Process for preparing target blank from high-purity terbium dysprosium

By mixing metallic terbium or dysprosium with high-purity calcium fluoride, smelting and die-casting in a vacuum smelting furnace, the purity and density of the target material are successfully improved, and the problem of difficulty in improving the purity of the target material in the existing technology is solved. , achieving the preparation and large-scale production of high-purity target materials.

CN118756104APending Publication Date: 2024-10-11GUANGXI GUOCHEN RARE EARTH METAL MATERIAL CO LTD

Patent Information

Application Number
CN202410827856.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, the density of metal dysprosium or terbium target materials is low and the purity is difficult to improve.

Method used

After the ingot of metal terbium or dysprosium is evenly mixed with high-purity calcium fluoride, it is smelted in a vacuum smelting furnace. The temperature and current intensity are controlled, and argon gas protection is used for smelting. The surface slag is then peeled off by a die-casting machine to obtain high-purity Target material.

Benefits of technology

It achieves the preparation of high-purity (up to 99.99%) metal terbium or dysprosium targets, solving the problems of low density and difficulty in improving purity. The process is simple and suitable for large-scale and automated production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756104A_ABST
    Figure CN118756104A_ABST
Patent Text Reader

Abstract

The invention discloses a process for preparing a target material blank by using high-purity terbium dysprosium, which comprises the following steps: crushing a cast ingot of metal terbium or metal dysprosium, and uniformly mixing the crushed cast ingot with calcium fluoride to obtain a mixed material, the weight ratio of the cast ingot to the calcium fluoride being (99.0-99.2): 1; the mixed material is added into a vacuum smelting furnace to be smelted, the smelting temperature ranges from 800 DEG C to 1500 DEG C, and the current intensity ranges from 4000 A to 12000 A; before smelting is started, argon is filled into the vacuum smelting furnace, and the pressure of an argon source is maintained at 1 MPa; after smelting is finished, the molten metal is subjected to heat preservation for 1-4 h at the temperature of 700-750 DEG C and then cooled, a blank is obtained, the blank is pressed and vibrated through a die-casting machine, surface slag is stripped, and a high-purity target material blank of the metal terbium or the metal dysprosium is obtained. By means of the method, the high-purity metal terbium target material and the high-purity metal dysprosium target material can be produced, and the problems that an existing target material is low in density, and the purity is difficult to improve are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth processing, and in particular relates to a process for preparing a target material body by using high-purity terbium and dysprosium. Background Art

[0002] Rare earth metals have unique electronic structures and chemical properties, making them widely used in contemporary communication technology, electronic computers, aerospace development, medicine and health, photosensitive materials, optoelectronic materials, energy materials and catalyst materials. For example, metal terbium targets can be used to manufacture high-performance electronic devices in the electronic semiconductor industry, such as thin film capacitors, integrated circuits, etc. In the coated glass industry, terbium targets can be used to prepare optical films with excellent performance, such as low-radiation coated glass, anti-reflective coated glass, etc. At the same time, in the thin-film solar energy industry, terbium targets are used to prepare solar cell films with high-efficiency photoelectric conversion performance. For example, dysprosium targets can be used to prepare magnetic films and magnetic devices, such as magnetic recording materials, magnetic sensors, magnetic storage, etc. At the same time, dysprosium targets have good chemical stability and corrosion resistance, and can be used to prepare corrosion-resistant coatings for use in aerospace, chemical equipment, marine engineering and other fields.

[0003] Metal dysprosium target or metal terbium target is usually obtained by melting, casting, processing, heat treating and other steps of metal dysprosium or metal terbium. However, due to the unique thermophysical properties of metal dysprosium or metal terbium, the prepared target has technical problems such as low density and difficulty in improving purity. Summary of the invention

[0004] In view of the above shortcomings, the present invention discloses a process for preparing a target body using high-purity terbium and dysprosium to produce high-purity metal terbium target and metal dysprosium target, thereby solving the problems of low density and difficulty in improving purity of existing target materials.

