 5.5 min in step 5 is changed to an annealing treatment in a 1150° C. environment for 3 min.

[0153] At room temperature, the performance of the Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment was tested as follows: The tensile strength of the finished Ni-based alloy prepared in this embodiment was 1450 MPa, the yield strength was 1010 MPa, and the elongation was 34% (see Table 1 below).

[0154] Example 9

[0155] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0156] The method for preparing the Ni-based alloy combining heterogeneous grain structure and precipitation in this embodiment is the same as that in Embodiment 8, except that the aging treatment temperature and time of the heat treatment system in step six are changed to 700° C. / 120 min.

[0157] At room temperature, the performance of the Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment was tested as follows: The finished Ni-based alloy prepared in this embodiment had a tensile strength of 1290 MPa, a yield strength of 910 MPa, and an elongation of 42% (see Table 1 below).

[0158] Example 10

[0159] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0160] The method for preparing the Ni-based alloy combining heterogeneous grain structure and precipitation in this embodiment is the same as that in Example 8, except that the aging treatment temperature and time of the heat treatment system in step six are changed to 800° C. / 30 min.

[0161] At room temperature, the performance of the Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment was tested as follows: The tensile strength of the finished Ni-based alloy prepared in this embodiment was 1300 MPa, the yield strength was 890 MPa, and the elongation was 40% (see Table 1 below).

[0162] Comparative Example 1 (conventional heat treatment)

[0163] This comparative example reproduces GH4698 obtained by conventional heat treatment process (which is also the process usually adopted by commercially available GH4698). The mass percentage of the alloy elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni and other inevitable impurity elements.

[0164] The specific preparation method is:

[0165] Step 1: Ni-based alloy smelting

[0166] According to the above mass percentage ratio of Cr single substance material, Al single substance material, Ti single substance material, Nb single substance material, Mo single substance material and Ni single substance material, each element is selected and placed in a vacuum induction melting furnace, and after the vacuum degree is evacuated to 9Pa, electric heating is sent, and when the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby use;

[0167] Step 2: Free Forging

[0168] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0169] Step 3: Heat treatment

[0170] The alloy ingot obtained in step 2 is subjected to the following heat treatment process: first heated to 1120°C and kept warm for 8 hours, then air-cooled; then heated to 1000°C and kept warm for 4 hours, then air-cooled; finally heated to 775°C and kept warm for 16 hours, then air-cooled.

[0171] At room temperature, the performance test of the Ni-based alloy prepared by the conventional heat treatment process in this comparative example is as follows: The tensile strength of the finished Ni-based alloy prepared in this comparative example is 1200 MPa, the yield strength is 750 MPa, and the elongation is 26% (see Table 1 below).

[0172] In addition, the high temperature performance test of the Ni-based alloy prepared by the conventional heat treatment process in this comparative example at 700°C is carried out as follows: the tensile strength of the finished Ni-based alloy prepared in this comparative example is 1000MPa, the yield strength is 690MPa, and the elongation is 18% (see Table 2 below).

[0173] The room temperature properties of the Ni-based alloys obtained in Comparative Example 1 and Examples 1-10 are compared, and the results are shown in Table 1:

[0174] Table 1: Performance test comparison table of traditional GH4698 and products of various examples at room temperature

[0175]

[0176]

[0177] It can be seen from the above table that the Ni-based alloys prepared in the present invention in combination with heterogeneous grain structure precipitation (ie, the alloys prepared in Examples 4-6 and 8-10) have significant advantages and excellent comprehensive performance.

[0178] In addition, by comparing Example 2 with Example 3, it is not difficult to see that the annealing time of the step 5 annealing treatment at 1100° C. cannot exceed 5.5 min, otherwise a homogeneous grain structure will be formed, and the tensile strength and yield strength will be inferior to those of a heterogeneous grain structure.

