Method for electro-deposition of high-corrosion-resistance aluminum-manganese alloy coating on magnesium alloy ionic liquid

Through anhydrous ethanol ultrasonic cleaning, sandblasting, pickling and activation treatment, combined with anhydrous manganese chloride and room temperature ionic liquid electrodeposition, a highly corrosion-resistant aluminum-manganese alloy coating was prepared, which solved the problem of magnesium alloy surface electroplating in the existing technology. The use of toxic substances and thermodynamic instability issues in the deposition process have resulted in a high-quality, dense aluminum-manganese alloy coating on the surface of the magnesium alloy, which has super corrosion resistance and protection properties.

CN118756271AInactive Publication Date: 2024-10-11ZHEJIANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410947147.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing magnesium alloy surface electrodeposition process, cyanide is highly toxic and its use is limited, the chemical nickel solution is thermodynamically unstable, the production cost is high, and the porosity of the coating is high, making it difficult to meet the corrosion resistance requirements of engineering neutral salt spray, and has not been seen. Research on electrodeposition of aluminum-manganese alloy coating on magnesium alloy surface in room temperature ionic liquid.

Method used

Ultrasonic cleaning with absolute ethanol, sandblasting to remove the oxide film, pickling and activation treatment are used to form a metallic zinc layer, followed by electrodeposition of aluminum-manganese coating in anhydrous manganese chloride and room temperature ionic liquid, and passivation treatment by chromate , to prepare highly corrosion-resistant aluminum-manganese alloy coatings.

Benefits of technology

A dense and smooth aluminum-manganese alloy coating on the magnesium alloy surface has been achieved. The coating has strong bonding force with the substrate, has super corrosion resistance and protection properties, and can withstand 500 hours of neutral salt spray without corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756271A_ABST
    Figure CN118756271A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of surface treatment, and provides a method for electro-deposition of a high-corrosion-resistance aluminum-manganese alloy coating on a magnesium alloy ionic liquid, which comprises the following steps: step 1, oil removal: carrying out room-temperature ultrasonic cleaning on a magnesium alloy matrix with absolute ethyl alcohol for 5-15 minutes; secondly, sand blasting is conducted, and an oxidation film naturally formed on the surface of the magnesium alloy is removed in a physical mode; 3, cleaning is conducted, after sand blasting, absolute ethyl alcohol is adopted for ultrasonic cleaning, and the cleaning time ranges from 5 min to 15 min; 4, acid pickling is conducted, specifically, the magnesium alloy surface is subjected to acid pickling through acid liquor; 5, activating, wherein the magnesium alloy matrix subjected to acid pickling is subjected to activating treatment; 6, zinc dipping, wherein a metal zinc layer is formed on the surface of the magnesium alloy in situ through a chemical replacement reaction; 7, an aluminum-manganese coating is electrodeposited, specifically, the aluminum-manganese coating is electrodeposited on the surface of the magnesium alloy, and electroplating liquid is prepared from anhydrous manganese chloride and room-temperature ionic liquid; and 8, passivation is conducted, specifically, a chromate passivating agent is adopted for conducting passivation treatment on the aluminum-manganese plating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of surface treatment and metal anticorrosion, and specifically is a method for electro-depositing a high-corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid. Background Art

[0002] As the lightest metal structural material, magnesium alloy has great potential for lightweight applications in aerospace, weapons and equipment and many other fields. However, its poor corrosion resistance greatly limits its wide application in aerospace and other fields. Electrodeposition of metal coatings on the surface of magnesium alloys is considered to be one of the most effective methods to improve the corrosion resistance of magnesium alloys.

[0003] At present, the two relatively mature process flows in the industry are "degreasing-pickling-activation-zinc immersion-cyanide pre-plating Cu-other electroplating" and "degreasing-pickling-activation-zinc immersion-chemical pre-plating Ni-other electroplating". The former involves highly toxic cyanide and is gradually restricted in use; the chemical nickel solution in the latter is a thermodynamically unstable system with a short service life, high production cost and high porosity of the coating. It is difficult for the existing coating system to meet the corrosion resistance requirements of 192 h neutral salt spray in engineering. Therefore, it is urgent to develop a new dense and corrosion-resistant coating system.

