Vanadium-cobalt alloyed high-speed steel roller and preparation method thereof

By adding cobalt, aluminum and vanadium to high-speed steel rolls, optimizing the alloy composition and heat treatment process, a vanadium-cobalt alloyed high-speed steel roll is formed, which solves the problems of low high-temperature hardness and poor wear resistance of high-speed steel rolls and achieves high-temperature wear resistance. Improvement and production efficiency.

CN118756031APending Publication Date: 2024-10-11ANHUI HUANBOWAN HIGH SPEED STEEL MILL ROLL CO TTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410774102.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing high-speed steel rolls have low hardness and poor wear resistance at high temperatures, resulting in short service life and difficulty in meeting the high-efficiency needs of hot rolling production.

Method used

Add more cobalt and aluminum elements to the high-speed steel roll, control the alloy composition through the medium frequency induction furnace melting process, add high-hardness MC carbide to generate element vanadium, and use the wire feeding method and heat treatment process to optimize the roll structure to form a vanadium-cobalt alloy High-speed steel rolls.

Benefits of technology

The high-temperature hardness and wear resistance of high-speed steel rolls are significantly improved. The hardness at 650°C is greater than 780HV. The high-temperature wear resistance is more than 5 times higher than that of high-chromium cast iron rolls. The production process is simple, the production efficiency is high, and the cost is reduced by more than 40%. The service life is equivalent to that of carbide rollers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004895020420000151
    Figure BDA0004895020420000151
  • Figure HDA0004895020500000011
    Figure HDA0004895020500000011
Patent Text Reader

Abstract

The invention discloses a vanadium-cobalt alloyed high-speed steel roller and a preparation method thereof and belongs to the technical field of rollers. A vanadium-cobalt alloyed high-speed steel outer layer and a medium-carbon low-alloy steel roller shaft are compounded into a whole in a hot charging mode, and the vanadium-cobalt alloyed high-speed steel roller comprises the following chemical components: 3.03%-3.37% of C, 6.71%-6.98% of V, 11.58%-12.09% of Co, 12.53%-12.88% of Cr, 1.34%-1.52% of Al, 3.32%-3.57% of Mo, 0.14%-0.19% of N, 1.25%-1.39% of Si, 4.13%-4.47% of Mn and 1t. 0.030% S, lt; and 4.2-4.5 kg of metal cored wire per ton of molten steel is added into the molten steel by adopting a wire feeding method, so that the solidification structure of the high-speed steel is refined. The vanadium-cobalt alloyed high-speed steel roller is high in high-temperature hardness, good in high-temperature wear resistance and good in using effect on a hot rolling mill.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a high-speed steel roll and a preparation method thereof, in particular to a vanadium-cobalt alloyed high-speed steel roll and a preparation method thereof, belonging to the technical field of steel rolling. Background Art

[0002] With the continuous development of steel rolling technology, the continuous improvement of rolled steel grades, and the increasing requirements of steel companies for rolling line operation efficiency, rolling lines urgently need rolls with higher wear resistance and longer single-time rolling time. In recent years, new material rolls such as high-speed steel and semi-high-speed steel with better performance have replaced traditional high-chromium cast iron and high-nickel-chromium infinitely chilled cast iron rolls and have been widely used in hot rolling stands. The rolling mill has achieved certain results in extending the roll change cycle, reducing the number of roll changes, and improving rolling efficiency. At present, high-speed steel rolls have been widely used in hot rolling production lines.

[0003] In order to further improve the performance of high-speed steel rollers, Chinese invention patent CN116065082A discloses a method for manufacturing high-tungsten-vanadium high-speed steel wear-resistant rollers, which uses a purifier with a preset formula in an electric furnace, puts the pure molten steel into the electric furnace for smelting, and smelts until foam appears in the electric furnace, then adds alloy powder steel into the electric furnace, and waits to obtain smelted molten steel; the unprocessed rollers are refined for a preset time period in the refining furnace to obtain refined rollers; the refined rollers are placed in a vacuum heat treatment furnace for quenching treatment to obtain treated rollers; the electroslag is remelted for a preset time period to prepare electrode ingots; the treated rollers are ground for a preset time period to remove the fatigue layer attached to the rollers to obtain forged rollers; the smelted molten steel is used, and the forged rollers are cast for a preset time period in combination with the electrode ingots to obtain manufactured high-tungsten-vanadium high-speed steel wear-resistant rollers. The above process is complex for preparing high-speed steel rollers and has low production efficiency. Chinese invention patent CN114959506A also discloses a high-speed steel for ultra-thin stainless steel rolling rollers and a preparation method thereof. The chemical components of the high-speed steel for ultra-thin stainless steel rolling rollers of the invention include, by mass percentage: C: 1.00%-1.15%; Si: 0.20%-0.50%; Mn: 0.20%-0.40%; P: 0%-0.025%; S: 0%-0.020%; Cr: 4.50%-5.00%; Mo: 6.00%-6.50%; W: 7.00%-7.50%; V: 2.00%-2.30%; Co: 2.00%-3.00%; N: ≤0.005%; Ti: ≤0.011%; RE: 0.015-0.025%; the remainder is iron and impurities. The high-speed steel for ultra-thin stainless steel rolling rolls produced by the invention has fine MC carbide particles in the steel, and has a relatively good carbide structure, excellent red hardness, high strength and high toughness. Chinese invention patent CN114082922A also discloses a method for manufacturing a high-speed steel roller, characterized in that: the high-speed steel roller includes an outer layer and an inner core, the chemical composition of the outer layer is calculated by weight percentage: C1.2-1.4%, Si0.5-0.6%, Mn0.5-1.0%, P≤0.080%, S≤0.080%, Cr1.0-2.1%, Ni3.0-4.1%, Mo1.0-1.5% and V4.0-4.5%, and the balance is Fe; the chemical composition of the inner core layer is calculated by weight percentage: C3.1-3.5%, Si1.0-1.5%, Mn1.1-1.8%, P≤0.080%, S≤0.080%, Cr≤0.15%, Ni0.5-0.7% and Mg≥0.04%, and the balance is Fe.Chinese invention patent CN113667898A also discloses a high-vanadium high-speed steel composite roll and its manufacturing method, including: a roll working layer and a roll core roller shaft, wherein the roll working layer is made of high-vanadium high-speed steel, and the chemical composition weight percentage of the high-vanadium high-speed steel is: C1.5-2.2%, Si0.8-1.6%, Mn0.5-1.0%, Cr4.0-7.0%, Mo3.0-6.0%, V8.0-12.0%, P≤0.035%, S≤0.030% and the balance is Fe. The high-vanadium high-speed steel composite roll and its manufacturing method provided by the invention make the casting production of high-vanadium high-speed steel composite roll a reality, breaking the inherent production mode that can only rely on powder sintering. However, in the above-mentioned high-speed steel rolls, there is either too much tungsten element with high density added, which is easy to cause serious segregation due to the centrifugal force during the centrifugal casting process; or there is too much nickel element added, the amount of residual austenite in the heat treatment structure of the roll is too much, and the residual austenite in the use of the roll is easy to change due to the rolling force, resulting in large internal stress of the roll and easy cracking during use; or there is too much vanadium element added, which is easy to crack along the grain boundary, the matrix is ​​easy to wear first, the rolled material adheres to the roll surface, the roll surface is easy to be rough, the surface quality of the rolled material is reduced, and the roll replacement cycle is accelerated. In addition, too much vanadium element is added, the number of MC is too much, and the hardness is too high, which makes the roll grinding difficult. At the same time, with the increase of vanadium content, the size of alloy carbide MC increases, and the toughness and thermal fatigue performance of the high-speed steel roll decrease.