[0179] Embodiment 11

[0180] In this embodiment, a homogeneous grain structure and a precipitated phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0181] The specific preparation method is:

[0182] Step 1: Ni-based alloy smelting

[0183] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0184] Step 2: Free Forging

[0185] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0186] Step 3: Solution treatment

[0187] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0188] Step 4: Rolling treatment

[0189] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0190] Step 5: Annealing

[0191] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100°C for 5.5 minutes and air-cooled. This process can obtain the desired heterogeneous grain structure;

[0192] Step 6: Aging Process

[0193] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 750° C. for 60 min and air-cooled.

[0194] The Ni-based alloy combined with homogeneous grain structure precipitation prepared in this embodiment was subjected to a high temperature performance test at 700°C as follows: The finished Ni-based alloy prepared in this embodiment had a tensile strength of 1175 MPa, a yield strength of 910 MPa, and an elongation of 21% (see Table 2 below).

[0195] Example 12

[0196] In this embodiment, a homogeneous grain structure and a precipitated phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0197] The specific preparation method is:

[0198] Step 1: Ni-based alloy smelting

[0199] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0200] Step 2: Free Forging

[0201] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0202] Step 3: Solution treatment

[0203] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0204] Step 4: Rolling treatment

[0205] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0206] Step 5: Annealing

[0207] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100°C for 5.5 minutes and air-cooled. This process can obtain the desired heterogeneous grain structure;

[0208] Step 6: Aging Process

[0209] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 700° C. for 60 min and then air-cooled.

[0210] The Ni-based alloy combined with homogeneous grain structure precipitation prepared in this embodiment was subjected to a high temperature performance test at 700°C as follows: The finished Ni-based alloy prepared in this embodiment had a tensile strength of 1108 MPa, a yield strength of 870 MPa, and an elongation of 23% (see Table 2 below).

[0211] Example 13

[0212] In this embodiment, a homogeneous grain structure and a precipitated phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0213] The specific preparation method is:

[0214] Step 1: Ni-based alloy smelting

[0215] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0216] Step 2: Free Forging

[0217] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0218] Step 3: Solution treatment

[0219] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0220] Step 4: Rolling treatment

[0221] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0222] Step 5: Annealing

[0223] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1100°C for 5.5 minutes and air-cooled. This process can obtain the desired heterogeneous grain structure;

[0224] Step 6: Aging Process

[0225] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 800° C. for 30 min and then air-cooled.

[0226] The high temperature performance test of the Ni-based alloy combined with homogeneous grain structure precipitation prepared in this embodiment at 700°C is as follows: The finished Ni-based alloy prepared in this embodiment has a tensile strength of 1121 MPa, a yield strength of 880 MPa, and an elongation of 22% (see Table 2 below).

[0227] Embodiment 14

[0228] In this embodiment, a heterogeneous grain structure and precipitate phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0229] The method for preparing the Ni-based alloy combining heterogeneous grain structure and precipitation in this embodiment is the same as that in Embodiment 11, except that the aging treatment temperature and time of the heat treatment system in step six are changed to 700° C. / 120 min.

[0230] The Ni-based alloy with heterogeneous grain structure and precipitation prepared in this embodiment was subjected to high temperature performance test at 700°C as follows: The finished Ni-based alloy prepared in this embodiment had a tensile strength of 1050 MPa, a yield strength of 800 MPa, and an elongation of 20% (see Table 2 below).

[0231] Embodiment 15

[0232] In this embodiment, a homogeneous grain structure and a precipitated phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0233] The specific preparation method is:

[0234] Step 1: Ni-based alloy smelting

[0235] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0236] Step 2: Free Forging

[0237] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0238] Step 3: Solution treatment

[0239] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0240] Step 4: Rolling treatment

[0241] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0242] Step 5: Annealing

[0243] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1150°C for 3.0 min and air-cooled. This process can obtain the desired heterogeneous grain structure;

[0244] Step 6: Aging Process

[0245] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 700° C. for 120 min and then air-cooled.

