Metal substrate surface anti-fingerprint treatment process
By carrying out pretreatment, anodizing, dyeing, hole sealing and anti-fingerprint treatment on the surface of aluminum and aluminum alloy products, and using a specific anti-fingerprint treatment liquid, the problem of complex and high-cost anti-fingerprint treatment in the existing technology is solved, and simplification is achieved Process and cost-reducing effects, forming a film that is anti-fingerprint, anti-fouling and anti-corrosion.
Patent Information
- Application Number
- CN202410855148.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
AI Technical Summary
The anti-fingerprint treatment process on the surface of existing aluminum and aluminum alloy products is complex and costly, making it difficult to meet the needs of industrial production.
Adopt a process including pretreatment, anodizing treatment, dyeing treatment, sealing treatment and anti-fingerprint treatment, use anti-fingerprint treatment liquid (hydration accelerator, buffer, silicate, phosphate, apatite, limestone, boric acid Aqueous solutions of salts, aluminates and wetting agents) are used for anti-fingerprint treatment, simplifying the process and reducing production costs.
It achieves a good anti-fingerprint effect on the surface of the metal substrate, reduces production costs, simplifies the process, and forms a film with oxidation stability, hydrophobicity and chemical inertness to prevent dirt and corrosion.
Smart Images

Figure CN118756285A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment, and in particular to an anti-fingerprint treatment process for a metal substrate surface. Background Art
[0002] Metal substrates, such as aluminum and aluminum alloys, are widely used in the fields of construction, decoration, fixtures, automobiles, etc. The surface hardness of aluminum and aluminum alloys is low and they are easily eroded and damaged by the external environment, so surface treatment is required to improve their performance. Surface treatment can not only improve the corrosion resistance, wear resistance and fatigue resistance of aluminum and aluminum alloys, but also improve their appearance quality and meet the decorative requirements of different application scenarios. With the continuous advancement of science and technology and the improvement of people's requirements for the quality of life, higher requirements are placed on aluminum and aluminum alloy products. During the use of aluminum and aluminum alloy products, fingerprints, oil, sweat stains and other traces of use are easily left on the surface, which affects their appearance, and fingerprints, oil, sweat stains, etc. left for a long time will accelerate corrosion and affect their service life. Therefore, it is extremely important to carry out anti-fingerprint treatment on aluminum and aluminum alloy products.
[0003] At present, the anti-fingerprint treatment process commonly used in the industry for aluminum and aluminum alloy products is usually to add an AF spraying or AF coating process after the surface anodizing treatment. The specific process flow diagram is as follows: Figure 1 The existing process requires the configuration of corresponding spraying equipment or coating equipment, and the process is complicated and has the disadvantages of high price and high cost.
[0004] Therefore, there is an urgent need for an anti-fingerprint treatment process for the surface of a metal substrate to address the deficiencies of the prior art. Summary of the invention
[0005] The object of the present invention is to provide a metal substrate surface anti-fingerprint treatment process, the metal substrate surface treatment process is simple and easy to implement, the production cost is low, and the metal substrate obtained by the treatment process has a good anti-fingerprint effect.
[0006] To achieve the above object, the present invention provides a process for anti-fingerprint treatment of a metal substrate surface, comprising the steps of:
[0007] Pre-treating the metal substrate to be processed;
[0008] The metal substrate is subjected to anodizing treatment;
[0009] Using dyeing liquid to dye the metal substrate;
[0010] Using a sealing liquid to perform a pore sealing treatment on the metal substrate;
[0011] The metal substrate is subjected to anti-fingerprint treatment by using an anti-fingerprint treatment liquid, wherein the anti-fingerprint treatment liquid is an aqueous solution including a hydration accelerator, a buffer, a silicate, a phosphate, apatite, limestone, a borate, aluminate and a wetting agent.