[0004] Chinese invention patent CN113621877A discloses a centrifugal composite high-speed steel roller for a rod and wire mill and its preparation method, which is formed by centrifugal composite casting of an outer layer, a primary core, and a secondary core; the chemical composition of the outer layer is C, Si, Mn, P, S, Cr, Ni, Mo, V, and the rest is iron and inevitable impurity elements; the chemical composition of the primary core is C, Si, Mn, P, S, Cr, Ni, M, and the rest is iron and inevitable impurity elements; the chemical composition of the secondary core is C, Si, Mn, P, S, Cr, Ni, Mo, V, W, Mg, Re, and the rest is iron and inevitable impurity elements. This invention aims at the rolling characteristics of the rod mill, through the reasonable allocation of chemical composition, and the use of special modification and heat treatment process technology, to produce a high-speed steel roller suitable for the rod and wire mill, which has stronger wear resistance and resistance to cold and hot fatigue. Chinese invention patent CN112831719A also discloses a durable high-speed steel roller and its manufacturing method, including a roller neck and a roller body composed of a working layer and a core, the chemical composition of the working layer is: 1.5-2.5% C, 0.90-1.50% Si, 0.40-1.40% Mn, P≤0.03%; S≤0.03%, 9.00-14.00% Cr, 0.50-2.00% Ni, 7.00-12.00% Mo, 1.00-3.00% V, 0.5-2.5% W, 0.10-1.00% Nb, and the rest is Fe and inevitable impurities. The invention effectively solves the problem of severe thermal cracking and large accident loss of conventional high-speed steel materials when used in the front section of hot-rolled strip finishing by designing reasonable alloy composition and heat treatment process, and improves the applicability of high-speed steel material rollers. Chinese invention patent CN112410673A also discloses a high-speed steel roll for rolling ultra-high strength steel plates and a manufacturing method thereof, including smelting and forging roll blanks, preliminary heat treatment and final heat treatment; the chemical composition and weight percentage are as follows: carbon 0.80-1.20%, silicon 0.20-1.45%, manganese 0.15-0.40%, chromium 7.70-8.30%, molybdenum 1.20-3.00%, vanadium 1.50-2.50%, tungsten 0.80-2.00%, niobium 0.40-0.60%, phosphorus ≤0.020%, sulfur ≤0.015%, and the rest are iron and unavoidable impurities. This invention optimizes the alloy composition and content on the one hand, and adopts injection molding instead of electroslag remelting to prepare steel ingots and adopts high-temperature overall quenching process on the other hand. It can eventually produce high-speed steel rolls with an overall hardness ≥ 62HRC and an internal grain size of 9 to 10, which can meet the complex working conditions of rolling ultra-high strength steel plates.Chinese invention patent CN111945053A also discloses a method for preparing a high-speed steel roll with composite modification treatment, wherein the high-speed steel roll material is smelted in a medium-frequency induction furnace, and the chemical composition and mass fraction of the molten steel in the furnace are controlled within 2.32-2.49% C, 4.17-4.33% W, 4.80-4.98% Mo, 9.63-9.85% Cr, 0.48-0.66% Mn, 0.57-0.81% Si, ≤0.035% S, ≤0.040% P, and the balance is Fe; then the molten steel is heated to 1615-1626°C, aluminum is added after being kept warm for 4-5 minutes, and then the molten steel is modified by a wire feeding method, and the molten steel is poured into a high-speed rotating mold on a centrifuge, and after the high-speed steel solidifies, the core is filled with ductile iron in a static state, and a high-speed steel roll with excellent performance and good use effect can be obtained after quenching and tempering. Chinese invention patent CN111101062A also discloses a hot-rolled improved centrifugal composite casting high Nb high-speed steel roll, comprising the following components by mass percentage: 1.50-1.70% C, 1.40-1.60% Si, 0.60-1.00% Mn, 1.00-1.50% Ni, 5.00-8.00% Cr, 3.00-5.00% Mo, 1.00-3.00% W, 4.00-6.00% Nb, 1.00-2.00% V, ≤0.03% S, ≤0.03% P, and the rest is Fe and unavoidable impurities. At the same time, the invention also discloses a preparation method of the above high Nb high-speed steel roll. The invention replaces the high-chromium steel rolls used for hot rolling roughing work rolls for a long time, breaks the composition restriction of traditional centrifugal composite high-speed steel, and this product can cover all the work rolls on the current hot rolling stand, and can also be used for rod and wire rolls, and ensures the consistency of the wear resistance of the entire roll. Chinese invention patent CN111151732A also discloses a method for preparing a high-speed steel roll for the rear section of headless strip rolling finishing, adopts three-layer centrifugal composite casting, and casts the outer layer, middle layer and core with high-strength ductile iron respectively, and controls the casting molten steel content of the middle layer and the core to be C1.8-2.8wt%, Si0.6-0.9wt%, Mn0.5-0.8wt%, Ni0.4-0.8wt%, P≤0.03wt%, S≤0.03wt%, Cr+Mo+Nb+V+W: 17-22wt%, and the balance is Fe and unavoidable impurities. The graphite obtained in the outer layer of this invention reduces the friction coefficient, while a certain amount of hard carbide enhances the wear resistance of the roller. This structure can effectively reduce the damage to the roller caused by the tail swing of the last stand. At the same time, the middle layer and the core adopt the method of wire feeding spheroidization and wire feeding inoculation (two wires each, a total of four wires fed simultaneously), which improves the spheroidization grade of ductile iron and the tensile strength, and greatly enhances the accident resistance of the roller.

[0005] Chinese invention patent CN110387506A discloses a highly wear-resistant centrifugal composite high-speed steel roller. The chemical composition and mass percentage are: outer layer: C1.6~1.9, Si0.30~0.80, Mn0.60~1.2, P≤0.035, S≤0.030, Cr3.50~6.50, Ni0.20~1.0, Mo3.0~6.0, V2.0~6.0, W2.0~6.0, Nb0.5~2.0, the rest is iron and impurities; middle layer and core: C2.95~3.4, Si2.0~3.0, Mn0.4~1.0, P≤0.05, S≤0.035, Re0.01~0.04, Mg0.03~0.08, Cr≤0.15, Ni≤0.5, Mo≤0.1, Cu≤0.1, the rest is iron and impurities. The invention has the characteristics of high hardness, high wear resistance, high heat strength and high red hardness. Chinese invention patent CN110343839A also discloses a heat treatment process for high-speed steel rolls. High-speed steel is a complex type of steel with a carbon content generally between 0.70% and 1.65%. It contains a large amount of alloy elements, with a total amount of up to 10% to 25%. According to the alloy elements contained, it can be divided into: ① tungsten high-speed steel (tungsten 9-18%); ② tungsten-molybdenum high-speed steel (tungsten 5-12%, molybdenum 2-6%); ③ high-molybdenum high-speed steel (tungsten 0-2%, molybdenum 5-10%); ④ vanadium high-speed steel, which is divided into high-speed steel with general vanadium content (vanadium 1-2%) and high vanadium content (vanadium 2.5-5%) according to the vanadium content; ⑤ cobalt high-speed steel (cobalt 5-10%). According to different uses, high-speed steel can be divided into general-purpose and special-purpose types. The heat treatment process of the high-speed steel of this invention performs a preheating during the quenching process to ensure the process requirements of quenching, enhance the impact toughness of the material, and perform two tempering treatments to make the tempering more sufficient.