[0246] The Ni-based alloy combined with homogeneous grain structure precipitation prepared in this embodiment was subjected to a high temperature performance test at 700°C as follows: The finished Ni-based alloy prepared in this embodiment had a tensile strength of 1150 MPa, a yield strength of 920 MPa, and an elongation of 20% (see Table 2 below).

[0247] Example 16

[0248] In this embodiment, a homogeneous grain structure and a precipitated phase are prepared in a Ni-based alloy, and the mass percentage of the elements is: 15Cr, 1.8Al, 2.5Ti, 2.0Nb, 3.1Mo, and the balance is Ni;

[0249] The specific preparation method is:

[0250] Step 1: Ni-based alloy smelting

[0251] According to the above mass percentage ratio, each element is selected and placed in a vacuum induction melting furnace. After the vacuum degree is evacuated to 9Pa, electric heating is sent. When the vacuum degree continues to be evacuated to 0.8Pa, protective gas argon is filled into the furnace; the smelted material is annealed, the oxide scale is removed, and then smelted in a vacuum consumable furnace. The vacuum process is consistent with the above, and finally the material ingot required for smelting is obtained for standby;

[0252] Step 2: Free Forging

[0253] The alloy ingot obtained in step 1 is heated to 1120° C., and is heat-treated for 150 min under an inert gas, and then hot-forged into a block sample for standby use;

[0254] Step 3: Solution treatment

[0255] Under the protection of inert gas argon, the block sample prepared in step 2 was solution treated in an environment of 1100°C for 90 minutes and then water quenched;

[0256] Step 4: Rolling treatment

[0257] The block obtained in step 3 is immersed in liquid nitrogen, and after being completely cooled, multiple rolling is performed, and the sample is cooled in liquid nitrogen for 5 minutes before each rolling. The thickness of the block sample is reduced by 70% after rolling.

[0258] Step 5: Annealing

[0259] Under the protection of inert gas argon, the rolled sample obtained in step 4 is annealed in an environment of 1150°C for 3.0 min and air-cooled. This process can obtain the desired heterogeneous grain structure;

[0260] Step 6: Aging Process

[0261] Under the protection of inert gas argon, the annealed sample obtained in step 5 was subjected to aging treatment in an environment of 800° C. for 30 min and then air-cooled.

[0262] The high temperature performance test of the Ni-based alloy combined with homogeneous grain structure precipitation prepared in this embodiment at 700°C is as follows: The finished Ni-based alloy prepared in this embodiment has a tensile strength of 1090 MPa, a yield strength of 860 MPa, and an elongation of 21% (see Table 2 below).

[0263] Table 2: Performance test comparison of traditional GH4698 and the products of Examples 11-16 at 700°C

[0264]

[0265]

[0266] The above embodiments are only examples. For example, in addition to using argon as a protective gas, nitrogen or other inert gases may also be used. For another example, in addition to the GH4698 formula (i.e., the composition by mass percentage is: 13-16Cr, 1.4-1.8Al, 2.3-2.8Ti, 1.8-2.2Nb, 2.8-3.2Mo, the balance is Ni, and other unavoidable impurity elements), other Ni-based alloy formulas may also be used, as long as they contain Ni, Al and Ti elements at the same time.

[0267] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A heterogeneous grain structure precipitation strengthened Ni-based alloy, characterized in that: The alloy contains Ni, Al and Ti elements, and is composed of two sizes of heterogeneous grains, one large and one small, wherein the size of the small-sized grains is 1-10μm, and the volume fraction accounts for 50% to 70%; the size of the large-sized grains is 20-30μm, and the volume fraction accounts for 30% to 50%; a number of small-sized grains are aggregated, and a number of large-sized grains are aggregated, and the areas where these small-sized grains are aggregated and the areas where large-sized grains are aggregated are alternately distributed, and at the same time, the precipitated phase Ni3(Al,Ti) is also dispersed in these small-sized grains and large-sized grains.

