Method and apparatus for manufacturing epitaxial wafer

By using an infrared temperature sensor to control the heater output in the epitaxial growth furnace, the consistency of the epitaxial growth processing conditions of the silicon wafer is ensured, the problem of unstable epitaxial layer quality in multi-station processing is solved, and the stability of the film thickness is achieved. Productivity improvements.

CN118756336APending Publication Date: 2024-10-11SUMCO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410737123.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-11-30
Filing Date
2019-10-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the multi-station processing method, after the epitaxial growth process of the silicon wafer, the quality of the epitaxial layer is unstable, especially between the first and second epitaxial growth processes after the cleaning process, the deviation of the film thickness is relatively large. Large, affecting the quality of the chip.

Method used

By using a non-contact infrared radiation temperature sensor in the epitaxial growth furnace cavity to detect the temperature of the wafer surface, and controlling the heater output to keep it within the specified temperature range, perform multiple epitaxial growth processes continuously and then perform a cleaning process and standby. The time is set so that the heater output variation rate is within the range of ±0.5% to ensure the consistency of the equipment status.

Benefits of technology

It effectively stabilizes the quality of epitaxial wafers, maintains epitaxial growth processing conditions, reduces the film thickness difference after the first and second epitaxial growth processing, and improves productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756336A_ABST
    Figure CN118756336A_ABST
Patent Text Reader

Abstract

Provided are a method and an apparatus for manufacturing an epitaxial wafer capable of stabilizing the quality of the epitaxial wafer in the case of performing a multi-station process. A carrier (16) on which a wafer (W) is placed; a gas supply system (3) for supplying a reaction gas or a purge gas into a chamber (11) of the epitaxial growth furnace; a halogen lamp (15) for heating the interior of the chamber; and an infrared radiation temperature sensor (4) for detecting the temperature of the surface of the wafer. And a controller (5) that controls the output of the heater so that the detected temperature is within a prescribed temperature range and that controls the gas supply system. The controller sets a standby time after the completion of the cleaning process until the first wafer is put into the chamber to a time during which the variation rate of the output of the heater falls within a prescribed range, and prohibits the first wafer from being put into the chamber until the time after the completion of the cleaning process reaches the standby time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method and a device for manufacturing an epitaxial wafer. Background Art

[0002] In the manufacture of silicon epitaxial wafers, in addition to batch epitaxial growth devices that perform epitaxial growth processing on multiple silicon wafers at the same time, single-wafer epitaxial growth devices that can also handle large-diameter silicon wafers are used. This single-wafer epitaxial growth device heats the wafer placed on a carrier to a high temperature in the chamber of the epitaxial growth furnace and rotates it, introduces silicon reaction gas through hydrogen carriers, and grows a silicon thin film on the surface of the wafer. As reaction gases for silicon epitaxial growth, monosilane gas (SiH4), chlorosilane gas (SiH2Cl2, SiHCl3), etc. are used.

[0003] During the reaction, products of material gases such as amorphous silicon and chlorosilane polymers adhere to and deposit on the walls and carriers in the chamber. If the deposits are peeled off during the epitaxial growth process and adhere to the wafer, they may be mixed into the thin film of the wafer as impurities and the quality of the wafer may be reduced. Therefore, during the epitaxial growth process of the wafers performed sequentially, a cleaning process is performed by supplying a cleaning gas such as hydrogen chloride gas and chlorine trifluoride gas into the chamber to remove the deposits. In addition, if the cleaning process is performed for each epitaxial growth process of each wafer, the productivity is reduced. Therefore, a so-called multi-station processing method is sometimes performed in which a cleaning process in the chamber is performed once after a plurality of epitaxial growth processes are performed in succession (Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-26776. Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, based on the equipment structure, the quality of the silicon epitaxial thin film on the surface of the silicon wafer is further improved in quality and precision. If the above-mentioned multi-station processing method is performed, the quality (e.g., film thickness) of the epitaxial layer obtained by the first epitaxial growth process after the cleaning process in the chamber and the quality (e.g., film thickness) of the epitaxial layer obtained by the second and subsequent epitaxial growth processes will deviate, resulting in a problem of unstable quality.

[0009] The problem to be solved by the present invention is to provide a method and apparatus for manufacturing epitaxial wafers, which can stabilize the quality of epitaxial wafers and keep the equipment conditions such as epitaxial growth processing conditions constant in a multi-station process in which a cleaning process in the chamber is performed after multiple consecutive epitaxial growth processes.