[0006] Chinese invention patent CN110000362A also discloses a high-tungsten-vanadium high-speed steel wear-resistant roller and its manufacturing method, which uses an electric furnace to melt the outer layer high-speed steel molten steel and the roller core molten iron respectively, firstly melts the roller outer layer high-speed steel in the electric furnace, and controls the chemical composition and mass fraction of the molten steel in the furnace to 10.23-10.67% W, 1.76-1.94% Mo, 2.81-2.97% C, ≤0.035% P, ≤0.030% S, 6.15-6. 42% Cr, 2.27-2.46% Nb, 2.24-2.41% Si, 0.64-0.83% Mn, the balance is Fe and other inevitable impurities, then the molten steel is heated to 1653-1677℃, aluminum and ferrovanadium are added in sequence, and then multi-element alloy particles are added into the ladle, and cast into rollers on a vertical centrifuge. After heat treatment, it has good toughness and excellent wear resistance, and is used for rolling high-strength low-alloy hot-rolled rebar with excellent use effect. Chinese invention patent CN117483785A also discloses a method for preparing a semi-high-speed steel roller, which is prepared by laser melting deposition technology; the method comprises the following steps: ① preparing a ductile iron core layer; ② pre-treating semi-high-speed steel powder; the chemical composition and weight percentage of the semi-high-speed steel powder are as follows: carbon 0.74-1.20%, silicon 0.70-0.90%, manganese 0.25-0.45%, phosphorus ≤0.030%, sulfur ≤0.020%, chromium 5.00-5.50%, nickel 0.20-0.30%, molybdenum 0.96-1.20%, vanadium 0.40-1.20%, and the rest are iron and inevitable impurities; ③ using laser melting deposition technology to deposit the semi-high-speed steel powder onto the ductile iron core layer to obtain a semi-high-speed steel roller. The semi-high-speed steel roller prepared by the invention has small grain size, uniform distribution of eutectic carbides, high density, no defects such as cracks and pores, and has high hardness and wear resistance. However, the high-speed steel rolls prepared by the above method all have low high-temperature hardness of the rolls, and their high-temperature wear resistance is still far behind that of cemented carbide rolls with excellent performance. Summary of the invention

[0007] The present invention aims at the disadvantages of low high-temperature hardness and poor high-temperature wear resistance of commonly used high-speed steel rollers. In order to improve the high-temperature hardness of the high-speed steel roller, thereby improving the high-temperature wear resistance of the high-speed steel roller and extending the service life of the hot-rolled high-speed steel roller, the present invention adds more cobalt and aluminum elements to the high-speed steel roller to improve its high-temperature hardness. In addition, more high-hardness MC carbide generating element vanadium is added to further improve the wear resistance of the roller. The specific preparation process steps of the vanadium-cobalt alloyed high-speed steel roller of the present invention are:

[0008] ① Use scrap steel, ferromolybdenum, cobalt, ferrochrome, recarburizer, ferromanganese, ferrosilicon, aluminum, ferrovanadium and ferrochrome nitride as furnace charge, and use medium frequency induction furnace to melt high-speed steel molten steel; firstly, mix and melt scrap steel, ferromolybdenum, cobalt, ferrochrome and recarburizer, add ferromanganese and ferrosilicon after the molten steel is melted, continue to heat the molten steel to 1578-1593℃, keep it warm for 5-6 minutes, then add aluminum, ferrovanadium and ferrochrome nitride in turn; after all the furnace charge is melted, test the composition of the molten steel, and compare the chemical composition and The mass fraction is controlled at: 3.03-3.37% C, 6.71-6.98% V, 11.58-12.09% Co, 12.53-12.88% Cr, 1.34-1.52% Al, 3.32-3.57% Mo, 0.14-0.19% N, 1.25-1.39% Si, 4.13-4.47% Mn, <0.030% S, <0.035% P, the balance is Fe and unavoidable impurities; then the molten steel is discharged into the ladle;

[0009] ② After all the molten steel enters the ladle, the metal cored wire is added to the molten steel in the ladle by a wire feeding method, and the amount of the metal cored wire added is 4.2-4.5kg / ton of molten steel; the method for making the metal cored wire is to firstly mix granular passivation magnesium powder, 30-50 mesh rare earth ferrosilicon powder, 20-60nm TiN powder, and 30-50 mesh silicon calcium barium alloy powder; the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder are 35-38%, 35-38%, 12-13% and 13-16% respectively, and the total mass composition of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder is 100%; then the evenly mixed powders are packaged with a low-carbon mild steel strip with a thickness of 0.18-0.23mm, and rolled into a metal cored wire with a diameter of φ5.0-6.0mm on an alloy cored wire unit;

[0010] ③ After the metal cored wire is completely melted in the molten steel for 6-8 minutes, the slag is removed and the molten steel is allowed to stand. When the temperature of the molten steel in the ladle drops to 1418-1433°C, the molten steel is quickly poured into the high-speed rotating mold to obtain the outer layer high-speed steel of the roller. The mold speed is 1060-1120 rpm. When the temperature of the inner surface of the outer layer high-speed steel of the roller drops to 1290-1360°C, the mold speed is reduced to 860-900 rpm; when the temperature of the inner surface of the outer layer high-speed steel of the roller drops below 1000°C, the machine is stopped to take out the outer layer high-speed steel of the roller, and rough processing is performed after sand cleaning and grinding;

[0011] ④ The rough-machined outer layer high-speed steel of the roller is heated to 1080-1100℃ with the furnace, kept warm for 60-90 minutes, taken out of the furnace and air-cooled to a temperature below 400℃, re-entered the furnace and heated to 610-630℃, kept warm for 6-8 hours, cooled in the furnace to a temperature below 200℃, and taken out of the furnace and air-cooled; then the inner hole of the outer layer high-speed steel of the roller is finely machined; the outer layer high-speed steel of the roller with the finely machined inner hole is continued to be heated to 550-580℃ in the furnace, kept warm for 6-8 hours, taken out of the furnace when the furnace is cooled to 450-480℃, and quickly hot-assembled with the medium-carbon low-alloy steel roller shaft to obtain a high-speed steel combined roller with an interference of 0.23-0.28mm. Finally, the high-speed steel combined roller is finely machined to the specified size and accuracy to obtain a vanadium-cobalt alloyed high-speed steel roller.

[0012] As mentioned above, the chemical composition and mass fraction of ferrochromium nitride are: Cr≥60%, N≥5.0%, C≤0.1%, Si≤1.5%, P≤0.03%, S≤0.04%, and the remainder is Fe and unavoidable impurities.

[0013] As mentioned above, the chemical composition and mass fraction of rare earth ferrosilicon are: 27.22-30.68% RE, 39.16-41.85% Si, <3.0% Mn, <5.0% Ca, <3.0% Ti, and the remainder is Fe and unavoidable impurities.

[0014] The granular passivated magnesium powder as described above is characterized in that a flame retardant with a thickness of 0.35-0.50 mm is coated on the surface of granular metal magnesium powder with a particle size of 0.8-1.8 mm, and the flame retardant is composed of 25-35% by mass of CaO, 35-40% by mass of MgCl2 and 30-35% by mass of Al2O3.

[0015] As mentioned above, the chemical composition and mass fraction of the silicon-calcium-barium alloy are: 30.66-33.71% Si, 16.37-17.75% Ca, 19.08-19.69% Ba, ≤0.8% C, ≤0.04% P, ≤0.06% S, and the remainder is Fe and unavoidable impurities.