[0012] Compared with the prior art, the surface treatment process with anti-fingerprint effect of the present invention includes pretreatment, anodizing, dyeing, sealing and anti-fingerprint treatment of the metal substrate. By arranging the anti-fingerprint treatment after the sealing treatment, there is no need to add a separate AF coating or AF spraying production line, which effectively reduces the production cost and significantly simplifies the production process. The anti-fingerprint treatment liquid of the present invention is an aqueous solution including a hydration accelerator, a buffer, a silicate, a phosphate, apatite, limestone, a borate, an aluminate and a wetting agent, which can form a layer of film with oxidation stability, hydrophobicity and chemical inertness on the surface of the metal substrate oxide film after sealing, so it has the effect of inhibiting surface dusting, improving surface smoothness and preventing dirt. Therefore, the present invention incorporates the anti-fingerprint treatment into the anodizing process of the metal substrate, so that the process is simple and easy, the production cost is low, and it has a good anti-fingerprint effect.
[0013] As a preferred technical solution, the mass concentration of the anti-fingerprint treatment liquid is 8-20 g / L.
[0014] As a preferred technical solution, the anti-fingerprint treatment is specifically to immerse the metal substrate in an anti-fingerprint treatment liquid, the temperature of the anti-fingerprint treatment liquid is 90-95°C, the time of the anti-fingerprint treatment is 15-25 minutes, and the pH of the anti-fingerprint treatment liquid is 5-7.
[0015] As a preferred technical solution, the pretreatment includes chemical polishing and one-time neutralization of the metal substrate.
[0016] As a preferred technical solution, the thickness of the oxide film obtained on the metal substrate after the anodizing treatment is 12 to 15 μm.
[0017] As a preferred technical solution, the electrolyte for the anodizing treatment is sulfuric acid, the mass concentration of the sulfuric acid is 200-220 g / L, the temperature of the electrolyte is 10-25°C, the treatment time is 50-60 min, and the treatment voltage is 10-15V.
[0018] As a preferred technical solution, the dye solution includes at least one of sulfuric acid, phosphoric acid, chromic acid and oxalic acid, and the mass concentration of the dye solution is 0.6-4 g / L.
[0019] As a preferred technical solution, the sealing treatment is specifically to immerse the metal substrate in a sealing liquid, the mass concentration of the sealing liquid is 12 to 13 g / L, the temperature of the sealing treatment is 85 to 95°C, the time of the sealing treatment is 30 to 45 minutes, and the pH of the sealing liquid is 5 to 7.
[0020] As a preferred technical solution, after the anti-fingerprint treatment, the metal substrate is further subjected to post-treatment, and the post-treatment includes secondary neutralization, water washing and drying.
[0021] As a preferred technical solution, the metal substrate is selected from aluminum or aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the process of anti-fingerprint treatment of metal substrate surface in the prior art;
[0023] Figure 2 It is a schematic diagram of the process of anti-fingerprint treatment of the metal substrate surface of the present invention;
[0024] Figure 3 This is a schematic diagram of the oxide film structure before the sealing treatment of the present invention;
[0025] Figure 4 This is a schematic diagram of the oxide film structure after the pore sealing treatment of the present invention;
[0026] Figure 5 This is a schematic diagram of the structure of the oxide film after anti-fingerprint treatment of the present invention. DETAILED DESCRIPTION
[0027] The present invention discloses a metal substrate surface anti-fingerprint treatment process, such as Figure 2 As shown, the steps include:
[0028] Pre-treating the metal substrate to be processed;
[0029] Anodizing the metal substrate;
[0030] The metal substrate is dyed with a dye solution;
[0031] The metal substrate is sealed with a sealing liquid;
[0032] Use anti-fingerprint treatment liquid to perform anti-fingerprint treatment on the metal substrate;
[0033] Post-processing of metal substrates.
[0034] Furthermore, the metal substrate of the present invention may be aluminum or an aluminum alloy.