[0005] The present invention is achieved by adopting the following technical solutions: A process for preparing a target body using high-purity terbium and dysprosium comprises the following steps: (1) crushing a metal terbium or metal dysprosium ingot and uniformly mixing it with calcium fluoride to obtain a mixed material, wherein the weight ratio of the ingot to calcium fluoride is (99.0-99.2):1; (2) adding the mixed material obtained in step (1) into a vacuum melting furnace for melting, wherein the melting temperature is 800° C. to 1500° C. and the current intensity is 4000A to 12000A; before the melting begins, argon is filled into the vacuum melting furnace, and the pressure of the argon source is maintained at 1 MPa; (3) After smelting, the molten metal is kept at 700°C to 750°C for 1h to 4h and then cooled to obtain a billet. The billet is then pressed and vibrated by a die-casting machine to peel off the surface slag to obtain a high-purity metal terbium or metal dysprosium target body.

[0006] The present invention crushes the ingot of metal terbium or metal dysprosium and mixes it with calcium fluoride to obtain a mixed material, and then places the mixed material in a vacuum melting furnace for melting under suitable conditions such as temperature and current intensity. If the temperature is below 800°C, the rare earth metal is difficult to melt and the impurity elements cannot be removed, and a qualified target material body cannot be obtained; when the temperature exceeds 1500°C, the metal is easy to sublimate and the metal body cannot be collected. After the melting is completed, the slag is removed. During the melting process, impurities such as Al, Fe, Mg, and Mn are mixed with F - The ions combine to form slag with compounds, which floats on the surface of the high-temperature molten metal. After cooling, the slag adheres to the surface of the metal. Therefore, the present invention uses a die-casting machine to press and vibrate the blank so that the surface slag is automatically peeled off and removed, and finally a high-purity metal terbium or metal dysprosium target body is obtained.

[0007] Furthermore, in step (1), the purity of the ingot of metal terbium or metal dysprosium is not less than 99.95%, and the purity of the calcium fluoride is not less than 99.99%.

[0008] Furthermore, in step (1), the particle size of the crushed terbium or dysprosium metal is 10 to 200 mm; the particle size of the calcium fluoride is 5 to 50 mm. By controlling the particle sizes of the terbium or dysprosium metal and calcium fluoride, it is beneficial to mix them evenly and improve the impurity removal effect.

[0009] Furthermore, the smelting time in step (2) is 120 minutes.

[0010] Furthermore, in step (2), before the smelting begins, the mixed material is placed in a vacuum melting furnace at room temperature, the vacuum melting furnace is covered and sealed, and then vacuum is drawn, argon is filled into the vacuum melting furnace for protection, the pressure of the argon source is maintained at 1 MPa, and then the power is turned on to heat the vacuum melting furnace, and the melting temperature is reached after 30 minutes.

[0011] Furthermore, in step (3), the molten metal is kept warm and then cooled at a rate of 15-20°C / min. By controlling the cooling rate, the original slag can be controlled to form surface slag on the surface of the blank, which is beneficial for subsequent stripping and removal.

[0012] Furthermore, in step (2), the concentration of the argon gas is 90%.

[0013] Compared with the prior art, this technical solution has the following beneficial effects: The present invention adopts a vacuum melting method to melt a mixture of metal terbium or metal dysprosium and calcium fluoride under the condition of continuous filling with argon gas, then removes scum from the molten metal and casts it into a mold, keeps it warm at a suitable temperature for a certain period of time, and then cools it to obtain a high-purity metal terbium or metal dysprosium target material body. The method of the present invention has a simple process and is easy to operate. The metal terbium or metal dysprosium is refined by controlling the temperature and current intensity of the vacuum melting furnace, thereby obtaining a high-purity metal terbium or metal dysprosium target material body, and its purity content can reach 99.99%, which solves the problem that the existing target material has low density and is difficult to improve purity. In addition, the process of the present invention is suitable for large-scale and automated production of metal terbium or metal dysprosium targets. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is a flow chart of the method described in Example 3. DETAILED DESCRIPTION

[0015] The present invention is further described by the following examples, but is not intended to be limiting of the present invention. Specific experimental conditions and methods not specified in the following examples are conventional methods commonly known to those skilled in the art.