[0016] As mentioned above, the chemical composition and mass fraction of low carbon mild steel are: 0.17-0.37% Si, 0.48-0.73% Mn, 0.13-0.19% Cr, ≤0.2% C, ≤0.04% P, ≤0.03% S, and the balance is Fe and unavoidable impurities.

[0017] As described above, the medium carbon low alloy steel is any one of 40Cr steel, 42CrMo steel and 35CrMo steel.

[0018] The present invention mainly solves the problems that the commonly used high-speed steel roller has low high-temperature hardness and poor high-temperature wear resistance. In order to improve the high-temperature hardness of the high-speed steel roller, thereby improving the high-temperature wear resistance of the high-speed steel roller and extending the service life of the hot-rolled high-speed steel roller, the present invention adds more cobalt and aluminum elements to the high-speed steel roller to improve its high-temperature hardness, and also adds more high-hardness MC carbide generating element vanadium to further improve the wear resistance of the roller. The specific preparation process steps of the vanadium-cobalt alloyed high-speed steel roller of the present invention are: using scrap steel, ferromolybdenum, metal cobalt, ferrochrome, carburizer, ferromanganese, ferrosilicon, metal aluminum, ferrovanadium and nitrided chromium iron (the chemical composition and mass fraction of the nitrided chromium iron are: Cr≥60%, N≥5.0%, C≤0.1%, Si≤1.5%, P≤0.03%, S≤0.04%, and the balance is Fe and inevitable impurities) as furnace materials, and adopts a medium-frequency induction furnace to melt high-speed steel molten steel. The above-mentioned furnace materials are convenient to source domestically, do not need to be introduced from abroad, and have stable prices. The present invention first mixes scrap steel, ferromolybdenum, metal cobalt, ferrochrome and a carburizer for heating and melting, adds ferromanganese and ferrosilicon after the molten steel is melted, and is used for pre-deoxidation and alloying, and then continues to heat the molten steel to 1578-1593°C, keeps the temperature for 5-6 minutes, and then sequentially adds metal aluminum, ferrovanadium and ferrochrome nitride. Aluminum and vanadium elements are severely oxidized, and adding metal aluminum and ferrovanadium at high temperature can quickly melt them, thereby improving the recovery rate of aluminum and vanadium elements. In addition, ferrochrome nitride has a low melting point of only about 700°C, and adding ferrochrome nitride at high temperature can quickly melt the ferrochrome nitride, so that the nitrogen element is stably present in the high-speed steel melt. After all the charges are melted, the composition of the molten steel is tested, and the chemical composition and mass fraction of the molten steel in the furnace are controlled at: 3.03-3.37% C, 6.71-6.98% V, 11.58-12.09% Co, 12.53-12.88% Cr, 1.34-1.52% Al, 3.32-3.57% Mo, 0.14-0.19% N, 1.25-1.39% Si, 4.13-4.47% Mn, <0.030% S, <0.035% P, the remainder is Fe and unavoidable impurities; then the molten steel is discharged from the furnace into the ladle.

[0019] In the high-speed steel roller of the present invention, more cobalt and vanadium are added, wherein vanadium has a strong affinity with carbon. In the high-speed steel, increasing the vanadium content is equivalent to shifting all points in the solidification phase diagram to the left. With the increase of the vanadium content, the eutectic reaction temperature of the high-speed steel decreases, and the formation temperature of MC increases. Vanadium is not only conducive to the formation of MC type carbides, but also significantly promotes the formation of lamellar M2C type carbides and inhibits skeletal M6C type carbides. Among various carbides of high-speed steel, MC carbides have the highest hardness, and MC is difficult to dissolve during high-temperature austenitization. It exists in the residual phase, which is conducive to grain refinement and improved wear resistance. Increasing the vanadium content can also significantly improve the high-temperature hardness of high-speed steel, which is also very beneficial to improving the high-temperature wear resistance of high-speed steel rollers. If the vanadium content is too high, cracks are likely to occur along the grain boundaries, the matrix is ​​likely to wear preferentially, the rolled material adheres to the roller surface, the roller surface is likely to be rough, the surface quality of the rolled material is reduced, and the roller replacement cycle is accelerated. In addition, too many MCs and too high hardness make roller grinding difficult. At the same time, as the vanadium content increases, the size of the alloy carbide MC increases, and the toughness and thermal fatigue performance of the high-speed steel roller decrease. When the vanadium content in the high-speed steel roller exceeds 10%, low-hardness M3C type carbides appear in the eutectic structure, reducing the wear resistance of the high-speed steel roller. In addition to purifying the molten steel and reducing the content of inclusions and gases in the high-speed steel roller, vanadium also improves the ability of the high-speed steel roller to resist thermal shock. Therefore, the vanadium content in the high-speed steel roller is controlled at 6.71-6.98%.

[0020] Cobalt is the only alloying element that can significantly improve the high temperature hardness and secondary hardness of high speed steel. At the same time, cobalt can also improve the thermal conductivity of steel, especially at 600-700℃. Most of the cobalt in high speed steel is dissolved in the matrix, and only a very small amount is dissolved in carbides. As the cobalt content increases, the hardness of high speed steel increases. Cobalt is very beneficial to improving the wear resistance of high speed steel rolls. The main reason why cobalt improves the red hardness of high speed steel is that it can increase the melting point of high speed steel, so it can allow the quenching temperature to be increased without significant grain growth, which allows more Mo, Cr, V and C to be dissolved in austenite. These elements exist in the matrix together with cobalt, resulting in the formation of more residual austenite, thereby increasing the secondary hardness value and improving the red hardness. Cobalt can also increase the recrystallization temperature of martensite, so that the substructure of martensite is maintained at a higher temperature, thereby increasing the nucleation rate and dispersion of secondary carbides, and improving the red hardness of high speed steel rolls. However, cobalt reduces the strength and toughness of high speed steel. The higher the cobalt content, the more obvious the reduction. The main reason is that during tempering, cobalt promotes the precipitation of Cr and Mo from martensite, which strengthens precipitation hardening, improves secondary hardness and thermal conductivity, but reduces strength and toughness. In addition, as the cobalt content increases, the pearlite transformation nose time of high-speed steel is shortened, the critical cooling rate of pearlite transformation increases, and the hardenability of high-speed steel is reduced. In order to give full play to the beneficial role of cobalt, improve the high-temperature wear resistance of high-speed steel rollers and extend the service life of rollers, it is necessary to add an appropriate amount of cobalt to the high-speed steel rollers. The present invention controls the cobalt content to 11.58-12.09% Co. In order to overcome the adverse effects of cobalt, the present invention adds 4.13-4.47% Mn and 0.14-0.19% N to improve the hardenability of high-speed steel. The effect of nitrogen in expanding the austenite zone is about 30 times that of nickel. Adding 0.14-0.19% N can ensure that the high-speed steel has good hardenability and no pores. In addition, cobalt also has a tendency to increase the decarburization tendency of high-speed steel rollers. The higher the content, the greater the impact. In order to prevent decarburization of high-speed steel rolls, 12.53-12.88% Cr and 1.25-1.39% Si are added under the premise of lowering the quenching temperature and shortening the quenching and holding time, which is beneficial to prevent decarburization. Chromium exists partially in M6C carbides in high-speed steel and can also form M 23 C6 carbide, M 23C6 can be completely dissolved at a lower quenching temperature, so that the solid solution reaches carbon-chromium saturation without affecting the grain size. Chromium can also promote the more complete dissolution of M6C in austenite, thereby improving the hardenability and red hardness of high-speed steel. In addition, when high-speed steel is tempered at 450-525℃, part of the chromium precipitates from the martensite to promote dispersion hardening, and the other part of the chromium is retained in the α solid solution to prevent softening when heated to a higher temperature. Chromium can also reduce oxidation in high-speed steel. If the chromium content is too high, the excess chromium will participate in the formation of carbides precipitated during tempering. Such chromium-containing carbides are easy to precipitate at lower temperatures, reducing the thermal stability of high-speed steel. In addition, for rollers with low chromium content, the surface of the rollers tends to become rough during use due to the preferential wear of the matrix and the adhesion of the rolled material to the roller surface, which increases the rolling friction coefficient and rolling force. Increasing the chromium content so that the roller contains a certain amount of M7C3 carbides is beneficial to improving the roughness resistance of the roller surface and reducing the rolling force. The increase of chromium content is also beneficial to improve the thermal shock resistance of high-speed steel rollers. The suitable chromium content in the high-speed steel roller of the present invention is 12.53-12.88% Cr. Al is dissolved in the matrix, which can improve the tempering stability, hardness and red hardness of high-speed steel. Al also reduces the decomposition temperature of M2C eutectic carbide, making it easy to decompose and granulate eutectic carbide when heated at high temperature, which is beneficial to improve the toughness of high-speed steel. However, Al increases the decarburization sensitivity of high-speed steel. Considering all factors, the Al content is controlled at 1.34-1.52%.