[0035] Furthermore, the purpose of pretreatment is to eliminate defects existing on the surface of the metal substrate to be processed and to improve the surface finish of the metal substrate so as to carry out subsequent processing. The pretreatment of the present invention includes chemical polishing and one-time neutralization of the metal substrate. Specifically, chemical polishing can be to immerse the metal substrate to be processed in a chemical polishing solution. The chemical polishing solution used can be an acid solution or an alkaline solution. The acid solution can be but not limited to at least one of sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid and hydrofluoric acid. The alkaline solution can be but not limited to sodium hydroxide. Among them, the concentration of the acid solution can be 10% to 25%, the mass concentration of the alkaline solution can be 10g / L to 50g / L, the temperature of the chemical polishing solution can be 80 to 90°C, and the processing time can be 100 to 180s. Specifically, the concentration of the acid solution of the present invention may be, but is not limited to, 10%, 15%, 20%, or 25%; the mass concentration of the alkali solution may be, but is not limited to, 10g / L, 20g / L, 30g / L, 40g / L, or 50g / L; the temperature of the chemical polishing solution may be, but is not limited to, 80°C, 82°C, 84°C, 86°C, 88°C, or 90°C; the treatment time may be, but is not limited to, 100s, 110s, 120s, 140s, 160s, or 180s. As an example, the chemical polishing solution may be a phosphoric acid and sulfuric acid solution having a mass concentration of 3 to 10:1, the temperature of the chemical polishing solution may be 85°C, and the treatment time may be 120s. The metal substrate after chemical polishing is washed with water, and the water washing may be, but is not limited to, double water washing to remove the chemical polishing solution remaining on the surface of the metal substrate. The washed metal substrate is neutralized once to further remove the chemical polishing. The primary neutralization liquid may be an acid solution or an alkali solution, the primary neutralization temperature may be room temperature, and the primary neutralization time may be 50 to 150 seconds. Specifically, the primary neutralization time may be, but not limited to, 50 seconds, 60 seconds, 70 seconds, 80 seconds, 90 seconds, 100 seconds, 120 seconds, 140 seconds, or 150 seconds. For example, the primary neutralization time is 60 seconds. The metal substrate after the primary neutralization is washed with water, and the washing may be, but not limited to, double washing or quadruple washing to remove impurities such as the neutralization liquid and salts on the surface of the metal substrate for subsequent anodizing treatment.
[0036] Furthermore, the pretreated metal substrate is anodized to form an oxide film on the surface of the metal substrate to improve the corrosion resistance, hardness and other properties of the metal substrate. At the same time, the oxide film has a large number of micropores, which can absorb a variety of beautiful and bright colors, and can further improve the processing diversity of metal substrate products. Specifically, the electrolyte used in the anodizing treatment of the present invention is sulfuric acid, the mass concentration of sulfuric acid is 200-220g / L, the temperature of the electrolyte is 10-25°C, the treatment time is 50-60min, and the treatment voltage is 10-15V. As an example, the mass concentration of sulfuric acid in the present invention may be, but is not limited to, 200g / L, 202g / L, 204g / L, 206g / L, 208g / L, 210g / L, 212g / L, 214g / L, 216g / L, 218g / L, 220g / L; the temperature of the electrolyte in the present invention may be, but is not limited to, 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, 23°C, 25°C; the anodizing treatment time in the present invention may be, but is not limited to, 50min, 52min, 54min, 56min, 58min, 60min; the treatment voltage in the present invention may be, but is not limited to, 10V, 11V, 12V, 13V, 14V, 15V. The thickness of the surface oxide film obtained after the metal substrate of the present invention is treated by anodization is 12 to 15 μm. Specifically, the thickness of the oxide film of the present invention can be, but is not limited to, 12 μm, 13 μm, 14 μm, or 15 μm. The metal substrate after anodization is washed with water to remove the electrolyte on the surface of the metal substrate for subsequent dyeing treatment. The washing can be, but is not limited to, double washing or quadruple washing. The schematic diagram of the oxide film structure before the sealing treatment of the present invention can be seen in Figure 3 .
