Preparation method of MQDs coordinated beta-Co (OH) 2 cobalt hydroxide nanosheet

Through the electrochemical reconstruction method, the interaction between MQDs and β-Co(OH)2 is used to prevent the reduction of cobalt hydroxide and form a nanosheet structure, which solves the problem of the activity of β-Co(OH)2 under alkaline conditions. and stability issues, achieving efficient electrocatalytic hydrogen evolution effect.

CN118756207APending Publication Date: 2024-10-11JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410774209.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

β-Co(OH)2 cobalt hydroxide is easily reduced completely under alkaline conditions, resulting in poor activity in the electrocatalytic hydrogen evolution reaction, and its crystal structure is unstable, which affects the long-term use effect of the catalyst.

Method used

Through the electrochemical reconstruction method, small molecule MQDs interact with β-Co(OH)2, and electrons are enriched at the end of MQDs, preventing the reduction of β-Co(OH)2 and forming MQDs-coordinated cobalt hydroxide nanoparticles. tablets, which enhances its alkaline hydrogen evolution activity and stability.

Benefits of technology

Significantly improves the alkaline hydrogen evolution efficiency and stability of the catalyst. Compared with non-noble metal/Co(OH)2 heterostructure catalysts, it shows better electrocatalytic activity and long-term performance. The synthesis process is simple, reducing time costs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756207A_ABST
    Figure CN118756207A_ABST
Patent Text Reader

Abstract

The cobalt hydroxide nanosheet coordinated with small molecules MQDs is rapidly obtained through one-step electrochemical reconstruction, electrons are enriched at the ends of the MQDs through interaction between the cobalt hydroxide nanosheet and the small molecules MQDs, reduction of beta cobalt hydroxide is prevented, and therefore the enhanced HER activity is obtained. Compared with a non-noble metal / Co (OH) 2 heterostructure catalyst reported at present, the catalytic efficiency and stability of alkaline hydrogen evolution of the MQDs coordinated cobalt hydroxide nanosheet are remarkably improved, the synthesis process is simple, and the time cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a high-performance catalyst, in particular to a MQDs-coordinated β-Co(OH) 2 A method for preparing cobalt hydroxide nanosheets. Background Art

[0002] Ti 2 C MXene quantum dots are a new type of zero-dimensional semiconductor nanomaterials derived from two-dimensional layered Ti 2 CMXene. MXene is derived from the bulk material MAX, where MAX is a layered ternary transition metal carbide, nitride or carbonitride, and its general formula is M n+1 AX n (M is an early transition metal such as Ti, Mo, V, etc., A is a main group III or IV element such as Al, Ga, etc., X is C and / or N, and n is 1, 2, 3), the layered structure is composed of hexagonally closely packed M n+1 X n The A layer and the A layer are overlapped by metallic bonds and van der Waals forces.

[0003] β-Cobalt hydroxide hydrogen evolution electrocatalyst: Electrolysis of water to produce hydrogen is a green and efficient way. The external power source drives the reduction reaction of hydrogen ions at the cathode. However, the efficient hydrogen evolution process is limited by the decomposition kinetics of water molecules and the adsorption and desorption kinetics of hydrogen ions under alkaline conditions. It is necessary to overcome a large reaction energy barrier to achieve this process. Cobalt hydroxide, as a transition metal-based catalyst (iron hydroxide, nickel hydroxide, etc.), has the advantages of high abundance, simple preparation, good electrochemical stability, etc. However, the material has poor conductivity and its surface is conducive to OH - , but not conducive to the adsorption of H + Secondly, according to the Bourbaix diagram (potential-PH diagram) of Co, Co(OH) 2 Under alkaline conditions, it is easily reduced to metallic cobalt, which has a strong bonding ability with H and is not easy to desorb to form hydrogen, resulting in poor electrocatalytic hydrogen evolution behavior.

[0004] The consumption of primary energy sources such as coal, oil, and natural gas has led to an increasing demand for the production of clean, efficient, and low-cost secondary energy. Hydrogen, with its high combustion calorific value, light weight, easy transportation, and pollution-free characteristics, has attracted widespread attention. Therefore, most scientific researchers have focused their efforts on finding more efficient methods for producing hydrogen. The methods for producing hydrogen that have emerged so far include electrocatalytic hydrogen production, photocatalytic hydrogen production, and photoelectrocatalytic hydrogen production. Among them, electrocatalytic hydrogen production is the simplest method, which directly uses an external power source; the latter two require an external light source and the equipment is relatively complex. In the electrocatalytic process, the energy barrier for decomposing water is high due to the need to consume the electrical energy of the external power source, so a catalyst is needed to reduce energy consumption. Precious metal Pt-based materials are often used as electrocatalytic hydrogen production catalysts, but their high cost and low reserves limit their application. The development of low-cost, efficient, and sustainable electrocatalysts has received increasing attention. Among them, transition metal-based catalysts have a d-band electronic structure similar to that of permetallics and are expected to become good candidates for electrocatalytic hydrogen evolution catalysts.