[0004] Metal Al and its alloy coating materials have excellent corrosion resistance, and the electrode potential is closer to that of magnesium alloys, making them very suitable for corrosion protection of magnesium alloys. However, the reduction potential of metal Al is more positive than that of hydrogen, so it cannot be prepared by electrodeposition from aqueous solution. Ionic liquids do not contain water, have a wide electrochemical window and high conductivity, and are a new ideal medium for electrodeposition of metal Al and its alloys. In addition, electrodeposition in anhydrous and oxygen-free ionic liquids is easier to obtain dense, high-quality coatings. Studies have shown that aluminum-manganese alloy coatings have super corrosion resistance, and the corrosion protection of neodymium iron boron (NdFeB) substrates can reach 1000 h of neutral salt spray without corrosion.

[0005] In addition, patent CN 101781785A discloses a method for electrodepositing a highly corrosion-resistant aluminum-manganese alloy on the surface of a magnesium alloy, but the aluminum-manganese alloy coating reported in the work is prepared by electrodeposition in an inorganic molten salt plating solution at a temperature close to 200°C. Therefore, the aluminum-manganese alloy coating has great application potential in the corrosion protection of magnesium alloys, but there is still no report on the research on the electrodeposition of aluminum-manganese alloy coating on the surface of magnesium alloy in room temperature ionic liquid and its corrosion resistance. Summary of the invention

[0006] In order to solve the above technical problems existing in the prior art, the present invention provides a method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid, comprising the following steps: Step 1: Degreasing The magnesium alloy substrate was ultrasonically cleaned with anhydrous ethanol at room temperature for 5 min to 15 min; Step 2: Sandblasting Physically remove the oxide film naturally formed on the surface of magnesium alloy; Step 3: Cleaning After sandblasting, ultrasonic cleaning was performed using anhydrous ethanol for 5 min to 15 min; Step 4: Pickling The surface of the magnesium alloy is pickled with an acid solution; Step 5: Activation The magnesium alloy substrate after pickling is activated; Step 6: Galvanizing A metallic zinc layer is formed in situ on the surface of the magnesium alloy by chemical replacement reaction; Step 7: Electrodeposition of aluminum-manganese coating An aluminum-manganese coating is electro-deposited on the surface of a magnesium alloy, wherein the electroplating solution is prepared from anhydrous manganese chloride and a room temperature ionic liquid; Step 8: Passivation The aluminum-manganese coating is passivated using a chromate passivator.

[0007] Furthermore, the physical method in step 2 includes sandpaper polishing and sandblasting; the sandpaper polishing mesh number is 400 mesh-5000 mesh; white corundum sand is used for sandblasting, the sandblasting pressure is 0.1 MPa-0.5 MPa, and the sandblasting time is 5 min-30 min.

[0008] Furthermore, the acid solution used for pickling in step 4 includes chromic acid, phosphoric acid, hydrochloric acid, hydrofluoric acid, nitric acid, acetic acid, citric acid or a combination thereof.

[0009] Furthermore, the concentration of the acid solution is 5 g / L-100 g / L, the pickling time is 1 min-10 min, and the temperature is room temperature.

[0010] Furthermore, the activation solution used in step five includes hydrofluoric acid, phosphoric acid, ammonium bifluoride, potassium fluoride, potassium pyrophosphate, sodium fluoride, sodium pyrophosphate, sodium carbonate or a combination thereof.

[0011] Furthermore, the concentration of the activation solution is 10 g / L-500 g / L, and the activation treatment time is 1 min-5 min.

[0012] Furthermore, the zinc immersion solution used in step six is ​​composed of ZnSO47H2O, K4P2O7, Na2CO3 and NaF solution; the zinc immersion temperature is 40°C-80°C, and the zinc immersion time is 2 min-10 min.

[0013] Furthermore, the ionic liquid in step seven is prepared from anhydrous aluminum chloride and a pyridine ionic liquid or an imidazole ionic liquid, the molar ratio of anhydrous aluminum chloride to the pyridine ionic liquid or the imidazole ionic liquid is between 2:1-1:1, and the concentration of anhydrous manganese chloride is 0.01 mol / L-0.2 mol / L.

[0014] Further, the pyridine ionic liquid includes N-ethylpyridine chloride, N-ethylpyridine bromide, N-ethylpyridine tetrafluoroborate, N-ethylpyridine trifluoromethanesulfonate and / or N-ethylpyridine hydrogen sulfate; the imidazole ionic liquid includes 1-methylimidazolium chloride, 1-methylimidazolium tetrafluoroborate, 1-ethylimidazolium chloride, 1-ethylimidazolium p-toluenesulfonate, 1-butylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium tetrafluoroborate and / or 1-ethyl-3-methylimidazolium trifluoromethanesulfonate; the plating solution temperature is 20°C-50°C, and the current density is 5 mA / cm 2 -100mA / cm 2 The electrodeposition time is 30 min-240 min, and the stirring method is gas stirring.