[0037] Further, the metal substrate after anodizing treatment is dyed, and the dye molecules are adsorbed in the micropores of the oxide film on the surface of the metal substrate, so that the metal substrate has different colors to meet the different market demands for the appearance color of metal products. The dye liquor of the present invention includes at least one of sulfuric acid, phosphoric acid, chromic acid and oxalic acid, and the mass concentration of the dye liquor is 0.6-4g / L. Specifically, the mass concentration of the dye liquor of the present invention may be, but is not limited to, 0.6g / L, 0.8g / L, 1.0g / L, 2.0g / L, 3.0g / L, 4.0g / L. Specifically, the dyeing treatment is specifically to immerse the substrate in the dye liquor, the temperature of the dye liquor is room temperature, and the immersion time is 5-8min, specifically but not limited to 5min, 6min, 7min, 8min. The metal substrate after dyeing treatment is washed with water to remove excess dye liquor for subsequent sealing treatment. The washing may be, but is not limited to, double washing or quadruple washing.
[0038] Furthermore, the metal substrate after dyeing is sealed to fix the color of the dye and further improve the corrosion resistance and wear resistance of the metal substrate. The sealing liquid of the present invention uses a nickel-containing sealing liquid, the mass concentration of the nickel-containing sealing liquid is 12-13 g / L, the sealing temperature of the present invention is 85-95°C, the sealing time is 30-45 minutes, and the pH of the sealing liquid is 5-7. Specifically, the nickel-containing sealing liquid is a sealing liquid commonly used in the art. As an example, the nickel-containing sealing liquid can be, but is not limited to, at least one of nickel fluoride, nickel acetate, and fluorine nickel salt. The temperature of the sealing treatment is 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, and 95°C; the time of the sealing treatment may be, but is not limited to, 30min, 32min, 34min, 36min, 38min, 40min, 42min, 44min, and 45min; the pH of the sealing liquid may be, but is not limited to, 5, 5.5, 6, 6.5, and 7. In the sealing process, the sealing is completed by the water absorption and expansion of the oxide in the pores of the oxide film of the metal substrate and the hydrolysis of the nickel ions in the nickel-containing sealing agent to form nickel hydroxide precipitates that are deposited in the pores. The metal substrate after the sealing treatment is washed with water to remove excess nickel-containing sealing liquid to facilitate subsequent anti-fingerprint treatment. The schematic diagram of the oxide film structure after the sealing treatment of the present invention can be found in Figure 4 .
[0039] Furthermore, the metal substrate after the sealing treatment is subjected to anti-fingerprint treatment to enhance the anti-fingerprint, anti-fouling and anti-corrosion effects of the metal substrate. The anti-fingerprint treatment liquid of the present invention is an aqueous solution comprising a hydration accelerator, a buffer, a silicate, a phosphate, apatite, limestone, a borate, an aluminate and a wetting agent. The anti-fingerprint treatment is specifically to immerse the metal substrate after the sealing treatment in the anti-fingerprint treatment liquid. The temperature of the anti-fingerprint treatment liquid of the present invention is 90 to 95°C, the time of the anti-fingerprint treatment is 15 to 25 minutes, the pH of the anti-fingerprint treatment liquid is 5 to 7, and the mass concentration of the anti-fingerprint treatment liquid is 8 to 20 g / L. Specifically, the temperature of the anti-fingerprint treatment may be, but is not limited to, 90°C, 91°C, 92°C, 93°C, 94°C, and 95°C; the time of the anti-fingerprint treatment may be, but is not limited to, 15min, 17min, 19min, 21min, 23min, and 25min; the pH of the anti-fingerprint treatment liquid may be, but is not limited to, 5, 5.5, 6, 6.5, and 7; the mass concentration of the anti-fingerprint treatment liquid may be, but is not limited to, 8g / L, 9g / L, 10g / L, 11g / L, 12g / L, 13g / L, 14g / L, 15g / L, 16g / L, 17g / L, 18g / L, 19g / L, and 20g / L. The anti-fingerprint treatment liquid of the present invention contains a hydration accelerator, a buffer, a silicate, a phosphate, apatite, a limestone, a borate, an aluminate and a wetting agent, which can form an anti-fingerprint film on the surface of the oxide film after sealing. The anti-fingerprint film has good hydrophobicity and anti-fouling effects. At the same time, the film can further prevent the escape of dye molecules and nickel ions in the pores of the oxide film. The metal substrate after anti-fingerprint treatment is washed with water to remove the anti-fingerprint treatment liquid remaining on its surface to facilitate subsequent processing. Specifically, the anti-fingerprint treatment liquid of the present invention can be ODM DEAL E-600TP of Heyun Technology Co., Ltd. or DX-500 of Japan Okuno Corporation, but the present invention is not limited to this. The schematic diagram of the oxide film structure after the sealing treatment of the present invention can be seen in Figure 5 .