[0005] As a transition metal-based catalyst, cobalt hydroxide has attracted attention due to its large storage capacity, low reaction kinetic overpotential and good electrochemical stability. It is often used in oxygen evolution reaction. This is due to its metal site for OH - adsorption and activation.

[0006] Cobalt hydroxide materials include a-Co(OH)2 and β-Co(OH)2, among which β-Co(OH)2 has a brucite structure, with hydroxyl ions tightly packed hexagonally, and cations filling all the octahedral gaps between every two adjacent layers of hydroxyl ions; forming a structural layer of coordinated octahedron. The structural layers are ionic bonds, and the structural layers are connected by phases. Compared with a-Co(OH)2, β-Co(OH)2 has higher specific capacity and conductivity, so it has a wide range of applications in the field of electrochemistry. β-Co(OH)2 can be used to prepare electrochemical energy storage devices such as catalysts, supercapacitors, fuel cells and lithium-ion batteries.

[0007] However, there is no anion intercalation between the β-phase cobalt hydroxide layers, resulting in Co 2+ In the voltage range of the hydrogen evolution reaction, it is directly reduced to metallic cobalt, and the strong bond between metallic cobalt and H atoms is not conducive to its desorption process, resulting in poor alkaline HER activity. For example, during the constant voltage stability test of alkaline hydrogen evolution, it is obvious that the catalyst shows a gradual decrease in current, indicating that the catalyst is not stable. Summary of the invention

[0008] In order to inhibit β-Co(OH) 2The cobalt hydroxide is completely reduced within the alkaline hydrogen evolution voltage range, thereby maintaining the stability of the crystal structure. The present invention quickly obtains small molecule MQDs-coordinated cobalt hydroxide nanosheets through a one-step electrochemical reconstruction, and the electrons are enriched at the MQDs end through the interaction between the two, preventing the reduction of β-cobalt hydroxide, thereby obtaining enhanced HER activity. Compared with the currently reported non-precious metal / Co(OH)2 heterostructure catalysts, the MQDs-coordinated cobalt hydroxide nanosheets of the present invention have significant improvements in the catalytic efficiency and stability of alkaline hydrogen evolution, and the synthesis process is simple, reducing the time cost.

[0009] The present invention adopts the following technical solution: a MQDs-coordinated β-Co(OH) 2 A method for preparing cobalt hydroxide nanosheets, the method comprising:

[0010] Titanium carbide (Ti 2 CT x )MXene multilayer nanosheets were added to an aqueous solution with a mass fraction of HCl, stirred for reaction under an argon atmosphere, and then filtered through a 0.22um filter membrane to collect the filtrate to obtain Ti 2 CT x MQDs solution;

[0011] Ti supported on a cobalt substrate 2 CT x MQDs, and as the cathode of the three-electrode system, undergo electrochemical reaction in KOH solution to obtain Ti loaded on the surface of the cobalt matrix. 2 CT x MQDs / β-Co(OH) 2 Nanosheet catalysts.

[0012] In the present invention, the catalyst composition before electrochemical reconstruction is MQDs / Co 2 (OH) 3 Cl / Co foam, MQDs surface has negatively charged functional groups, Co 2 (OH) 3 The Cl surface has a positive charge, and the two form a heterostructure through electrostatic self-assembly. Then, during the electrochemical activation process, the -OH in the alkaline electrolyte replaces the Co on the surface of the cobalt foam. 2 (OH) 3 Cl in Cl - , generating β-Co(OH) 2 At the same time, MQDs were reassembled onto the surface of cobalt hydroxide to form MQDs / β-Co(OH) 2 / Co foam provides good electrocatalytic activity.

[0013] Furthermore, the mass fraction of the aqueous solution of HCl is 8%, and the stirring reaction time is 72 hours.

[0014] Furthermore, the cobalt substrate is a porous foamed cobalt; the loading method is: immersing the porous foamed cobalt in Ti 2 CT x MQDs solution.

[0015] Furthermore, the soaking time is 2-15 hours.

[0016] Furthermore, the electrolyte was 1M KOH solution and the current density was -10mA / cm 2 .

