Chemical gold palladium gold manufacturing process of circuit board
Through the nickel-free chemical gold-palladium process, through degreasing, micro-etching, pickling and multi-layer gold layer formation, the problems of high-frequency line signal loss and weakened bonding force in the existing technology are solved, and an environmentally friendly and economical High-frequency circuit production enhances the anti-friction and welding performance of the circuit.
Patent Information
- Application Number
- CN202410315115.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing circuit board surface treatment processes, such as electroless nickel gold, electroless nickel palladium gold, and chemical thin nickel palladium gold, cannot meet the needs of high-frequency communication 5G/6G and fine lines, and the cost is high, and there are line signal losses and bonding strength. issues such as weakening and void risk.
Using a nickel-free chemical gold-palladium production process, through the steps of degreasing, micro-etching, pickling, chemical gold, chemical palladium and chemical gold again, two gold layers are formed to improve the hardness and bonding strength of the circuit. Reduce signal loss, and generate palladium and gold layers through environmentally friendly reactions to prevent voids and poor contacts.
It achieves cost reduction, improves the anti-friction performance and bonding force of high-frequency lines, reduces signal loss, enhances welding performance, and avoids the problems of line voids and weakened bonding force. The process is environmentally friendly and can recycle micro-etching liquid and pickling liquid.
Smart Images

Figure CN118756124A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of circuit board manufacturing, in particular to a chemical gold-palladium manufacturing process for a circuit board. Background Art
[0002] With the development of the electronics industry, especially high-frequency communication 5G / 6G and the upgrading of artificial intelligence, the existing circuit board surface treatments commonly used in chemical nickel-gold (ENIG), chemical nickel-palladium-gold (ENEPIG), chemical thin nickel-palladium-gold (Thin Ni ENEPIG) and chemical palladium-gold (EPIG) can no longer meet product requirements. Therefore, an alternative process for surface treatment suitable for high-frequency communication 5G / 6G and fine lines is needed.
[0003] Among them, the chemical nickel-gold (ENIG) process will cause insoluble particles in the Ni plating solution, which will cause the nickel surface to passivate. The exposure time and water washing time after nickel deposition are too long, and the passivation of the nickel surface will weaken the bonding with the circuit board. The chemical nickel-palladium-gold (ENEPIG) can meet the functions of welding and gold wire at the same time, but it cannot meet the production requirements of finer lines. When the produced lines are finer, it will lead to poor lines, and when the nickel thickness exceeds 5um, the signal loss of the line will increase sharply. The chemical thin nickel-palladium-gold (Thin Ni ENEPIG) process also has the same technical problems; in addition, the chemical palladium-gold (EPIG) production process can produce fine lines, but the copper layer lines are prone to voids and internal gaps, and the risk of defects is high.
[0004] There is also a relatively good chemical palladium gold process on the market, namely direct induction gold (DIG). This process removes nickel and can produce fine circuits and high-frequency products, but the cost is extremely high.
[0005] In view of the above technical problems, it is urgent to propose a palladium production process that can reduce costs and process fine and high-frequency circuits. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the deficiencies in the prior art, the present invention provides a chemical gold-palladium manufacturing process for a circuit board.
[0008] (II) Technical solution
[0009] In order to realize the chemical gold-palladium manufacturing process of the above circuit board, the process of the present invention comprises the following steps:
[0010] S1: Degreasing, micro-etching and pickling. Put the circuit board containing the copper layer into the degreasing agent for degreasing. Put the degreasing circuit board into the micro-etching liquid for micro-etching to roughen the copper surface and keep it fresh. Put the roughened circuit board into the pickling liquid for pickling to remove the oxide on the copper surface and keep the copper surface fresh.
[0011] S2: Chemical gold, placing the circuit board after step S1 into a gold bath solution to restore the gold layer on the copper surface;
[0012] S3: Chemical palladium: placing the circuit board with the gold layer into a palladium bath solution to reduce the palladium layer on the surface of the gold layer;
[0013] S4: Chemical gold, placing the circuit board with a palladium layer into a gold bath solution, and reducing a gold layer on the palladium layer.
[0014] In this process, firstly, the entire production process does not use nickel-containing processes, and nickel elements will not appear in the chemical electroplating solution. After production, there will be no weakening of the circuit bonding force caused by nickel passivation on the copper surface. In addition, since nickel is not used, the loss of the entire circuit can be reduced in the process of making finer circuits, which is conducive to the production of high-frequency circuits. Finally, compared with the chemical palladium-gold production method, since the palladium layer is restored between the two gold layers, the palladium layer itself has a stronger hardness than the gold layer. On the one hand, it can improve the anti-friction and deformation performance of the circuit. On the other hand, it can improve the bonding strength of the gold layer in contact with the copper surface and prevent the gold layer from having voids and poor contact.