[0040] Further, the metal substrate after anti-fingerprint treatment is post-treated. The post-treatment includes secondary neutralization, water washing and drying of the metal substrate. The secondary neutralization solution used for the secondary neutralization is an alkali solution, the mass concentration of the alkali solution can be 50-60g / L, the temperature of the secondary neutralization reaction is room temperature, and the time of the secondary neutralization reaction is 100-200s. Specifically, the mass concentration of the alkali solution can be but not limited to 50, 52, 54, 56, 58, 60g / L; the time of the secondary neutralization reaction can be but not limited to 100s, 120s, 140s, 160s, 180s, 200s. The drying temperature can be 80-100°C, and the drying time can be 10-30min. Specifically, the drying temperature can be but not limited to 80°C, 85°C, 90°C, 95°C, 100°C; the drying time can be but not limited to 10min, 15min, 20min, 25min, 30min. As an example, the post-treatment of the present invention can be to place the metal substrate after anti-fingerprint treatment in a 60g / L sodium hydroxide solution, react at room temperature for 120s, wash with water to remove the secondary neutralization liquid, salts and other impurities remaining on the surface of the metal substrate, and then place it in an oven and dry it at 90°C for 20min.
[0041] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.
[0042] Example 1
[0043] This embodiment provides an aluminum alloy surface treatment process with an anti-fingerprint effect, comprising the steps of:
[0044] (1) placing the aluminum alloy to be processed in a mixture of phosphoric acid and sulfuric acid with a mass concentration of 3:1, reacting at 85° C. for 120 seconds, and then washing with water; then placing the aluminum alloy in 20% hydrochloric acid, reacting at room temperature for 60 seconds, and then washing with water;
[0045] (2) subjecting the aluminum alloy to anodizing treatment, wherein the electrolyte is sulfuric acid with a mass concentration of 200 g / L, the treatment voltage is 14 V, the temperature is 18° C., the treatment time is 50 min, the thickness of the obtained aluminum alloy oxide film is 12 μm, and the anodizing treatment is followed by water washing;
[0046] (3) The aluminum alloy was immersed in sulfuric acid with a mass concentration of 1 g / L for dyeing, the temperature of the sulfuric acid was room temperature, and then washed with water after immersion for 5 minutes;
[0047] (4) placing the aluminum alloy in nickel fluoride with a mass concentration of 12 g / L for sealing treatment, the sealing temperature is 85° C., the sealing time is 30 min, the pH of the sealing solution is 5, and the aluminum alloy is washed with water after the sealing treatment;
[0048] (5) placing the aluminum alloy in an anti-fingerprint treatment liquid with a mass concentration of 20 g / L for anti-fingerprint treatment, the temperature of the anti-fingerprint treatment liquid is 90° C., the anti-fingerprint treatment time is 15 min, the pH of the anti-fingerprint treatment liquid is 5, and washing is performed after the anti-fingerprint treatment, wherein the anti-fingerprint treatment liquid is DX-500 produced by Japan Okuno Corporation;
[0049] (6) The aluminum alloy was placed in a sodium hydroxide solution with a mass concentration of 60 g / L, reacted at room temperature for 120 seconds, washed with water, and dried in an oven at 90° C. for 20 minutes to obtain an aluminum alloy with an anti-fingerprint effect.