[0017] Furthermore, titanium carbide (Ti 2 CT x )MXene multilayer nanosheets were prepared by the following method: 2 AlC is the bulk material, and HCl and lithium fluoride are used as etchants to etch Ti 2 AlC was etched and cleaned to obtain a two-dimensional layered Ti 2 CT x MXene.

[0018] In certain embodiments of the present invention, the following steps are taken:

[0019] (1) Ti 2 CT x Preparation of MXene: 30 ml of 6M HCl was added to a polytetrafluoroethylene beaker, and 1.4 g of LiF was added to the above solution. Stir for 30 min, and then 1 g of Ti was weighed. 2 The AlC sample was slowly added to the above solution and stirred for 30 hours. After that, it was repeatedly washed with deionized water and centrifuged at 8000 rpm for 5 minutes until the upper solution was neutral. The lower precipitate was collected and freeze-dried to obtain a two-dimensional layered Ti 2 CT x MXene.

[0020] (2) Preparation of Ti 2 CT x MQDs: Prepare 8% HCl and add 200 mg Ti 2 CT x , stirred for 72 h under argon atmosphere, and then filtered through a 0.22 um filter membrane to collect the filtrate with an average size of 3.64 nm and a concentration of 2.5 mg / ml Ti 2 CT x MQDs solution (such as Figure 1 ).

[0021] (3) Preparation of Ti 2 CT x MQDs / Co 2 (OH) 3 Cl / Co foam integrated electrode: Cut 1*2cm cobalt foam into pieces, wash them in acetone and ethanol for 10min, and dry them in vacuum at 60℃. 2 CT x MQDs solution, soak the dried cobalt foam into Ti 2 CT x The immersion time in the MQDs solution was controlled to be 2 h to 15 h. Afterwards, the solution was dried under vacuum at 60 °C to obtain a series of pre-catalyst Ti 2 CT x MQDs / Co 2 (OH) 3 In this step, since the MQDs solution obtained in step 2 is acidic, if the time is too long, the foamed cobalt will be corroded, causing the catalyst to become brittle and difficult to operate; on the other hand, too much MQDs loading will affect the Co 2 (OH) 3 The release of Cl from the lattice of Cl affects the formation of β-cobalt hydroxide, thus affecting the catalytic activity; too short a time will affect Co 2 (OH) 3 The Cl and MQDs loading is too small, and the active phase is too little, which affects the catalytic activity.

[0022] (4) Electrochemical reconstruction of Ti 2 CT x MQDs / β-Co(OH) 2 / Co foam electrocatalyst: The integrated electrode prepared in step (3) was used as the cathode of the three-electrode system, the graphite rod was used as the counter electrode, and the saturated calomel electrode was used as the reference electrode. 2 The reaction was carried out for 3 h at a current density of 2 (OH) 3 The lattice -Cl in Cl is replaced by -OH in KOH to form β-Co(OH) 2 Nanosheets, finally Ti loaded on the surface of cobalt foam 2 CT x MQDs / β-Co(OH) 2 Nanosheet catalyst (Ti 2 CT x MQDs / β-Co(OH) 2 / Co foam). In this step, the applied current density cannot be too small, otherwise it will prolong the generation time of β-cobalt hydroxide, resulting in too high a time cost; the applied current density cannot be too large, and can be selected in the range of -10 to -50 mA cm-2. If it is too large, it will cause too many hydrogen bubbles to be generated on the catalyst surface, affecting the mechanical stability of the generated catalyst.

[0023] The beneficial effects of the present invention are as follows: the present invention utilizes the electron transfer between MQDs and cobalt hydroxide to enrich the electrons at the MQDs end, thereby inhibiting the reduction of divalent cobalt, and the catalyst exhibits a significant optimization of the alkaline electrocatalytic hydrogen evolution activity of cobalt hydroxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It's Ti 2 CT x The TEM image of MQDs shows that the average size of MQDs is 3.64 nm.

[0025] Figure 2 Add Ti 2 CT x SEM images of MQDs before and after electrochemical activation for 3h. 2 CT x MQDs / Co 2 (OH) 3 SEM image of the original Cl / Co foam catalyst before electrochemical reaction; Figure b is the SEM image of Ti 2 CT x MQDs / Co 2 (OH) 3 SEM image of Cl / Co foam after 3h of electrochemical reaction. The nanosheet morphology can be seen in the image, and the phase is Ti 2 CT x MQDs / β-Co(OH) 2 / Co foam. Figure c is Co 2 (OH) 3 SEM image of the original Cl / Co foam catalyst before electrochemical reaction; Figure d is the SEM image of Co 2 (OH) 3 SEM image of Cl / Co foam after 3 hours of electrochemical reaction. No nanosheet morphology is seen in the image.