[0021] After all the molten steel enters the ladle, the metal cored wire is added to the molten steel in the ladle by a wire feeding method, and the amount of the metal cored wire added is 4.2-4.5 kg / ton of molten steel. The method for making the metal cored wire is as follows: first, granular passivated magnesium powder (the granular passivated magnesium powder is characterized in that: a flame retardant with a thickness of 0.35-0.50 mm is coated on the surface of granular metal magnesium powder with a particle size of 0.8-1.8 mm, and the flame retardant is composed of 25-35% by mass of CaO, 35-40% by mass of MgC l2 and 30-35% Al2O3), 30-50 mesh rare earth ferrosilicon powder (the chemical composition and mass fraction of the rare earth ferrosilicon are: 27.22-30.68% RE, 39.16-41.85% Si, <3.0% Mn, <5.0% Ca, <3.0% Ti, the balance is Fe and inevitable impurities), 20-60nm TiN powder, 30-50 mesh silicon calcium barium alloy powder (the chemical composition and mass fraction of the silicon calcium barium alloy are: 30.66- 33.71% Si, 16.37-17.75% Ca, 19.08-19.69% Ba, ≤0.8% C, ≤0.04% P, ≤0.06% S, the balance is Fe and unavoidable impurities) are mixed evenly; the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon-calcium-barium alloy powder are 35-38%, 35-38%, 12-13% and 13-16% respectively, and the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon-calcium-barium alloy powder are 35-38%, 35-38%, 12-13% and 13-16% respectively. The total mass composition is 100%; the uniformly mixed powder is then packed with a 0.18-0.23mm thick low carbon mild steel (the chemical composition and mass fraction of the low carbon mild steel are: 0.17-0.37% Si, 0.48-0.73% Mn, 0.13-0.19% Cr, ≤0.2% C, ≤0.04% P, ≤0.03% S, and the balance is Fe and inevitable impurities) steel strip, and rolled into a metal cored wire with a diameter of φ5.0-6.0mm on an alloy cored wire unit. The metal cored wire processed by adding granular passivation magnesium powder, rare earth ferrosilicon powder, nano TiN powder and silicon calcium barium alloy powder with mass compositions of 35-38%, 35-38%, 12-13% and 13-16% respectively can significantly refine the solidification structure of high speed steel, and also has the comprehensive effects of purifying the high speed steel structure, reducing inclusions, and improving the strength, toughness and thermal fatigue resistance of high speed steel. In particular, TiN has a melting point of 2950°C, good thermal shock resistance, and will not melt when added to molten steel. Nano-TiN can serve as the solidification crystallization core of primary austenite and promote significant refinement of the solidification structure.

[0022] After the metal cored wire of the present invention is completely melted in the molten steel for 6-8 minutes, the slag is removed and the molten steel is allowed to stand. When the temperature of the molten steel in the ladle drops to 1418-1433°C, the molten steel is quickly poured into a high-speed rotating mold to obtain the outer layer high-speed steel of the roller. The mold speed is 1060-1120 rpm. When the temperature of the inner surface of the outer layer high-speed steel of the roller drops to 1290-1360°C, the mold speed is reduced to 860-900 rpm to reduce the risk of high-speed steel cracking. When the temperature of the inner surface of the outer layer high-speed steel of the roller drops below 1000°C, the machine is stopped to take out the outer layer high-speed steel of the roller, and rough processing is performed after sand cleaning and grinding. The rough-processed outer layer high-speed steel of the roller is heated to 1080-1100°C with the furnace, and after keeping warm for 60-90 minutes, it is taken out of the furnace and air-cooled to a temperature below 400°C, so that a martensite + residual austenite matrix structure can be obtained, and the pearlite structure is eliminated. Re-enter the furnace and heat it to 610-630℃. After keeping it warm for 6-8 hours, cool it to a temperature below 200℃ and air cool it out of the furnace. This can eliminate the residual austenite and improve the wear resistance of the high-speed steel roller. Then, the inner hole of the high-speed steel on the outer layer of the roller is fine-machined. The high-speed steel on the outer layer of the roller with the finely machined inner hole is continued to be heated to 550-580℃. After keeping it warm for 6-8 hours, cool it to 450-480℃ and take it out of the furnace to eliminate the internal stress of the high-speed steel. At this time, it is quickly hot-assembled with the medium-carbon low-alloy steel roller shaft to obtain a high-speed steel composite roller with an interference of 0.23-0.28mm. Finally, the high-speed steel composite roller is fine-machined to the specified size and accuracy to obtain a vanadium-cobalt alloyed high-speed steel roller.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] (1) The high-speed steel roll of the present invention has high high-temperature hardness, with a hardness of more than 780 HV at 650°C, and has excellent high-temperature wear resistance. The high-temperature wear resistance of the high-speed steel roll of the present invention at 650°C is more than 5 times that of the high-chromium cast iron roll, and more than 60% that of the ordinary high-speed steel roll;

[0025] (2) The high-speed steel roller production process of the present invention is simple, the production efficiency is high, the roller shaft can be reused, and energy saving and consumption reduction are obvious;

[0026] (3) The high-speed steel roller of the present invention has high hardness, with a room temperature hardness greater than 850 HV and an impact toughness greater than 14 J / cm 2 , when rolling rebar on a hot rolling mill, its service life is equivalent to that of a cemented carbide roll, and its production cost is reduced by more than 40%. Its promotion and application will have good economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of high speed steel roll

[0028] 1-Outer layer high speed steel, 2-Roller. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below with reference to the examples, but the present invention is not limited to the following examples.