[0015] In this process, the micro-etching solution is a sodium persulfate aqueous solution. After micro-etching, the micro-etching solution will not contain other particles and impurities except that the concentration of the acid solution is reduced. The copper on the copper surface reacts with copper oxide to form copper sulfate soluble in water. For the micro-etching solution, only sodium persulfate and / or sodium sulfate need to be added. Under the condition of controlling the concentration of the acid solution in the micro-etching solution, it can be recycled for multiple times.
[0016] In the pickling solution, only sulfuric acid is needed to react with copper oxide to generate water-soluble copper sulfate and water. Since the reaction between sulfuric acid and copper oxide in the micro-etching solution is the same as that in the pickling solution, even during the pickling process, the copper surface can still be placed in the micro-etching solution for pickling, and there is no need to prepare a separate pickling solution.
[0017] In the two chemical gold steps of step S2 and step S4, the chemical gold adopts an ion replacement reduction reaction, the gold particles are replaced by gold atoms and attached to the copper surface or the palladium layer, the gold bath solution will not form other impurity ions, and the reduction reaction adopted in the two steps is the same, and it can be put into the gold bath solution in step S2 again after completing step S3, which can save the production process and improve the work efficiency. In addition, the gold layer can also prevent oxidation and improve the welding performance.
[0018] In step S3, the chemical target reacts to generate palladium and phosphorus, wherein the palladium is attached to the gold layer and the phosphorus is precipitated in the liquid. In addition, hydrogen and alkali ions are generated. The entire reaction process is an environmentally friendly reaction and does not produce corrosion or heavy metal ions. After the palladium bath solution has been reducing palladium for a period of time, it is only necessary to add palladium ions to the solution and adjust the pH. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a flow chart of the process of the present invention;
[0020] Figure 2 A comparison diagram of signal loss between a circuit board manufactured by the process of the present invention and a circuit board of the prior art;
[0021] Figure 3 It is a microscopic comparison diagram of a circuit board made by the process of the present invention and a circuit board made by the prior art. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] See also Figure 1 The circuit board chemical gold-palladium production process disclosed in the present invention comprises the following steps:
[0024] S1: Degreasing, micro-etching and pickling. Put the circuit board containing the copper layer into the degreasing agent for degreasing. Put the degreased circuit board into the micro-etching liquid for micro-etching to roughen the copper surface and keep it fresh. Put the roughened circuit board into the pickling liquid for pickling to remove the oxide on the copper surface and keep the copper surface fresh.
[0025] In this step, the preliminary treatment of the copper layer by degreasing, micro-etching and pickling is aimed at removing the oil stains and copper oxide on the surface of the copper layer, ensuring that the exposed copper surface is the new inner copper, and making the copper surface have a greater roughness. In this case, when gold plating or reducing the gold layer on the copper surface, the bonding degree of the gold layer and the copper surface can be guaranteed, and the conductive properties of the copper surface and the gold layer can be improved, the resistance can be reduced, and the loss to the high-frequency line can be reduced.
[0026] In this step, the micro-etching solution is sodium persulfate or potassium hydrogen persulfate aqueous solution; the micro-etching solution is sodium persulfate aqueous solution, and the micro-etching time is not less than 1 minute, wherein sodium persulfate reacts with water to generate hydrogen peroxide, sulfuric acid and sodium sulfate that is easily soluble in water, hydrogen peroxide oxidizes the copper surface to form copper oxide, and copper oxide reacts with sulfuric acid to produce copper sulfate that is easily soluble in water, thereby removing part of the copper and copper oxide on the copper surface to ensure the freshness of the copper surface. The reaction formula is as follows:
[0027] 2NaSO4+H2O→Na2SO4+H2SO5
[0028] H2SO5+H2O→H2SO4+H2O2
[0029] H2O2+Cu→CuO+2H2O
[0030] CuO+H2SO4→CuSO4+H2O
[0031] Furthermore, the pickling solution is a diluted sulfuric acid solution, and the pickling solution is used to remove a small amount of copper oxide on the surface of the copper layer that is easily oxidized, and produce copper sulfate that is easily soluble in water.