[0026] Figure 3 Ti 2 CT x MQDs / Co 2 (OH) 3 Voltage-time diagram of Cl / Co foam catalyst after electrochemical activation for 3 h.

[0027] Figure 4 Ti 2 CT x MQDs / Co 2 (OH) 3 SEM and EDS element distribution diagrams of Cl / Co foam after electrochemical activation for 3 hours, where Figure a shows Ti with obvious nanosheet morphology on the surface 2 CT x MQDs / β-Co(OH) 2 Figure a is the SEM image of the / Co foam catalyst, Figure b is the corresponding element distribution map, and Figures c and g are the EDS images of the uniformly distributed Ti, Co, Cl, C, and O elements, respectively.

[0028] Figure 5 This is the performance diagram of alkaline hydrogen evolution.

[0029] Figure 6 Ti 2 CT x MQDs / β-Co(OH) 2 / Linear voltammetric scan of Co foam-9h;

[0030] Figure 7 Ti 2 CT x MQDs / Co 2 (OH) 3 Cl / Co foam-9h and comparative sample Co 2 (OH) 3 Constant current stability test chart of Cl / Co foam. DETAILED DESCRIPTION

[0031] The following examples are used to further illustrate the present invention, and their purpose is to illustrate the present invention and should not be construed as limiting the scope of the present invention. Unless otherwise specified, all parts by weight and weight percentages are used below.

[0032] The raw materials used in the present invention, unless otherwise specified, are conventional commercially available products; the methods used in the present invention, unless otherwise specified, are conventional methods in the art.

[0033] Example 1: Ti 2 CT x Preparation of MQDs solution

[0034] (1) Take 30 ml of 6 mol / L HCl aqueous solution, add 1.4 g of LiF, stir for 30 min, then add 1 g of Ti at a rate of 1 g / 10 mins. 2AlC, stirred for 30 h; then washed repeatedly with deionized water, centrifuged at 8000 rpm for 5 min until the upper solution was neutral, and the lower precipitate was collected and freeze-dried to obtain a two-dimensional layered Ti 2 CT x MXene.

[0035] (2) Take 60 ml of 8% HCl aqueous solution and add 200 mg Ti 2 CT x MXene was stirred for 72 h under argon atmosphere, and then filtered through a 0.22 μm filter membrane to collect the filtrate to obtain a concentration of 2.5 mg / ml Ti 2 CT x MQDs solution. Figure 1 As shown, the average size is 3.64 nm.

[0036] Example 2

[0037] A Ti 2 CT x MQDs / β-Co(OH) 2 The preparation method of Co foam comprises the following steps:

[0038] S1. Preparation of Ti 2 CT x MQDs / Co 2 (OH) 3 Cl / Co foam integrated electrode:

[0039] S1.1. Wash the cobalt foam with a size of 1*2 cm and a thickness of 1.5 mm in acetone for 10 min, then in ethanol for 10 min, and dry in vacuum at 60°C;

[0040] S1.2, soak the dry foamed cobalt into Ti 2 CT x In MQDs solution, Ti 2 CT x The concentration of MQDs solution was 2.5 mg / ml, the dosage was 10 ml, and the immersion time was 2 h, 4 h, 6 h, 9 h, 12 h, and 15 h, respectively;

[0041] S1.3, vacuum drying at 60°C to obtain Ti 2 CT x MQDs / Co 2 (OH) 3 Cl / Co foam integrated electrode;

[0042] S2. Electrochemical reconstruction to prepare Ti 2 CTx MQDs / β-Co(OH) 2 / Co foam:

[0043] Ti 2 CT x MQDs / Co 2 (OH) 3 The Cl / Co foam integrated electrode was used as the cathode of the three electrodes, the graphite rod was used as the counter electrode, and the saturated calomel electrode was used as the reference electrode. In the KOH solution, the concentration of the KOH solution was 1 mol / L, the dosage was 80 ml, and the reaction was carried out by power-on. The current density was -10 mA / cm 2 , the time is 3h, and the voltage change during the 3h deposition process is shown in Figure 3 It can be seen that under constant current, the voltage drops rapidly with the increase of time and remains stable within 3 hours. After 3 hours of deposition, the product Ti 2 CT x MQDs / β-Co(OH) 2 / Co foam, in which the product Ti based on 9 hours of immersion 2 CT x MQDs / β-Co(OH) 2 / Co foam-9h Figure 2 b and Figure 4 .