[0030] Embodiment 1:

[0031] A vanadium-cobalt alloyed high-speed steel roll and a preparation method thereof are provided. The vanadium-cobalt alloyed high-speed steel roll is obtained by hot-packing and compounding a vanadium-cobalt alloyed high-speed steel outer layer 1 and a 40Cr medium-carbon low-alloy steel roll shaft 2. The specific preparation process steps are as follows:

[0032] ① Use scrap steel, ferromolybdenum, metal cobalt, ferrochrome, carburizer, ferromanganese, ferrosilicon, metal aluminum, ferrovanadium and ferrochrome nitride as furnace materials, and adopt medium frequency induction furnace to melt high speed steel liquid steel; firstly, mix scrap steel, ferromolybdenum, metal cobalt, ferrochrome and carburizer and heat and melt them, add ferromanganese and ferrosilicon after the molten steel is melted, continue to heat the molten steel to 1578℃, keep it warm for 6 minutes, then add metal aluminum, ferrovanadium and ferrochrome nitride in turn (the chemical composition and mass fraction of the ferrochrome nitride are: 62.74%Cr, 5.85%N, 0.06%C, 1.22%Si , 0.028% P, 0.035% S, the balance is Fe and inevitable impurities); after all the charges are melted, the composition of the molten steel is tested, and the chemical composition and mass fraction of the molten steel in the furnace are controlled at: 3.03% C, 6.98% V, 11.58% Co, 12.88% Cr, 1.34% Al, 3.57% Mo, 0.14% N, 1.39% Si, 4.13% Mn, 0.024% S, 0.032% P, the balance is Fe and inevitable impurities; then the molten steel is discharged from the furnace into the ladle;

[0033] ② After all the molten steel enters the ladle, the metal cored wire is added to the molten steel in the ladle by a wire feeding method, and the amount of the metal cored wire added is 4.2kg / ton of molten steel; the method for making the metal cored wire is to firstly coat the surface of granular passivated magnesium powder (the granular passivated magnesium powder is characterized in that: a flame retardant with a thickness of 0.35-0.39mm is coated on the surface of granular metal magnesium powder with a particle size of 0.8-1.8mm, and the flame retardant is composed of 25% by mass of CaO, 40% by mass of MgCl2 and 35% by mass of Al2O3), 30-50 mesh rare earth ferrosilicon (the chemical composition and mass fraction of the rare earth ferrosilicon are: 27.22% RE, 41.85% Si, 1.46% Mn, 2.82% Ca, 1.17% Ti, and the balance is Fe and inevitable impurities) powder, 20-60nm TiN powder, 30-50 mesh silicon calcium barium alloy (the chemical composition and mass fraction of the silicon calcium barium alloy are: The mass fraction is: 30.66% Si, 17.75% Ca, 19.08% Ba, 0.37% C, 0.029% P, 0.051% S, the balance is Fe and inevitable impurities) powder is mixed evenly; the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder are 35%, 38%, 12% and 15% respectively, and the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder are 35%, 38%, 12% and 15% respectively. The total mass composition of the alloy powder is 100%; the uniformly mixed powder is then packed with a 0.18 mm thick low carbon mild steel (the chemical composition and mass fraction of the low carbon mild steel are: 0.17% Si, 0.73% Mn, 0.13% Cr, 0.17% C, 0.035% P, 0.022% S, and the balance is Fe and unavoidable impurities) steel strip, and rolled into a metal cored wire with a diameter of φ5.0 mm on an alloy cored wire unit;

[0034] ③ After the metal cored wire is completely melted in the molten steel for 7 minutes, the slag is removed and the molten steel is allowed to stand. When the temperature of the molten steel in the ladle drops to 1427°C, the molten steel is quickly poured into a high-speed rotating mold to obtain the outer layer high-speed steel 1 of the roller. The mold speed is 1090 rpm. When the temperature of the inner surface of the outer layer high-speed steel 1 of the roller drops to 1310-1340°C, the mold speed is reduced to 880 rpm. When the temperature of the inner surface of the outer layer high-speed steel 1 of the roller drops below 1000°C, the machine is stopped to take out the outer layer high-speed steel 1 of the roller, and rough processing is performed after sand cleaning and grinding.

[0035] ④ The rough-machined roller outer layer high-speed steel 1 is heated to 1090℃ with the furnace, kept warm for 80 minutes, taken out of the furnace and air-cooled to a temperature below 400℃, then re-entered the furnace and heated to 620℃, kept warm for 7 hours, cooled in the furnace to a temperature below 200℃, and taken out of the furnace and air-cooled; then the inner hole of the roller outer layer high-speed steel 1 is finely machined; the roller outer layer high-speed steel 1 with the finely machined inner hole is continued to be heated to 570℃ in the furnace, kept warm for 7 hours, and taken out of the furnace when the furnace is cooled to 460℃, and quickly hot-assembled with the 40Cr medium-carbon low-alloy steel roller shaft 2 to obtain a high-speed steel combined roller with an interference of 0.25mm. Finally, the high-speed steel combined roller is finely machined to the specified size and accuracy to obtain a vanadium-cobalt alloyed high-speed steel roller. Its mechanical properties are shown in Table 1.

[0036] Embodiment 2:

[0037] A vanadium-cobalt alloyed high-speed steel roll and a preparation method thereof are provided. The vanadium-cobalt alloyed high-speed steel roll is obtained by hot-packing and compounding a vanadium-cobalt alloyed high-speed steel outer layer 1 and a 42CrMo medium-carbon low-alloy steel roll shaft 2. The specific preparation process steps are as follows:

[0038] ① Use scrap steel, ferromolybdenum, metal cobalt, ferrochrome, carburizer, ferromanganese, ferrosilicon, metal aluminum, ferrovanadium and ferrochrome nitride as furnace materials, and adopt medium frequency induction furnace to melt high-speed steel molten steel; firstly, mix scrap steel, ferromolybdenum, metal cobalt, ferrochrome and carburizer and heat and melt them, add ferromanganese and ferrosilicon after the molten steel is melted, continue to heat the molten steel to 1593℃, keep it warm for 5 minutes, then add metal aluminum, ferrovanadium and ferrochrome nitride in turn (the chemical composition and mass fraction of the ferrochrome nitride are: 61.80%Cr, 5.41%N, 0.07%C, 1.16%Si , 0.025% P, 0.033% S, the balance is Fe and inevitable impurities); after all the charges are melted, the composition of the molten steel is tested, and the chemical composition and mass fraction of the molten steel in the furnace are controlled at: 3.37% C, 6.71% V, 12.09% Co, 12.53% Cr, 1.52% Al, 3.32% Mo, 0.19% N, 1.25% Si, 4.47% Mn, 0.028% S, 0.029% P, the balance is Fe and inevitable impurities; then the molten steel is discharged from the furnace into the ladle;

[0039] ② After all the molten steel enters the ladle, the metal cored wire is added to the molten steel in the ladle by a wire feeding method, and the amount of the metal cored wire added is 4.5kg / ton of molten steel; the method for making the metal cored wire is to first coat the surface of granular passivated magnesium powder (the granular passivated magnesium powder is characterized in that: a flame retardant with a thickness of 0.44-0.50mm is coated on the surface of granular metal magnesium powder with a particle size of 0.8-1.8mm, and the flame retardant is composed of 35% by mass of CaO, 35% by mass of MgCl2 and 30% by mass of Al2O3), 30-50 mesh rare earth ferrosilicon (the chemical composition and mass fraction of the rare earth ferrosilicon are: 30.68% RE, 39.16% Si, 2.06% Mn, 3.88% Ca, 1.63% Ti, and the balance is Fe and inevitable impurities) powder, 20-60nm TiN powder, 30-50 mesh silicon calcium barium alloy (the chemical composition and mass fraction of the silicon calcium barium alloy are: 30.68% RE, 39.16% Si, 2.06% Mn, 3.88% Ca, 1.63% Ti, and the balance is Fe and inevitable impurities) powder. The mass compositions of the granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon-calcium-barium alloy powder are 38%, 36%, 13% and 13% respectively. The total mass composition of the gold powder is 100%; the uniformly mixed powder is then packed with a 0.23mm thick low-carbon mild steel (as mentioned above, the chemical composition and mass fraction of the low-carbon mild steel are: 0.37% Si, 0.48% Mn, 0.19% Cr, 0.14% C, 0.027% P, 0.024% S, and the balance is Fe and unavoidable impurities) steel strip, and rolled into a metal cored wire with a diameter of φ6.0mm on an alloy cored wire unit;