[0032] Among them, the micro-etching time of not less than 1 minute can effectively improve the roughness of the copper surface after micro-etching, and its roughness can meet the minimum requirement of the bonding degree between the gold layer and the copper surface.
[0033] In addition, the micro-etching solution is an aqueous solution of sodium persulfate. After micro-etching, no other particles or impurities will appear in the micro-etching solution except that the concentration of the acid solution is reduced. The copper on the copper surface reacts with copper oxide to form copper sulfate soluble in water. For the micro-etching solution, only sodium persulfate and / or sodium sulfate need to be added. Under the condition of controlling the concentration of the acid solution in the micro-etching solution, it can be recycled for multiple times.
[0034] In the pickling solution, only sulfuric acid is needed to react with copper oxide to generate water-soluble copper sulfate and water. Since the reaction between sulfuric acid and copper oxide in the micro-etching solution is the same as that in the pickling solution, even during the pickling process, the copper surface can still be placed in the micro-etching solution for pickling, and there is no need to prepare a separate pickling solution.
[0035] The present invention also includes step S2: chemical gold, placing the circuit board after step S1 into a gold bath solution to restore the gold layer on the copper surface.
[0036] The chemical gold reduction reaction formula is:
[0037] Au + +R→Au+R -
[0038] In the reduction reaction, the gold cations gain electrons, are reduced to gold atoms, and are attached to the palladium layer or the copper surface to form the gold layer, wherein R refers to elemental ions that are prone to lose electrons relative to the gold cations.
[0039] After completing step S2, it is necessary to complete step S3 and step S4 in sequence.
[0040] Among them, step S3: chemical palladium, putting the circuit board with the gold layer into a palladium bath solution, and reducing the palladium layer on the surface of the gold layer.
[0041] In this step, the palladium bath solution is an aqueous solution of palladium ions and phosphate ions, wherein the chemical palladium reaction process is as follows:
[0042] Main reaction:
[0043] Pd 2+ +H2PO2 - +H2O→Pd+H2PO3 - +2H +
[0044] Side reaction:
[0045] H2O+H2PO2 - →H2+H2PO3 -
[0046] 4H2PO2 - →2P+2H2PO3 - +2OH - +H2
[0047] Step S4: chemical gold, placing the circuit board with the palladium layer into a gold bath solution, reducing a gold layer on the palladium layer, and the gold layer can prevent oxidation and improve welding performance.
[0048] The circuit board in S2 is placed in the gold bath solution for no less than 4 minutes, and the reduced gold layer is no less than 0.01um thick. The circuit board in S4 is placed in the gold bath solution for no less than 9 minutes, and the reduced gold layer is no less than 0.04um thick.
[0049] The thickness of the gold layer reduced in S2 is smaller than that in S4 in order to improve the conductive properties of the gold layer and the copper surface in S2, while the thickness of the gold layer in S4 is thicker in order to improve the friction resistance and circuit strength of the circuit surface.
[0050] Among them, the time requirements of not less than 4 minutes and not less than 9 minutes are to complete the requirements of reducing the gold layer of corresponding thickness. Only when the reduction reaction meets the corresponding time requirements can the thickness of the gold layer in contact with the copper surface and the gold layer in contact with the palladium layer reach 0.01um and 0.04um or more respectively.
[0051] In this process, firstly, the whole production process does not use nickel-containing processes, and nickel elements will not appear in the chemical electroplating solution. After production, there will be no weakening of the circuit bonding force caused by nickel passivation on the copper surface. In addition, since nickel is not used, the loss of the entire circuit can be reduced in the process of making finer circuits, which is conducive to the production of high-frequency circuits. Finally, compared with the chemical palladium-gold production method, since the palladium layer is restored between the two gold layers, the palladium layer itself has a stronger hardness than the gold layer. On the one hand, it can improve the anti-friction and deformation performance of the circuit. On the other hand, it can improve the bonding strength of the gold layer in contact with the copper surface, and prevent the gold layer from having voids, poor contact, etc. In addition, the gold layer can also prevent oxidation and improve welding performance.
[0052] Finally, the applicant manufactured a circuit board according to the process described in the specification, and conducted a comparative analysis of the signal loss of the circuit board using a PNA network analyzer, and compared and observed the microstructure with the prior art.
[0053] like Figure 2 , Figure 2 It is a comparison diagram of signal loss between a circuit board made by the process of the present invention and a circuit board of the prior art.