[0015] Furthermore, the passivation parameters in step eight are: pH 1.1-1.8, temperature 20-40°C, time 15s-3min, and the passivation film drying temperature is 50-80°C.

[0016] The magnesium alloy electrodeposited high corrosion-resistant aluminum-manganese alloy coating prepared by the method of the present invention has a cellular structure and is flat and dense, has no coating defects in surface morphology and cross-sectional morphology, has a coating thickness of about 10 μm, has a strong interface bonding force with the magnesium alloy substrate, and has super corrosion protection performance for the magnesium alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the surface morphology of the aluminum-manganese alloy coating on the surface of the magnesium alloy under a scanning electron microscope; Figure 2 This is the cross-sectional morphology of the aluminum-manganese alloy coating on the surface of the magnesium alloy under a scanning electron microscope; Figure 3 This is the surface morphology of the cross-cut area of ​​the aluminum-manganese alloy coating under a scanning electron microscope after the cross-cut method was used to test the bonding strength; Figure 4 This is a photograph of the appearance of the sample after the aluminum-manganese alloy coating on the surface of the magnesium alloy was passivated and subjected to a neutral salt spray test for 500 h. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the accompanying drawings.

[0019] The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid of the present invention comprises the following steps: Step 1: Degreasing The machined magnesium alloy sheets (including but not limited to AZ31B, AZ91D, AZ41, ZK61M, ZM5, etc.) were cut into small-size specimens of 10 mm×20 mm×6 mm. The specimens were ultrasonically cleaned with anhydrous ethanol at room temperature for 5 min to 15 min to fully remove the oil stains that may be attached to the surface of the specimens, so as to obtain a fully clean magnesium alloy surface.

[0020] Step 2: Sandblasting Physical methods are used to completely remove the oxide film naturally formed on the surface of the magnesium alloy to expose the fresh surface of the magnesium alloy matrix. Physical methods include but are not limited to sandpaper polishing and sandblasting. The mesh size of sandpaper polishing is 400-5000 mesh; white corundum sand is used for sandblasting, the sandblasting pressure is 0.1 MPa-0.5 MPa, and the sandblasting time is 5 min-30 min, until the surface appearance of the magnesium alloy is uniform.

[0021] Step 3: Cleaning In order to remove the sand particles remaining or embedded on the surface of the magnesium alloy due to sandblasting, the samples were immediately ultrasonically cleaned with anhydrous ethanol after sandblasting for 5 min to 15 min.

[0022] Step 4: Pickling In order to fully remove the oxide film of the magnesium alloy, the surface of the magnesium alloy is pickled with an acid solution. The acid solution used includes but is not limited to chromic acid, phosphoric acid, hydrochloric acid, hydrofluoric acid, nitric acid, acetic acid, citric acid or a combination thereof. The concentration of the acid solution is 5 g / L-100 g / L, the pickling time is 1 min-10 min, and the temperature is room temperature (20-25°C).

[0023] Step 5: Activation In order to remove the thin oxide film formed by reoxidation of the magnesium alloy during the pretreatment process, and to form a protective film in situ on the surface of the magnesium alloy to prevent the magnesium alloy from corroding in the subsequent treatment solution, the magnesium alloy sample after pickling is further activated. The components of the activation solution include but are not limited to hydrofluoric acid, phosphoric acid, ammonium bifluoride, potassium fluoride, potassium pyrophosphate, sodium fluoride, sodium pyrophosphate, sodium carbonate or a combination thereof. The concentration of various components in the activation solution is 10 g / L-500 g / L, and the activation treatment time is 1 min-5 min.

[0024] Step 6: Galvanizing The essence of zinc immersion is to form a thin layer of metal zinc layer in situ on the surface of magnesium alloy through chemical replacement reaction. This zinc layer can prevent magnesium alloy from being oxidized in subsequent processes and undergo replacement reaction with metal ions in the electrolyte, which can effectively ensure the bonding strength between the subsequent coating and the magnesium alloy matrix. The zinc immersion solution is mainly composed of ZnSO47H2O (30 g / L -60 g / L), K4P2O7 (120 g / L -160 g / L), Na2CO3 (5 g / L -10 g / L) and NaF (5 g / L -10 g / L). The zinc immersion temperature is 40℃-80℃, and the zinc immersion time is 2 min-10min.