[0050] Example 2
[0051] This embodiment provides an aluminum alloy surface treatment process with an anti-fingerprint effect, comprising the steps of:
[0052] (1) placing the aluminum alloy to be processed in a mixture of phosphoric acid and sulfuric acid with a mass concentration of 5:1, reacting at 80° C. for 150 seconds, and then washing with water; then placing the aluminum alloy in 25% hydrochloric acid, reacting at room temperature for 80 seconds, and then washing with water;
[0053] (2) anodizing the aluminum alloy, wherein the electrolyte is sulfuric acid with a mass concentration of 210 g / L, the treatment voltage is 11 V, the temperature is 20° C., the treatment time is 55 min, and the thickness of the obtained aluminum alloy oxide film is 14 μm. After the anodizing treatment, the aluminum alloy is washed with water;
[0054] (3) The aluminum alloy was immersed in sulfuric acid with a mass concentration of 0.5 g / L for dyeing, the temperature of the sulfuric acid was room temperature, and then washed with water after immersion for 7 minutes;
[0055] (4) placing the aluminum alloy in nickel fluoride with a mass concentration of 12 g / L for sealing treatment, the sealing temperature is 90° C., the sealing time is 38 min, the pH of the sealing solution is 6, and the aluminum alloy is washed with water after the sealing treatment;
[0056] (5) placing the aluminum alloy in an anti-fingerprint treatment liquid with a mass concentration of 15 g / L for anti-fingerprint treatment, the temperature of the anti-fingerprint treatment liquid is 92° C., the anti-fingerprint treatment time is 21 min, the pH of the anti-fingerprint treatment liquid is 6, and washing is performed after the anti-fingerprint treatment, wherein the anti-fingerprint treatment liquid is ODM DEAL E-600TP of Heyun Technology Co., Ltd.;
[0057] (6) The aluminum alloy was placed in a sodium hydroxide solution with a mass concentration of 55 g / L, reacted at room temperature for 150 seconds, washed with water, and dried in an oven at 85° C. for 30 minutes to obtain an aluminum alloy with an anti-fingerprint effect.
[0058] Example 3
[0059] This embodiment provides an aluminum alloy surface treatment process with an anti-fingerprint effect, comprising the steps of:
[0060] (1) placing the aluminum alloy to be processed in a mixture of phosphoric acid and sulfuric acid with a mass concentration of 8:1, reacting at 90° C. for 110 seconds, and then washing with water; then placing the aluminum alloy in 18% hydrochloric acid, reacting at room temperature for 100 seconds, and then washing with water;
[0061] (2) anodizing the aluminum alloy, wherein the electrolyte is sulfuric acid with a mass concentration of 218 g / L, the treatment voltage is 15 V, the temperature is 24° C., the treatment time is 60 min, the thickness of the obtained aluminum alloy oxide film is 15 μm, and the anodizing treatment is followed by water washing;
[0062] (3) The aluminum alloy was immersed in sulfuric acid with a mass concentration of 3 g / L for dyeing, the temperature of the sulfuric acid was room temperature, and then washed with water after immersion for 8 minutes;
[0063] (4) The aluminum alloy was placed in nickel acetate with a mass concentration of 13 g / L for sealing treatment, the sealing temperature was 95° C., the sealing time was 43 min, the pH of the sealing solution was 6.8, and the aluminum alloy was washed with water after the sealing treatment;
[0064] (5) placing the aluminum alloy in an anti-fingerprint treatment liquid with a mass concentration of 10 g / L for anti-fingerprint treatment, the temperature of the anti-fingerprint treatment liquid is 95° C., the anti-fingerprint treatment time is 24 min, the pH of the anti-fingerprint treatment liquid is 6.8, and washing is performed after the anti-fingerprint treatment, wherein the anti-fingerprint treatment liquid is ODM DEAL E-600TP of Heyun Technology Co., Ltd.;
[0065] (6) The aluminum alloy was placed in a sodium hydroxide solution with a mass concentration of 50 g / L, reacted at room temperature for 180 seconds, washed with water, and dried in an oven at 95° C. for 15 minutes to obtain an aluminum alloy with an anti-fingerprint effect.