[0016] Embodiment 1: A process for preparing a target body using high-purity terbium and dysprosium, comprising the following steps: (1) crushing a metal terbium ingot and uniformly mixing it with calcium fluoride to obtain a mixed material, wherein the weight ratio of the ingot to calcium fluoride is 99.1:1; the purity of the metal terbium ingot is 99.952%, and the purity of the calcium fluoride is 99.993%; the particle size of the metal terbium after crushing is 50 mm; and the particle size of the calcium fluoride is 10 mm; (2) adding the mixed material obtained in step (1) into a vacuum melting furnace for melting, the melting temperature is 1000°C, the current intensity is 10000A, before the melting starts, the mixed material is placed in the vacuum melting furnace at room temperature, the vacuum melting furnace is covered and sealed, and then vacuum is drawn, argon is filled into the vacuum melting furnace for protection, the pressure of the argon source is maintained at 1MPa, and then the power is turned on to heat the vacuum melting furnace, and the melting temperature is reached after 30 minutes; the concentration of the argon is 90%; the melting time is 120min; (3) After smelting, the molten metal is kept at 720°C for 3 hours and then cooled at a rate of 16°C / min to obtain a billet. The billet is then vibrated by a die-casting machine to peel off the surface slag to obtain a high-purity terbium metal target body. After testing, the purity of the terbium metal target body is 99.993%.

[0017] Embodiment 2: A process for preparing a target body using high-purity terbium and dysprosium, comprising the following steps: (1) crushing a metal terbium ingot and uniformly mixing it with calcium fluoride to obtain a mixed material, wherein the weight ratio of the ingot to calcium fluoride is 99.0:1; the purity of the metal terbium ingot is 99.955%, and the purity of the calcium fluoride is 99.992%; the particle size of the metal terbium after crushing is 10 mm; and the particle size of the calcium fluoride is 5 mm; (2) adding the mixed material obtained in step (1) into a vacuum melting furnace for melting, the melting temperature is 800°C, the current intensity is 4000A, before the melting starts, the mixed material is placed in the vacuum melting furnace at room temperature, the vacuum melting furnace is covered and sealed, and then vacuum is drawn, argon is filled into the vacuum melting furnace for protection, the pressure of the argon source is maintained at 1MPa, and then the power is turned on to heat the vacuum melting furnace, and the melting temperature is reached after 30 minutes; the concentration of the argon is 90%; the melting time is 120min; (3) After smelting, the molten metal is kept at 700°C for 4 hours and then cooled at a rate of 15°C / min to obtain a billet. The billet is then vibrated by a die-casting machine to peel off the surface slag to obtain a high-purity terbium metal target body. After testing, the purity of the terbium metal target body is 99.991%.

[0018] Embodiment 3: A process for preparing a target body using high-purity terbium and dysprosium, comprising the following steps: (1) crushing a metal dysprosium ingot and uniformly mixing it with calcium fluoride to obtain a mixed material, wherein the weight ratio of the ingot to calcium fluoride is 99.15:1; the purity of the metal dysprosium ingot is 99.951%, and the purity of the calcium fluoride is 99.993%; the particle size of the metal dysprosium after crushing is 100 mm; and the particle size of the calcium fluoride is 30 mm; (2) adding the mixed material obtained in step (1) into a vacuum melting furnace for melting, the melting temperature is 1200°C, the current intensity is 8000A, before the melting starts, the mixed material is placed in the vacuum melting furnace at room temperature, the vacuum melting furnace is covered and sealed, and then vacuum is drawn, argon is filled into the vacuum melting furnace for protection, the pressure of the argon source is maintained at 1MPa, and then the power is turned on to heat the vacuum melting furnace, and the melting temperature is reached after 30 minutes; the concentration of the argon is 90%; the melting time is 120min; (3) After smelting, the molten metal is kept at 740°C for 2 hours and then cooled at a rate of 18°C / min to obtain a billet. The billet is then vibrated by a die-casting machine to peel off the surface slag to obtain a high-purity metal dysprosium target body. After testing, the purity of the metal dysprosium target body is 99.994%.