2. The heterogeneous grain structure precipitation strengthened Ni-based alloy according to claim 1, characterized in that: The size of the precipitated phase Ni3(Al,Ti) is 10-45nm, and the volume fraction in the alloy is 18%-30%.

3. The heterogeneous grain structure precipitation strengthened Ni-based alloy according to claim 1, characterized in that: The alloy contains the following elements in mass percentages: 1-5% Al, 2-7% Ti, 30-60% Ni; Preferably, the alloy contains the following elements and their corresponding mass percentages: 13-16% Cr, 1.4-1.8% Al, 2.3-2.8% Ti, 1.8-2.2% Nb, 2.8-3.2% Mo, the balance being Ni, and other inevitable impurity elements.

4. The method for preparing a heterogeneous grain structure precipitation-strengthened Ni-based alloy according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. According to the preset element types and corresponding mass percentages of the Ni-based alloy, raw materials are prepared, and the raw materials are placed in a smelting furnace and smelted under a protective atmosphere to obtain an alloy ingot; the element types contained in the Ni-based alloy include Ni, Al and Ti elements; S2. The alloy ingot obtained in S1 is heated under a protective atmosphere, thereby free forging into a block to obtain a uniform equiaxed crystal structure; S3. The block obtained in S2 is solution treated under a protective atmosphere to obtain a uniform supersaturated solid solution; S4. The block obtained in S3 is subjected to liquid nitrogen cold rolling treatment to reduce the thickness by at least 60%, thereby obtaining a block of target thickness; S5. The block obtained in S4 is annealed in a protective atmosphere to form heterogeneous grains of two sizes, one large and one small, in the alloy, wherein the size of the small-sized grains is 1-10 μm, and the volume fraction accounts for 50% to 70%; the size of the large-sized grains is 20-30 μm, and the volume fraction accounts for 30% to 50%; S6. The block obtained in S5 is subjected to aging treatment under a protective atmosphere to generate a precipitated phase Ni3(Al,Ti) in the block, thereby obtaining a heterogeneous grain structure precipitation strengthened Ni-based alloy.

5. The preparation method according to claim 4, characterized in that: In step S5, the annealing treatment is performed at 1100-1150°C for 3-5.5 min; Preferably, after the annealing treatment is completed, the block is cooled by air cooling.

6. The preparation method according to claim 4, characterized in that: In step S6, the aging treatment temperature is 700-800°C, and the aging treatment time is 30-120min; Preferably, after the aging treatment is completed, cooling is performed by air cooling.

7. The preparation method according to claim 4, characterized in that: In step S1, the smelting furnace is specifically a vacuum induction smelting furnace; Accordingly, melting is performed under a protective atmosphere, specifically vacuum melting is performed under a protective atmosphere; Preferably, after the raw materials are placed in the vacuum induction melting furnace, the vacuum degree in the furnace is first evacuated to <9Pa, and then electric heating is supplied. When the vacuum degree continues to reach 1.2-0.6Pa, a protective atmosphere is then filled into the furnace.

8. The preparation method according to claim 4, characterized in that: In step S2, the alloy ingot obtained in S1 is heated in a protective atmosphere, specifically at a temperature of 1100-1150° C. for 150-210 min; Preferably, after free forging is completed, cooling is performed by air cooling.

9. The preparation method according to claim 4, characterized in that: In step S3, the solution treatment temperature used in the solution treatment is 1100-1120° C., the holding time is 90-120 min, and then the solution is cooled by water.

10. The preparation method according to claim 4, characterized in that: In step S4, the cold rolling treatment is to first immerse the block in liquid nitrogen for at least 3 minutes to completely cool the block, and then roll it, and repeat this process multiple times until the block reaches the target thickness; Preferably, the rolling speed is 4-6 m / min; More preferably, in steps S1, S2, S3, S5, and S6, the protective gas is independently selected from argon or nitrogen.