[0054] As can be seen from the figure, the signal loss ratio of the circuit boards made by the corresponding process is in the following order from large to small: electroless nickel immersion gold ENIG> nickel palladium gold ENEPIG> chemical tin Im-Tin> chemical palladium nickel palladium gold Thin NiENEPIG> chemical gold palladium gold IGEPIG, among which chemical gold palladium has the smallest signal loss.
[0055] like Figure 3 , is a microscopic comparison diagram of a circuit board made by the process of the present invention and a circuit board made by the prior art.
[0056] from Figure 3 The characteristics can be seen in the following table.
[0057]
[0058] It should be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0059] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
Claims
1. A process for producing chemical gold-palladium gold for a circuit board, characterized in that: The process comprises the following steps in sequence: S1: Degreasing, micro-etching and pickling. Put the circuit board containing the copper layer into the degreasing agent for degreasing. Put the degreasing circuit board into the micro-etching liquid for micro-etching to roughen the copper surface and keep it fresh. Put the roughened circuit board into the pickling liquid for pickling to remove the oxide on the copper surface and keep the copper surface fresh. S2: Chemical gold, placing the circuit board after step S1 into a gold bath solution to restore the gold layer on the copper surface; S3: Chemical palladium: placing the circuit board with the gold layer into a palladium bath solution to reduce the palladium layer on the surface of the gold layer; S4: Chemical gold, placing the circuit board with a palladium layer into a gold bath solution, and reducing a gold layer on the palladium layer.
2. The chemical gold-palladium gold manufacturing process for a circuit board as claimed in claim 1, characterized in that: The micro-etching solution is a sodium persulfate or potassium hydrogen persulfate aqueous solution.
3. The chemical gold-palladium manufacturing process for a circuit board as claimed in claim 2, characterized in that: The micro-etching solution is a sodium persulfate aqueous solution, and the micro-etching time is not less than 1 minute. The sodium persulfate reacts with water to generate hydrogen peroxide, sulfuric acid and sodium sulfate that is easily soluble in water. The hydrogen peroxide oxidizes the copper surface to form copper oxide, and the copper oxide reacts with sulfuric acid to produce copper sulfate that is easily soluble in water, thereby removing part of the copper and copper oxide on the copper surface to ensure the freshness of the copper surface. The reaction formula is as follows: 2NaSO4+H2O→Na2SO4+H2SO5 H2SO5+H2O→H2SO4+H2O2 H2O2+Cu→CuO+2H2O CuO+H2SO4→CuSO4+H2O 4. The chemical gold-palladium gold manufacturing process for a circuit board as claimed in claim 1, characterized in that: The pickling solution is a diluted sulfuric acid solution, and the pickling solution is used to remove a small amount of copper oxide that is easily oxidized on the surface of the copper layer to produce copper sulfate that is easily soluble in water.
5. The chemical gold-palladium gold manufacturing process for a circuit board as claimed in claim 1, characterized in that: The circuit board described in S2 is placed in the gold bath solution for no less than 4 minutes, and the thickness of the reduced gold layer is no less than 0.01 um.
6. The chemical gold-palladium gold manufacturing process for a circuit board as claimed in claim 5, characterized in that: The circuit board described in S4 is placed in the gold bath solution for not less than 9 minutes, and the thickness of the reduced gold layer is not less than 0.04 um.
7. The process for producing chemical gold-palladium gold for a circuit board as claimed in claim 1, characterized in that: The chemical gold reduction reaction formula is: At + +R→Au+R - The gold cations gain electrons in the reduction reaction, are reduced to gold atoms, and are attached to the palladium layer or the copper surface to form the gold layer, wherein R refers to element ions that are prone to lose electrons relative to the gold cations.
8. The process for producing chemical gold-palladium gold for a circuit board as claimed in claim 1, characterized in that: The palladium tank solution in S3 is an aqueous solution of palladium ions and phosphate ions, wherein the chemical palladium reaction process is as follows: Main reaction: <h2 style=";text-align:left;direction:ltr">Pd<h2 style=";text-align:left;direction:ltr"> 2+ <h2 style=";text-align:left;direction:ltr"> +H2PO2-+H2O→Pd+H2PO3-+2H<h2 style=";text-align:left;direction:ltr"> + Side reaction: H2O+H2PO2-→H2+H2PO3- 4H2PO2-→2P+2H2PO3-+2OH - +H2。
Citation Information
Patent Citations
Chemical palladium solution applied to PCB chemical gold palladium clad layer
CN110318047A
Substrate and method for producing the same