[0010] Means used to solve problems

[0011] The present invention solves the above-mentioned problems by a method for manufacturing an epitaxial wafer, wherein:

[0012] The wafers are placed one at a time into the chamber of the epitaxial growth furnace.

[0013] The temperature of the surface of the wafer is measured by a non-contact temperature sensor, and the output of the heater in the chamber is controlled so that the detected temperature is within a specified temperature range.

[0014] Supplying reaction gas into the aforementioned chamber, while allowing the epitaxial layer to grow in the vapor phase on the surface of the wafer,

[0015] After the epitaxial growth process is performed multiple times in succession, a cleaning process is performed to remove the deposits deposited in the aforementioned chamber.

[0016] in,

[0017] The standby time from the completion of the cleaning process until the first wafer is loaded into the chamber is set to a time when the variation rate of the output of the heater during the multiple epitaxial growth processes falls within a predetermined range, and the epitaxial growth process is performed.

[0018] In the present invention, the waiting time is more preferably a time during which the variation rate of the output of the heater in the first epitaxial growth process after the cleaning process and the output of the heater in the second and subsequent epitaxial growth processes falls within a range of ±0.5%.

[0019] In the present invention, a quartz upper dome is provided on the upper portion of the epitaxial growth furnace, and the non-contact temperature sensor can be configured to detect the temperature of the surface of the wafer from outside the epitaxial growth furnace through the quartz dome.

[0020] In the present invention, the non-contact temperature sensor is, for example, an infrared radiation temperature sensor.

[0021] In addition, the present invention solves the above-mentioned problems by means of an epitaxial wafer manufacturing device, the epitaxial wafer manufacturing device comprising:

[0022] A monolithic epitaxial growth furnace having at least a quartz upper dome,

[0023] A carrier for mounting a chip,

[0024] A gas supply system for supplying reaction gas or cleaning gas into the chamber of the epitaxial growth furnace,

[0025] Heating the heater in the aforementioned cavity,

[0026] an infrared radiation temperature sensor for detecting the temperature of the surface of the wafer from outside the chamber through the upper quartz dome, and

[0027] a controller for controlling the output of the heater so that the temperature detected by the infrared radiation temperature sensor is within a predetermined temperature range and for controlling the gas supply system,

[0028] In the epitaxial wafer manufacturing apparatus,

[0029] The aforementioned controller is,

[0030] controlling the gas supply system so as to perform a cleaning process to remove the deposits deposited in the chamber after performing multiple epitaxial growth processes in succession,

[0031] The waiting time from the completion of the cleaning process to the first wafer being introduced into the chamber is set to a time when the variation rate of the output of the heater during the multiple epitaxial growth processes falls within a predetermined range.

[0032] Until the time after the completion of the cleaning process reaches the standby time, the first input of the wafer is prohibited. If the time after the completion of the cleaning process exceeds the standby time, the first input of the wafer is allowed.

[0033] Effects of the Invention

[0034] According to the present invention, the standby time from the completion of the cleaning process to the placement of the first wafer into the chamber is set to a time during which the rate of change of the heater output falls within a specified range when multiple epitaxial growth processes are performed. Therefore, in the case of multi-station processing, the quality of the epitaxial wafer can be stabilized and the equipment status such as the epitaxial growth processing conditions can be kept constant. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a block diagram showing one embodiment of an epitaxial wafer manufacturing apparatus according to the present invention.

[0036] Figure 2 This is a diagram showing the temperature transition in the processing steps (multi-station processing) of one embodiment of the method for producing an epitaxial wafer of the present invention.

[0037] Figure 3 This is a diagram showing the results of a confirmation experiment in which the relative film thickness of the epitaxial layer was measured when the standby time was set to 0 to 300 seconds.

[0038] Figure 4 This is a diagram showing the results of a confirmation experiment in which the relative temperature of the silicon wafer surface was measured when the waiting time was set to 0 to 300 seconds.

[0039] Figure 5 This is a diagram showing the results of a confirmation experiment in which the relative output of a halogen lamp was measured when the standby time was set to 0 to 300 seconds.

[0040] Figure 6 This is a diagram showing the results of a confirmation experiment in which the relative temperature of the upper dome was measured when the waiting time was set to 0 to 300 seconds.