[0040] ③ After the metal cored wire is completely melted in the molten steel for 8 minutes, the slag is removed and the molten steel is allowed to stand. When the temperature of the molten steel in the ladle drops to 1433°C, the molten steel is quickly poured into a high-speed rotating mold to obtain the outer layer high-speed steel 1 of the roller. The mold speed is 1120 rpm. When the temperature of the inner surface of the outer layer high-speed steel 1 of the roller drops to 1335-1360°C, the mold speed is reduced to 900 rpm. When the temperature of the inner surface of the outer layer high-speed steel 1 of the roller drops below 1000°C, the machine is stopped to take out the outer layer high-speed steel 1 of the roller, and rough processing is performed after sand cleaning and grinding.

[0041] ④ The rough-machined roller outer layer high-speed steel 1 is heated to 1100℃ with the furnace, kept warm for 60 minutes, taken out of the furnace and air-cooled to a temperature below 400℃, then re-entered the furnace and heated to 630℃, kept warm for 6 hours, cooled in the furnace to a temperature below 200℃, and taken out of the furnace and air-cooled; then the inner hole of the roller outer layer high-speed steel 1 is finely machined; the roller outer layer high-speed steel 1 with the finely machined inner hole is continued to be heated to 580℃ in the furnace, kept warm for 6 hours, and taken out of the furnace when the furnace is cooled to 480℃, and quickly hot-assembled with the 42CrMo medium-carbon low-alloy steel roller shaft 2 to obtain a high-speed steel combined roller with an interference of 0.28mm. Finally, the high-speed steel combined roller is finely machined to the specified size and accuracy to obtain a vanadium-cobalt alloyed high-speed steel roller. Its mechanical properties are shown in Table 1.

[0042] Embodiment 3:

[0043] A vanadium-cobalt alloyed high-speed steel roll and a preparation method thereof are provided. The vanadium-cobalt alloyed high-speed steel roll is obtained by hot-packing and compounding a vanadium-cobalt alloyed high-speed steel outer layer 1 and a 35CrMo medium-carbon low-alloy steel roll shaft 2. The specific preparation process steps are as follows:

[0044] ① Use scrap steel, ferromolybdenum, metal cobalt, ferrochrome, carburizer, ferromanganese, ferrosilicon, metal aluminum, ferrovanadium and ferrochrome nitride as furnace materials, and adopt medium frequency induction furnace to melt high speed steel liquid steel; firstly, mix scrap steel, ferromolybdenum, metal cobalt, ferrochrome and carburizer and heat and melt them, add ferromanganese and ferrosilicon after the molten steel is melted, continue to heat the molten steel to 1586℃, keep it warm for 5.5 minutes, then add metal aluminum, ferrovanadium and ferrochrome nitride in turn (the chemical composition and mass fraction of the ferrochrome nitride are: 62.72%Cr, 5.70%N, 0.08%C, 1.16%S i, 0.029% P, 0.031% S, the balance is Fe and inevitable impurities); after all the charges are melted, the composition of the molten steel is tested, and the chemical composition and mass fraction of the molten steel in the furnace are controlled to be: 3.26% C, 6.85% V, 11.74% Co, 12.70% Cr, 1.48% Al, 3.51% Mo, 0.17% N, 1.32% Si, 4.38% Mn, 0.024% S, 0.031% P, the balance is Fe and inevitable impurities; then the molten steel is discharged from the furnace into a ladle;

[0045] ② After all the molten steel enters the ladle, the metal cored wire is added to the molten steel in the ladle by a wire feeding method, and the amount of the metal cored wire added is 4.3kg / ton of molten steel; the method for making the metal cored wire is to first coat the surface of granular passivated magnesium powder (the granular passivated magnesium powder is characterized in that: a flame retardant with a thickness of 0.38-0.43mm is coated on the surface of granular metal magnesium powder with a particle size of 0.8-1.8mm, and the flame retardant is composed of 30% by mass of CaO, 38% by mass of MgCl2 and 32% by mass of Al2O3), 30-50 mesh rare earth ferrosilicon (the chemical composition and mass fraction of the rare earth ferrosilicon are: 28.71% RE, 40.67% Si, 1.37% Mn, 2.66% Ca, 1.29% Ti, and the balance is Fe and inevitable impurities) powder, 20-60nm TiN powder, 30-50 mesh silicon calcium barium alloy (the chemical composition and mass fraction of the silicon calcium barium alloy are: The mass fractions are: 32.52% Si, 16.84% Ca, 19.55% Ba, 0.41% C, 0.028% P, 0.037% S, the balance is Fe and unavoidable impurities) powders are mixed evenly; the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder are 37%, 36%, 13% and 14% respectively, and the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder are 37%, 36%, 13% and 14% respectively. The total mass composition of the alloy powder is 100%; the uniformly mixed powder is then packed with a 0.20 mm thick low-carbon mild steel (the chemical composition and mass fraction of the low-carbon mild steel are: 0.26% Si, 0.57% Mn, 0.16% Cr, 0.18% C, 0.037% P, 0.021% S, and the balance is Fe and unavoidable impurities) steel strip, and rolled into a metal cored wire with a diameter of φ5.5 mm on an alloy cored wire unit;

[0046] ③ After the metal cored wire is completely melted in the molten steel for 6 minutes, the slag is removed and the molten steel is allowed to stand. When the temperature of the molten steel in the ladle drops to 1418°C, the molten steel is quickly poured into a high-speed rotating mold to obtain the outer layer high-speed steel 1 of the roller. The mold speed is 1060 rpm. When the temperature of the inner surface of the outer layer high-speed steel 1 of the roller drops to 1290-1320°C, the mold speed is reduced to 860 rpm. When the temperature of the inner surface of the outer layer high-speed steel 1 of the roller drops below 1000°C, the machine is stopped to take out the outer layer high-speed steel 1 of the roller, and rough processing is performed after sand cleaning and grinding.

[0047] ④ The rough-machined roller outer layer high-speed steel 1 is heated to 1080℃ with the furnace, kept warm for 90 minutes, taken out of the furnace and air-cooled to a temperature below 400℃, then re-entered the furnace and heated to 610℃, kept warm for 8 hours, cooled in the furnace to a temperature below 200℃, and taken out of the furnace and air-cooled; then the inner hole of the roller outer layer high-speed steel 1 is finely machined; the roller outer layer high-speed steel 1 with the finely machined inner hole is continued to be heated to 550℃ in the furnace, kept warm for 8 hours, and taken out of the furnace when the furnace is cooled to 450℃, and quickly hot-assembled with the 35CrMo medium-carbon low-alloy steel roller shaft 2 to obtain a high-speed steel combined roller with an interference of 0.23mm. Finally, the high-speed steel combined roller is finely machined to the specified size and accuracy to obtain a vanadium-cobalt alloyed high-speed steel roller. Its mechanical properties are shown in Table 1.