[0066] Comparative Example 1
[0067] This comparative example provides an aluminum alloy surface treatment process with an anti-fingerprint effect, comprising the steps of:
[0068] (1) placing the aluminum alloy to be processed in a mixture of phosphoric acid and sulfuric acid with a mass concentration of 3:1, reacting at 85° C. for 120 seconds, and then washing with water; then placing the aluminum alloy in 20% hydrochloric acid, reacting at room temperature for 60 seconds, and then washing with water;
[0069] (2) subjecting the aluminum alloy to anodizing treatment, wherein the electrolyte is sulfuric acid with a mass concentration of 200 g / L, the treatment voltage is 14 V, the temperature is 18° C., the treatment time is 50 min, the thickness of the obtained aluminum alloy oxide film is 12 μm, and the anodizing treatment is followed by water washing;
[0070] (3) The aluminum alloy was immersed in sulfuric acid with a mass concentration of 1 g / L for dyeing, the temperature of the sulfuric acid was room temperature, and then washed with water after immersion for 5 minutes;
[0071] (4) placing the aluminum alloy in nickel fluoride with a mass concentration of 12 g / L for sealing treatment, the sealing temperature is 85° C., the sealing time is 30 min, the pH of the sealing solution is 5, and the aluminum alloy is washed with water after the sealing treatment;
[0072] (5) The aluminum alloy was placed in a sodium hydroxide solution with a mass concentration of 60 g / L, reacted at room temperature for 120 seconds, washed with water, and dried in an oven at 90° C. for 20 minutes.
[0073] Comparative Example 2
[0074] This comparative example provides an aluminum alloy surface treatment process with an anti-fingerprint effect, comprising the steps of:
[0075] (1) placing the aluminum alloy to be processed in a mixture of phosphoric acid and sulfuric acid with a mass concentration of 3:1, reacting at 85° C. for 120 seconds, and then washing with water; then placing the aluminum alloy in 20% hydrochloric acid, reacting at room temperature for 60 seconds, and then washing with water;
[0076] (2) subjecting the aluminum alloy to anodizing treatment, wherein the electrolyte is sulfuric acid with a mass concentration of 200 g / L, the treatment voltage is 14 V, the temperature is 18° C., the treatment time is 50 min, the thickness of the obtained aluminum alloy oxide film is 12 μm, and the anodizing treatment is followed by water washing;
[0077] (3) The aluminum alloy was immersed in sulfuric acid with a mass concentration of 1 g / L for dyeing, the temperature of the sulfuric acid was room temperature, and then washed with water after immersion for 5 minutes;
[0078] (4) placing the aluminum alloy in nickel fluoride with a mass concentration of 12 g / L for sealing treatment, the sealing temperature is 85° C., the sealing time is 30 min, the pH of the sealing solution is 5, and the aluminum alloy is washed with water after the sealing treatment;
[0079] (5) placing the aluminum alloy in a sodium hydroxide solution with a mass concentration of 60 g / L, reacting at room temperature for 120 seconds, washing with water, and drying in an oven at 90° C. for 20 minutes;
[0080] (6) The dried aluminum alloy is subjected to AF coating to obtain an aluminum alloy with an anti-fingerprint effect.
[0081] The aluminum alloys with anti-fingerprint effect obtained by the processes of Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to hydrophobicity test and anti-fingerprint test respectively. The specific test methods are as follows, and the test results are shown in Table 1.
[0082] 1. Hydrophobicity test: tested with a water drop angle tester;
[0083] 2. Anti-fingerprint performance test:
[0084] Marker test: Use a marker to mark the panel, then wipe it off and observe the residual mark.