[0041] Figure 7 This is a diagram showing the results of measuring the relationship between the waiting time and the relative temperature of the upper dome during the first to third epitaxial growth processes. DETAILED DESCRIPTION

[0042] Hereinafter, embodiments of the present invention will be described based on the drawings. Figure 1 This is a block diagram showing one embodiment of an epitaxial wafer manufacturing apparatus A according to the present invention.

[0043] like Figure 1 As shown in FIG. 1 , the epitaxial growth furnace 1 has a chamber 11 for forming an epitaxial layer on a silicon wafer W. The chamber 11 includes an upper dome 12, a lower dome 13, and a dome mounting body 14 that fixes and supports the upper dome 12 and the lower dome 13. The upper dome 12 and the lower dome 13 are made of a transparent material such as quartz, and a plurality of halogen lamps 15 are arranged above and below the epitaxial growth furnace 1 to heat a carrier 16 and a silicon wafer W placed on the carrier 16. The plurality of halogen lamps 15 are as shown in FIG. Figure 1 The halogen lamps 15 are arranged in a ring shape above and below the epitaxial growth furnace 1 as shown in part in FIG. 1 , and the output of each halogen lamp 15 is controlled by a drive unit 24 which is controlled by a control signal from a controller 5. The halogen lamps 15 correspond to an example of a heater according to the present invention.

[0044] The epitaxial growth furnace 1 further has a carrier 16 that divides the chamber 11 into an upper space 11a and a lower space 11b. The carrier 16 is in the shape of a circular plate, and is fixed to the outer periphery of its lower surface by means of a support arm 18 connected to a carrier rotating shaft 17, and rotates by rotating the carrier rotating shaft 17. In addition, a total of three through holes are formed in the outer periphery of the carrier 16 at intervals of 120 degrees toward its circumferential direction. In each through hole, a lifting pin 19 for lifting and lowering the silicon wafer W is loosely inserted. The lifting and lowering of the lifting pin 19 is performed by a lifting arm 20. The rotation drive of these carrier rotating shafts 17 and the lifting and lowering drive of the lifting arm 20 are performed by a driving unit 21, and the driving unit 21 is controlled by a command signal from a controller 5.

[0045] In addition, the material of the carrier 16 can be formed of SiC on the surface to prevent impurities from being mixed in when forming the epitaxial layer, and the material of the coated material is not particularly limited. Generally, a material having a silicon carbide (SiC) film coated on the surface of a carbon substrate is often used, but the entire carrier 16 can also be formed of SiC.

[0046] A gas supply port 22 and a gas exhaust port 23 are arranged opposite to each other at a height position of the dome mounting body 14 that is substantially equal to the upper surface of the susceptor 16. During the epitaxial growth process, a mixed gas is supplied from the gas supply port 22 to the inside of the chamber 11 in parallel (horizontally) with respect to the upper surface of the silicon wafer W. The mixed gas is prepared by diluting a silicon reaction gas such as trichlorosilane (SiHCl3) with a carrier gas such as hydrogen (H2 gas) and, as required, mixing a small amount of a dopant such as diborane (B2H6) therein. The supplied mixed gas passes through the surface of the silicon wafer W to grow an epitaxial layer, and is then discharged from the gas exhaust port 23 to the outside of the chamber 11.

[0047] On the other hand, during the cleaning process, while the silicon wafer W is transported out of the chamber 11 by a wafer transport mechanism (not shown) through a gate valve (not shown), a cleaning gas such as hydrogen chloride (HCl) gas is introduced into the chamber 11 from the gas supply port 22 according to a predetermined procedure and discharged from the gas discharge port 23. Thus, deposits attached to the susceptor 16 and the like are removed by dry etching. Such supply / discharge of the reaction gas and the cleaning gas is performed by the gas supply system 3, and the gas supply system 3 is controlled by a control signal from the controller 5.

[0048] In the central part above the epitaxial growth furnace 1, an infrared radiation temperature sensor 4 is provided, which optically detects the amount of infrared radiation emitted from the silicon wafer W through the upper dome 12, thereby detecting the surface temperature of the silicon wafer W in a non-contact manner. In addition, when an object radiates infrared radiation from its surface and the temperature of the object surface is determined according to the amount of infrared radiation, infrared radiation has the characteristic of transmitting energy in space. The infrared radiation temperature sensor 4 optically reads the infrared radiation transmitted in the space and measures the temperature without bringing the object into contact with the sensor. The detection signal detected by the infrared radiation temperature sensor 4 is read out to the controller 5, and the controller performs, for example, PID control (Proportional Integral Differential Controller) on the output of the halogen lamp 15 by the drive unit 24 according to the surface temperature of the silicon wafer W thus detected. That is, during the epitaxial growth process, the drive unit 24 is controlled to control the output of each halogen lamp 15 so that the surface temperature of the silicon wafer W is within a specified temperature range. For example, the following control is performed: when the detected surface temperature of the silicon wafer W is lower than a predetermined temperature range, the output of the halogen lamp 15 is increased, and when it is higher than the predetermined temperature range, the output of the halogen lamp 15 is reduced.