[0019] Embodiment 4: A process for preparing a target body using high-purity terbium and dysprosium, comprising the following steps: (1) crushing a metal dysprosium ingot and uniformly mixing it with calcium fluoride to obtain a mixed material, wherein the weight ratio of the ingot to calcium fluoride is 99.2:1; the purity of the metal dysprosium ingot is 99.951%, and the purity of the calcium fluoride is 99.991%; the particle size of the metal dysprosium after crushing is 200 mm; and the particle size of the calcium fluoride is 50 mm; (2) adding the mixed material obtained in step (1) into a vacuum melting furnace for melting, the melting temperature is 1500°C, the current intensity is 12000A, before the melting starts, the mixed material is placed in the vacuum melting furnace at room temperature, the vacuum melting furnace is covered and sealed, and then vacuum is drawn, argon is filled into the vacuum melting furnace for protection, the pressure of the argon source is maintained at 1MPa, and then the power is turned on to heat the vacuum melting furnace, and the melting temperature is reached after 30 minutes; the concentration of the argon is 90%; the melting time is 120min; (3) After smelting, the molten metal is kept at 750°C for 1 hour and then cooled at a rate of 20°C / min to obtain a billet. The billet is then vibrated by a die-casting machine to peel off the surface slag to obtain a high-purity metal dysprosium target body. After testing, the purity of the metal dysprosium target body is 99.992%.

[0020] Experimental Example 1: A terbium metal target body was prepared according to the method described in Example 1, wherein in step (3), different cooling speeds were used to reduce the temperature, and the purity of the obtained terbium metal target body was tested. The specific results are shown in Table 1.

[0021] Table 1 Purity test results of terbium metal target body materials obtained at different cooling rates

[0022] It can be seen from the above data that a slow cooling rate can still form intact surface slag on the metal surface. Accelerating the cooling rate can improve the process efficiency. However, too fast a cooling rate (over 20°C / min) will affect the formation of surface slag, causing part of the slag to adhere to the surface of the metal terbium and be unable to be stripped off, thereby reducing the purity of the metal terbium target.

[0023] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A process for preparing a target body using high-purity terbium and dysprosium, characterized in that: The following steps are involved: (1) crushing a metal terbium or metal dysprosium ingot and uniformly mixing it with calcium fluoride to obtain a mixed material, wherein the weight ratio of the ingot to calcium fluoride is (99.0-99.2):1; (2) adding the mixed material obtained in step (1) into a vacuum melting furnace for melting, wherein the melting temperature is 800° C. to 1500° C. and the current intensity is 4000A to 12000A; before the melting begins, argon is filled into the vacuum melting furnace, and the pressure of the argon source is maintained at 1 MPa; (3) After smelting, the molten metal is kept at 700°C to 750°C for 1h to 4h and then cooled to obtain a billet. The billet is then pressed and vibrated by a die-casting machine to peel off the surface slag to obtain a high-purity metal terbium or metal dysprosium target body.

2. The process for preparing a target body using high-purity terbium and dysprosium according to claim 1, characterized in that: In step (1), the purity of the ingot of metal terbium or metal dysprosium is not less than 99.95%, and the purity of the calcium fluoride is not less than 99.99%.

3. The process for preparing a target body using high-purity terbium and dysprosium according to claim 1, characterized in that: In step (1), the particle size of the crushed metal terbium or metal dysprosium is 10 to 200 mm; and the particle size of the calcium fluoride is 5 to 50 mm.

4. The process for preparing a target body using high-purity terbium and dysprosium according to claim 1, characterized in that: The smelting time in step (2) is 120 minutes.

5. The process for preparing a target body using high-purity terbium and dysprosium according to claim 1, characterized in that: In step (2), before the smelting begins, the mixed material is placed in a vacuum melting furnace at room temperature, the vacuum melting furnace is covered and sealed, and then vacuum is drawn. Argon gas is filled into the vacuum melting furnace for protection, and the pressure of the argon gas source is maintained at 1 MPa. Then, the power is turned on to heat the vacuum melting furnace, and the melting temperature is reached after 30 minutes.

6. The process for preparing a target body using high-purity terbium and dysprosium according to claim 1, characterized in that: In step (3), the molten metal is kept warm and then cooled at a rate of 15 to 20°C / min.

7. The process for preparing a target body using high-purity terbium and dysprosium according to claim 1, characterized in that: In step (2), the concentration of the argon gas is 90%.

Citation Information

Patent Citations

  • Preparation method of rare earth metal Tb and Dy employing electro-deoxidization

    CN101629307A

  • Manufacturing method of dysprosium / terbium target

    CN112725675A

  • Preparation method of terbium target blank

    CN113846298A

  • Preparation method of terbium-iron alloy

    CN114703387A

  • Preparation method of metal scandium rare earth target material

    CN115747731A

Cited By

  • Preparation method of high-purity compact dysprosium cast ingot

    CN120885661A