[0025] Step 7: Electrodeposition of aluminum-manganese coating The electroplating solution is prepared from anhydrous manganese chloride and a room temperature ionic liquid, wherein the ionic liquid is prepared from anhydrous aluminum chloride and a pyridine ionic liquid (including but not limited to N-ethylpyridinium chloride, N-ethylpyridinium bromide, N-ethylpyridinium tetrafluoroborate, N-ethylpyridinium trifluoromethanesulfonate, N-ethylpyridinium hydrogen sulfate, etc.) or an imidazole ionic liquid (including but not limited to 1-methylimidazolium chloride, 1-methylimidazolium tetrafluoroborate, 1-ethylimidazolium chloride, 1-ethylimidazolium p-toluenesulfonate, 1-butylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, etc.), the molar ratio of anhydrous aluminum chloride to the pyrazole ionic liquid or the imidazole ionic liquid is between 2:1 and 1:1, and the concentration of anhydrous manganese chloride is 0.01 mol / L -0.2 mol / L. The plating solution temperature is 20℃-50℃, and the current density is 5 mA / cm 2 -100 mA / cm 2 The electrodeposition time is 30 min-240 min, and the stirring method is gas stirring.

[0026] Step 8: Passivation The aluminum-manganese coating was passivated with a chromate passivating agent (Alodine 1200s). Passivation parameters: pH 1.1-1.8, temperature 20-40°C, time 15s-3min. The passivation film drying temperature was 50-80°C.

[0027] Between step 4, step 5, step 6, step 7 and step 8, at least two water washes are required after each process, and the washing time is 2-5 minutes. Example 1

[0028] AZ31B magnesium substrate, 1000 grit sandpaper polishing, anhydrous ethanol ultrasonic treatment for 10 min, chromic acid (100 g / L) pickling at room temperature for 2 min, hydrofluoric acid (300 g / L, 40% volume fraction) activation at room temperature for 3 min, zinc immersion at 80 ° C for 10 min, the zinc immersion solution is composed of ZnSO47H2O (30 g / L), K4P2O7 (130 g / L), Na2CO3 (5 g / L) and NaF (6 g / L), the current density of the electrodeposition of aluminum-manganese alloy is 15 mA / cm 2 , the plating solution temperature is 20℃, the electrodeposition time is 80 min, and the gas is stirred. The concentration of anhydrous manganese chloride is 0.08 mol / L. Through the above surface treatment, the ionic liquid electrodeposition preparation of aluminum-manganese alloy coating is successfully achieved on the surface of magnesium alloy. Example 2

[0029] AZ31B magnesium substrate, 1000 grit sandpaper polishing, anhydrous ethanol ultrasonic 10 min, chromic acid (100 g / L) pickling at room temperature for 3 min, ammonium bifluoride (120 g / L) activation at room temperature for 2 min, 70 ° C zinc immersion for 5 min, zinc immersion solution composed of ZnSO47H2O (30 g / L), K4P2O7 (130 g / L), Na2CO3 (5 g / L) and NaF (6 g / L), the current density of the electrodeposition of aluminum manganese alloy is 15 mA / cm 2 , the bath temperature was 20℃, the electrodeposition time was 80 min, and the gas was stirred. The concentration of anhydrous manganese chloride was 0.08 mol / L. Through the above surface treatment, the ionic liquid electrodeposition preparation of aluminum-manganese alloy coating was successfully achieved on the surface of magnesium alloy. Example 3

[0030] AZ31B magnesium substrate, 1000 grit sandpaper polishing, anhydrous ethanol ultrasonic 10 min, citric acid (10 g / L) pickling at room temperature for 1 min, ammonium bifluoride (100 g / L) activation at room temperature for 3 min, 80 ° C zinc immersion for 10 min, zinc immersion solution composed of ZnSO47H2O (30 g / L), K4P2O7 (130 g / L), Na2CO3 (5 g / L) and NaF (6 g / L), the current density of the electrodeposition of aluminum manganese alloy is 15 mA / cm 2 , the bath temperature was 20℃, the electrodeposition time was 80 min, and the gas was stirred. The concentration of anhydrous manganese chloride was 0.08 mol / L. Through the above surface treatment, the ionic liquid electrodeposition preparation of aluminum-manganese alloy coating was successfully achieved on the surface of magnesium alloy.