[0049] The controller 5 is composed of a computer having a CPU, ROM, and RAM, and controls the wafer transport mechanism and gate valve, the gas supply system 3, the driver 24 of the halogen lamp 15, and the driver 21 of the carrier 16, which are not shown in the figure. Therefore, a processing program (hereinafter also referred to as a process recipe) for the device related to the process sequence and control parameters (control target values ​​such as temperature, pressure, type of gas and gas flow rate, time, etc.) for manufacturing epitaxial wafers, and a processing program (hereinafter also referred to as a cleaning recipe) related to the process sequence and control parameters for cleaning the epitaxial growth furnace and the exhaust pipe are established. During the epitaxial growth process, the process recipe is read to control the wafer transport mechanism, the gate valve, the gas supply system 3, the driver 24 of the halogen lamp 15, and the driver 21 of the carrier 16. During the cleaning process, the cleaning recipe is read to control the wafer transport mechanism, the gate valve, the gas supply system 3, the driver 24 of the halogen lamp 15, and the driver 21 of the carrier 16.

[0050] In the epitaxial wafer manufacturing apparatus A of the present embodiment, a so-called multi-station process is performed. The multi-station process refers to an operation method in which a cleaning process is performed once to remove the deposits deposited in the chamber 11 after a plurality of epitaxial manufacturing processes are performed continuously. An example of the multi-station process is shown in FIG. Figure 2 In the example shown in the figure, after three epitaxial growth processes, namely, the first, second and third epitaxial growth processes are continuously performed, a cleaning process is performed once, and this process is repeated.

[0051] On one side of the epitaxial growth furnace 1, a gate valve and a loading chamber (not shown) are provided. The silicon wafer W before the epitaxial growth process is put into the chamber 11 from the loading chamber through the gate valve, and the silicon wafer W after the epitaxial growth process is taken out of the loading chamber through the gate valve. That is, the gate valve (not shown) is opened, and the silicon epitaxial wafer W after the film formation is transported out of the chamber 11 through the gate valve by the wafer transport mechanism (not shown). In addition, the gate valve is closed, the drive unit 24 is controlled to control the output of the halogen lamp 15, the temperature in the chamber 11 of the epitaxial growth furnace 1 is raised to a predetermined temperature, and the gas supply system 3 is controlled to supply a cleaning gas such as hydrogen chloride gas and chlorine trifluoride gas into the chamber 11 for a predetermined time to remove the deposit (cleaning process). Next, the halogen lamp 15 is turned off, and the chamber 11 of the epitaxial growth furnace 1 is purged with hydrogen gas and cooled. Here, the temperature rise to the aforementioned predetermined temperature (cleaning process temperature) is preferably 1130°C to 1250°C, and the higher the temperature, the shorter the supply time of the cleaning gas. The predetermined time for supplying the cleaning gas is set to a time sufficient to remove the silicon deposits deposited in the chamber and the silicon deposits attached to the inner wall of the quartz upper dome 12. The cleaning treatment temperature is preferably set higher than the temperature of the epitaxial growth treatment described later. Thus, the silicon deposits can be cleaned in a short time.

[0052] When the cleaning process is finished, after the silicon wafer W before film formation is put into the chamber 11, the drive unit 24 is controlled to control the output of the halogen lamp 15, the internal temperature of the chamber 11 is raised to a predetermined temperature between 1000 and 1200°C, and the gas supply system 3 is controlled to supply monosilane gas (SiH4), chlorosilane gas (SiH2Cl2, SiHCl3) and other reaction gases together with carrier gases such as hydrogen or inert gas into the chamber 11 for a predetermined time, and an epitaxial layer is formed on the surface of the silicon wafer W (epitaxial growth process). Next, the halogen lamp 15 is turned off, and the chamber 11 is purged with hydrogen and cooled, and the silicon epitaxial wafer W after film formation is taken out of the chamber 11, and the next silicon wafer W before film formation is put in, and the epitaxial growth process is performed in the same manner as the first epitaxial growth process. After repeating this epitaxial growth process three times, the above-mentioned cleaning process is performed.