[0085] Table 1 Performance test results of Examples 1 to 3 and Comparative Examples 1 to 2
[0086]
[0087] Please refer to Table 1 for the test results of Example 1 and Comparative Example 1, specifically see the hydrophobic performance test results. The larger the water drop angle, the stronger the hydrophobicity of the aluminum alloy surface, so its surface anti-fingerprint and anti-fouling effects are more obvious. The water drop angle on the aluminum alloy surface in Example 1 of the present invention is 98°, and the water drop angle on the aluminum alloy surface in Comparative Example 1 is 41°. Combined with the anti-fingerprint performance test, it can be seen that for the marker pen dirt test, Example 1 of the present invention can be wiped clean after 2 wipes, while Comparative Example 1 needs to be wiped 9 times. Therefore, the combination of the two can fully illustrate that the anti-fingerprint aluminum alloy obtained by the anti-fingerprint processing process of the present invention has excellent hydrophobic properties and anti-fingerprint effects.
[0088] By comparing Example 1 with Comparative Example 2, it can be seen that the hydrophobicity and anti-fingerprint performance of Example 1 of the present invention are basically equivalent to those of Comparative Example 2. However, in the process of anti-fingerprint treatment, the present invention does not need to add new AF coating production lines and equipment, and anti-fingerprint treatment can be performed during the anode process. Compared with the process of Comparative Example 2, the anti-fingerprint treatment process of the metal substrate surface of the present invention is simple and easy, and significantly reduces the production cost, and is suitable for industrial production. Specifically, the cost of using the treatment process of Example 1 of the present invention is 2 yuan / pcs; the cost of using the treatment process in Comparative Example 2 is 12 yuan / pcs. Therefore, the production process of the present invention can be greatly reduced in cost compared with the traditional AF coating process.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. Anti-fingerprint treatment process for metal substrate surface, characterized in that: Includes steps: Pre-treating the metal substrate to be processed; The metal substrate is subjected to anodizing treatment; Using dyeing liquid to dye the metal substrate; Using a sealing liquid to perform a pore sealing treatment on the metal substrate; The metal substrate is subjected to anti-fingerprint treatment by using an anti-fingerprint treatment liquid, wherein the anti-fingerprint treatment liquid is an aqueous solution including a hydration accelerator, a buffer, a silicate, a phosphate, apatite, limestone, a borate, aluminate and a wetting agent.
2. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The mass concentration of the anti-fingerprint treatment liquid is 8-20 g / L.
3. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The anti-fingerprint treatment is specifically to immerse the metal substrate in an anti-fingerprint treatment liquid, the temperature of the anti-fingerprint treatment liquid is 90-95° C., the anti-fingerprint treatment time is 15-25 minutes, and the pH of the anti-fingerprint treatment liquid is 5-7.
4. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The pretreatment includes chemical polishing and primary neutralization of the metal substrate.
5. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The thickness of the oxide film obtained by the anodizing treatment of the metal substrate is 12 to 15 μm.
6. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The electrolyte for the anodizing treatment is sulfuric acid, the mass concentration of the sulfuric acid is 200-220 g / L, the temperature of the electrolyte is 10-25° C., the treatment time is 50-60 min, and the treatment voltage is 10-15V.
7. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The dye solution includes at least one of sulfuric acid, phosphoric acid, chromic acid and oxalic acid, and the mass concentration of the dye solution is 0.6-4 g / L.
8. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The sealing treatment is specifically to immerse the metal substrate in a sealing liquid, the mass concentration of the sealing liquid is 12-13 g / L, the temperature of the sealing liquid is 85-95° C., the sealing treatment time is 30-45 min, and the pH of the sealing liquid is 5-7.
9. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: After the anti-fingerprint treatment, the metal substrate is subjected to post-treatment, and the post-treatment includes secondary neutralization, water washing and drying.
10. The anti-fingerprint treatment process for the metal substrate surface according to claim 1, characterized in that: The metal substrate is selected from aluminum or aluminum alloy.