[0044] The foamed cobalt obtained in step S1.2 was immersed in an 8% HCl aqueous solution for 15 hours, and then dried to obtain Co 2 (OH) 3 Cl / Co foam-15h; and Ti obtained in step S1.3 2 CT x MQDs / Co 2 (OH) 3 Cl / Co foam-15h for comparison, Figure 2 As shown in c and a. It can be seen from the figure that Ti 2 CT x The presence of MQDs solution does not affect the generated Co 2 (OH) 3 The morphology of Cl.

[0045] The above Co 2 (OH) 3 Cl / Co foam-15h was electrochemically reconstructed according to step S2, and the product was named Co 2 (OH) 3 Cl / Co foam-15hD, its morphology is as follows Figure 2 d. By comparison Figure 2 b and d, it can be seen that the product obtained in the embodiment of the present invention exhibits β-Co(OH) 2 The flake morphology shows that Ti 2 CT x MQDs effectively induce Co 2 (OH) 3 Cl is converted into Co(OH)2 nanosheets. Figure 4 It can be seen that the SEM image after electrochemical activation shows that the irregular surface morphology has changed to hexagonal β-Co(OH) 2 The morphology of the nanosheets and EDS showed that Ti 2 CT x MQDs are evenly distributed on the surface of nanosheets.

[0046] Figure 5 The product Ti obtained at different immersion times in steps S1 and 2 of this embodiment 2 CT x MQDs / β-Co(OH) 2 The linear voltammetric scanning curve of / Cofoam shows that all products show excellent electrocatalytic alkaline hydrogen evolution performance, especially the Ti 2 CT x MQDs / β-Co(OH) 2 / Co foam-9h, which has the largest current at different voltages, that is, the catalytic activity is the best.

[0047] Figure 6 Ti 2 CT x MQDs / β-Co(OH) 2 The linear voltammetric scanning graph of / Co foam-9h shows that compared with the original Cofoam, the control sample without quantum dots, and the commercial platinum carbon, the Ti 2 CT x MQDs-induced β-Co(OH) 2 The electrocatalyst has good hydrogen evolution activity.

[0048] The above Co 2 (OH) 3 Cl / Co foam-15hD and Ti 2 CT x MQDs / β-Co(OH) 2 / Co foam-9h constant current stability test was carried out, by applying a constant current and observing the change trend of the voltage value over time. Figure 7 As shown in the figure, it can be seen that Co 2 (OH)3 Within 2 h of reaction, the generated cobalt hydroxide nanosheets were reduced, which led to rapid dissolution under the applied voltage, resulting in a sharp decline in performance and a gradual decrease in stability. 2 CT x MQDs / β-Co(OH) 2 / Co foam-9h always maintains a constant voltage value under the applied voltage, which proves the stable catalytic performance. It can be seen that QDs play a positive role in maintaining the generated cobalt hydroxide nanosheets.

[0049] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing MQDs-coordinated β-Co(OH)2 cobalt hydroxide nanosheets, characterized in that: The method includes: Titanium carbide (Ti2CT x )MXene multilayer nanosheets were added to an aqueous solution of HCl, stirred and reacted under an argon atmosphere, and then filtered through a 0.22um filter membrane and the filtrate was collected to obtain Ti2CT x MQDs solution; Ti2CT supported on a cobalt substrate x MQDs, and as the cathode of the three-electrode system, electrochemical reaction was carried out in KOH solution to obtain Ti2CT loaded on the surface of the cobalt matrix. x MQDs / β-Co(OH)2 nanosheet catalyst.

2. The preparation method according to claim 1, characterized in that: The mass fraction of the aqueous solution of HCl is 8%. The stirring reaction time is 72 hours.

3. The preparation method according to claim 1, characterized in that: The cobalt substrate is porous foam cobalt; the loading method is: immersing the porous foam cobalt in Ti2CT x MQDs solution.

4. The preparation method according to claim 3, characterized in that: The soaking time is 2-15h.

5. The preparation method according to claim 1, characterized in that: The electrolyte is 1M KOH solution, and the current density is -10mA / cm 2 .

6. The preparation method according to claim 1, characterized in that: Titanium carbide (Ti2CT x )MXene multilayer nanosheets were prepared by the following method: Ti2AlC was used as the bulk material, HCl and lithium fluoride were used as etchants to etch Ti2AlC, and two-dimensional layered Ti2CT was obtained after cleaning. x MXene.