[0031] like Figure 1 and Figure 2As shown in the figure, the coating presents a typical cellular structure and is flat and dense. No coating defects are observed in the surface morphology and cross-sectional morphology. The coating thickness is about 10 μm. Figure 3 As shown in the figure, the 100-grid test showed that no peeling or shedding of the coating occurred after the grid was taped and torn off, indicating that the pretreatment process basically ensured the interface bonding strength between the coating and the magnesium alloy substrate. Figure 4 As shown in the figure, the neutral salt spray test results show that the aluminum-manganese alloy coating has super strong corrosion protection performance for magnesium alloy, and can achieve 500 hours of neutral salt spray without corrosion.

Claims

1. A method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid, comprising the following steps: Step 1: Degreasing The magnesium alloy substrate was ultrasonically cleaned with anhydrous ethanol at room temperature for 5 min to 15 min; Step 2: Sandblasting Physically remove the oxide film naturally formed on the surface of magnesium alloy; Step 3: Cleaning After sandblasting, ultrasonic cleaning was performed using anhydrous ethanol for 5 min to 15 min; Step 4: Pickling The surface of the magnesium alloy is pickled with an acid solution; Step 5: Activation The magnesium alloy substrate after pickling is activated; Step 6: Galvanizing A metallic zinc layer is formed in situ on the surface of the magnesium alloy by chemical replacement reaction; Step 7: Electrodeposition of aluminum-manganese coating An aluminum-manganese coating is electro-deposited on the surface of a magnesium alloy, wherein the electroplating solution is prepared from anhydrous manganese chloride and a room temperature ionic liquid; Step 8: Passivation The aluminum-manganese coating is passivated using chromate passivator.

2. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: The physical method in step 2 includes sandpaper polishing and sandblasting; the sandpaper polishing mesh number is 400 mesh-5000 mesh; white corundum sand is used for sandblasting, the sandblasting pressure is 0.1 MPa-0.5 MPa, and the sandblasting time is 5 min-30 min.

3. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: The acid solution used for pickling in step 4 includes chromic acid, phosphoric acid, hydrochloric acid, hydrofluoric acid, nitric acid, acetic acid, citric acid or a combination thereof.

4. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 3, characterized in that: The concentration of the acid solution is 5 g / L-100 g / L, the pickling time is 1 min-10 min, and the temperature is room temperature.

5. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: The activation solution used in step five includes hydrofluoric acid, phosphoric acid, ammonium bifluoride, potassium fluoride, potassium pyrophosphate, sodium fluoride, sodium pyrophosphate, sodium carbonate or a combination thereof.

6. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 5, characterized in that: The concentration of the activation solution is 10 g / L-500 g / L, and the activation treatment time is 1 min-5 min.

7. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: The zinc immersion solution used in step six is ​​composed of ZnSO47H2O, K4P2O7, Na2CO3 and NaF solution; the zinc immersion temperature is 40°C-80°C, and the zinc immersion time is 2 min-10 min.

8. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: The ionic liquid in step seven is prepared from anhydrous aluminum chloride and a pyridine ionic liquid or an imidazole ionic liquid, the molar ratio of anhydrous aluminum chloride to the pyridine ionic liquid or the imidazole ionic liquid is between 2:1 and 1:1, and the concentration of anhydrous manganese chloride is 0.01 mol / L -0.2 mol / L.

9. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: The pyridine ionic liquid includes N-ethylpyridinium chloride, N-ethylpyridinium bromide, N-ethylpyridinium tetrafluoroborate, N-ethylpyridinium trifluoromethanesulfonate and / or N-ethylpyridinium hydrogen sulfate; the imidazole ionic liquid includes 1-methylimidazolium chloride, 1-methylimidazolium tetrafluoroborate, 1-ethylimidazolium chloride, 1-ethylimidazolium p-toluenesulfonate, 1-butylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium tetrafluoroborate and / or 1-ethyl-3-methylimidazolium trifluoromethanesulfonate; the plating solution temperature is 20°C-50°C, and the current density is 5 mA / cm 2 -100 mA / cm 2 The electrodeposition time is 30 min-240 min, and the stirring method is gas stirring.

10. The method for electro-depositing a high corrosion-resistant aluminum-manganese alloy coating using a magnesium alloy ionic liquid as claimed in claim 1, characterized in that: In step 8, the passivation parameters are as follows: pH 1.1-1.8, temperature 20-40°C, time 15s-3min, and the passivation film drying temperature is 50-80°C.

Citation Information

Patent Citations

  • Preparation method of Al-Mn alloy prevention plating layer on surface of metallic matrix

    CN103103588A

  • Process for electroplating aluminum or aluminum-manganese alloy coating with super corrosion resistance and no hydrogen embrittlement

    CN117867611A