[0048] Table 1 Mechanical properties of vanadium-cobalt alloyed high-speed steel rolls

[0049]

[0050] Due to the large amount of cobalt, aluminum and silicon added, the high-speed steel roller of the present invention has high high-temperature hardness, and the hardness at 650°C is greater than 780HV, and it has excellent high-temperature wear resistance. A high-temperature wear test at 650°C was carried out on a high-temperature wear testing machine. The high-temperature wear resistance of the high-speed steel roller material of the present invention at 650°C is more than 5 times higher than that of high-chromium cast iron roller material, and more than 60% higher than that of ordinary high-speed steel roller material. The production process of the high-speed steel roller of the present invention is simple, the production efficiency is high, the roller shaft can be reused, and energy saving and consumption reduction are obvious. The high-speed steel roller of the present invention has high hardness, the room temperature hardness is greater than 850HV, and the impact toughness is greater than 14J / cm 2 The tensile strength is greater than 820MPa. When rolling threaded steel on a hot rolling mill, the amount of steel passing through a single groove and the amount of roller grinding are equivalent to those of a hard alloy roller, and the production cost is reduced by more than 40%. The invention also overcomes the shortcomings of the hard alloy roller being brittle and prone to cracking during use. The promotion and application of the roller of the invention has good economic and social benefits.

Claims

1. A method for preparing a vanadium-cobalt alloyed high-speed steel roll, It is characterized in that The following steps are involved: ① Use scrap steel, ferromolybdenum, cobalt, ferrochrome, recarburizer, ferromanganese, ferrosilicon, aluminum, ferrovanadium and ferrochrome nitride as furnace charge, and use medium frequency induction furnace to melt high-speed steel molten steel; firstly, mix and melt scrap steel, ferromolybdenum, cobalt, ferrochrome and recarburizer, add ferromanganese and ferrosilicon after the molten steel is melted, continue to heat the molten steel to 1578-1593℃, keep it warm for 5-6 minutes, then add aluminum, ferrovanadium and ferrochrome nitride in turn; after all the furnace charge is melted, test the composition of the molten steel, and compare the chemical composition and The mass fraction is controlled at: 3.03-3.37% C, 6.71-6.98% V, 11.58-12.09% Co, 12.53-12.88% Cr, 1.34-1.52% Al, 3.32-3.57% Mo, 0.14-0.19% N, 1.25-1.39% Si, 4.13-4.47% Mn, <0.030% S, <0.035% P, the balance is Fe and unavoidable impurities; then the molten steel is discharged into the ladle; ② After all the molten steel enters the ladle, the metal cored wire is added to the molten steel in the ladle by a wire feeding method, and the amount of the metal cored wire added is 4.2-4.5kg / ton of molten steel; the method for making the metal cored wire is to firstly mix granular passivation magnesium powder, 30-50 mesh rare earth ferrosilicon powder, 20-60nm TiN powder, and 30-50 mesh silicon calcium barium alloy powder; the mass compositions of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder are 35-38%, 35-38%, 12-13% and 13-16% respectively, and the total mass composition of granular passivation magnesium powder, rare earth ferrosilicon powder, nano-TiN powder and silicon calcium barium alloy powder is 100%; then the evenly mixed powders are packaged with a low-carbon mild steel strip with a thickness of 0.18-0.23mm, and rolled into a metal cored wire with a diameter of φ5.0-6.0mm on an alloy cored wire unit; ③ After the metal cored wire is completely melted in the molten steel for 6-8 minutes, the slag is removed and the molten steel is allowed to stand. When the temperature of the molten steel in the ladle drops to 1418-1433°C, the molten steel is quickly poured into the high-speed rotating mold to obtain the outer layer high-speed steel of the roller. The mold speed is 1060-1120 rpm. When the temperature of the inner surface of the outer layer high-speed steel of the roller drops to 1290-1360°C, the mold speed is reduced to 860-900 rpm; when the temperature of the inner surface of the outer layer high-speed steel of the roller drops below 1000°C, the machine is stopped to take out the outer layer high-speed steel of the roller, and rough processing is performed after sand cleaning and grinding; ④ The rough-machined outer layer high-speed steel of the roller is heated to 1080-1100℃ with the furnace, kept warm for 60-90 minutes, taken out of the furnace and air-cooled to a temperature below 400℃, re-entered the furnace and heated to 610-630℃, kept warm for 6-8 hours, cooled in the furnace to a temperature below 200℃, and taken out of the furnace and air-cooled; then the inner hole of the outer layer high-speed steel of the roller is finely machined; the outer layer high-speed steel of the roller with the finely machined inner hole is continued to be heated to 550-580℃ in the furnace, kept warm for 6-8 hours, taken out of the furnace when the furnace is cooled to 450-480℃, and quickly hot-assembled with the medium-carbon low-alloy steel roller shaft to obtain a high-speed steel combined roller with an interference of 0.23-0.28mm. Finally, the high-speed steel combined roller is finely machined to the specified size and accuracy to obtain a vanadium-cobalt alloyed high-speed steel roller.

2. A method for preparing a vanadium-cobalt alloyed high-speed steel roll according to claim 1, It is characterized in that The chemical composition and mass fraction of the ferrochromium nitride are: Cr≥60%, N≥5.0%, C≤0.1%, Si≤1.5%, P≤0.03%, S≤0.04%, and the remainder is Fe and unavoidable impurities.

3. A method for preparing a vanadium-cobalt alloyed high-speed steel roll according to claim 1, It is characterized in that The chemical composition and mass fraction of the rare earth ferrosilicon are: 27.22-30.68% RE, 39.16-41.85% Si, <3.0% Mn, <5.0% Ca, <3.0% Ti, and the remainder is Fe and unavoidable impurities.

4. A method for preparing a vanadium-cobalt alloyed high-speed steel roll according to claim 1, It is characterized in that The granular passivated magnesium powder is a granular magnesium powder with a particle size of 0.8-1.8 mm, on the surface of which a flame retardant with a thickness of 0.35-0.50 mm is coated. The flame retardant is composed of 25-35% by mass of CaO, 35-40% by mass of MgCl 2 and 30-35% Al 2 O 3 composition.

5. A method for preparing a vanadium-cobalt alloyed high-speed steel roll according to claim 1, It is characterized in that The chemical composition and mass fraction of the silicon-calcium-barium alloy are: 30.66-33.71% Si, 16.37-17.75% Ca, 19.08-19.69% Ba, ≤0.8% C, ≤0.04% P, ≤0.06% S, and the remainder is Fe and unavoidable impurities.

6. A method for preparing a vanadium-cobalt alloyed high-speed steel roll according to claim 1, It is characterized in that The chemical composition and mass fraction of the low carbon mild steel are: 0.17-0.37% Si, 0.48-0.73% Mn, 0.13-0.19% Cr, ≤0.2% C, ≤0.04% P, ≤0.03% S, and the remainder is Fe and unavoidable impurities.

7. A method for preparing a vanadium-cobalt alloyed high-speed steel roll according to claim 1, It is characterized in that The medium carbon low alloy steel is any one of 40Cr steel, 42CrMo steel and 35CrMo steel.

8. A vanadium-cobalt alloyed high-speed steel roll prepared according to the method of any one of claims 1 to 7.

Citation Information

Cited By

  • Preparation method of wear-resistant high-speed steel plate strip roller

    CN120984854A