[0053] Here, the inventors of the present application have investigated and found that, when the cleaning process temperature is set higher than the epitaxial growth process temperature, the film thickness of the formed silicon epitaxial wafer W varies depending on the time between the completion of the cleaning process and the first epitaxial growth process. Figure 31 is a diagram showing the results of a confirmation experiment, wherein the cleaning process temperature is set to be higher than the epitaxial growth process temperature, and the manufacturing device A of the same epitaxial wafer is used to perform the cleaning process and three epitaxial growth processes under the same conditions. When the time between the end of the cleaning process and the first epitaxial growth process (hereinafter referred to as the standby time, which is also the cooling time of the chamber 11) is set to 0 seconds, 60 seconds, 120 seconds, 180 seconds, 240 seconds and 300 seconds, the relative film thickness of the center of the wafer of the epitaxial layer is measured. In addition, the experiment is performed when the epitaxial thickness is 4 μm. According to the results of the confirmation experiment, the increase or decrease rate of the second film thickness and the third film thickness is an increase or decrease of less than 0.2% at any level, and there is almost no difference, but the increase or decrease rate of the first film thickness and the film thickness after the second time is reduced by a value of more than 0.5%, which is so large that it cannot be ignored. In addition, the shorter the standby time, the thicker the first film thickness, and the longer the standby time, the thinner the first film thickness. Therefore, it can be seen that as long as an appropriate time is selected, the increase / decrease rate of the film thickness after the first reduction and the second reduction becomes smaller. In addition, the increase / decrease rate is set to a value defined by ((absolute value of (n+1)th value [μm]-nth value [μm])) / nth value [μm]×100[%] (where n is a value greater than 1).

[0054] The film thickness of the epitaxial layer during the epitaxial growth process is such that the higher the surface temperature of the silicon wafer W, the thicker it is. Therefore, the controller 5 performs PID control on the output of the halogen lamp 15 according to the surface temperature of the silicon wafer W detected by the infrared radiation temperature sensor 4, and controls it in such a way that the surface temperature of the silicon wafer W becomes within a specified temperature range. Figure 4 4 is a graph showing the measurement results of the relative temperature of the surface of the silicon wafer W detected by the infrared radiation temperature sensor 4 in the above-mentioned confirmation experiment. According to the results, the surface temperature of the silicon wafer W was maintained within the prescribed temperature range from the first to the third time. Although the surface temperature of the silicon wafer W was maintained within the prescribed temperature range, Figure 3 As shown, the difference between the first film thickness and the second and subsequent film thicknesses becomes larger. In addition, the variation of the surface temperature of the silicon wafer W is preferably less than ±1 degree.

[0055] in addition, Figure 5 This is a diagram showing the results of measuring the change in the relative output of the halogen lamp 15 in the above-mentioned confirmation experiment. According to the results, the output of the halogen lamp 15 is controlled to be smaller as the waiting time is shorter, and the output of the halogen lamp 15 is controlled to be larger as the waiting time is longer. It is believed that this is because the internal temperature of the epitaxial growth furnace 1 is maintained at a high state as the waiting time is shorter, so the output of the halogen lamp 15 is controlled to be smaller, and the internal temperature of the epitaxial growth furnace 1 is lowered as the waiting time is longer, so the output of the halogen lamp 15 is controlled to be larger.

[0056] However, if Figure 4 and Figure 5 As shown in FIG. 1 , although the output of the halogen lamp 15 is PID-controlled so that the surface temperature of the silicon wafer W detected by the infrared radiation temperature sensor 4 is within a predetermined temperature range, Figure 3 As shown in the figure, the first film thickness also deviates, and it is presumed that there is some other reason. Therefore, the inventors focused on the temperature of the upper dome 12, and used an infrared radiation temperature sensor that can measure the quartz surface (not shown in the figure) to measure the temperature of the upper dome 12 in the above confirmation experiment during the epitaxial growth process. The results are shown in Figure 6 . Figure 6 The figure shows the results of a confirmation experiment in which the relative temperature of the upper dome 12 was measured when the waiting time was set to 0 seconds, 60 seconds, 120 seconds, 180 seconds, 240 seconds, and 300 seconds under the condition that the cleaning process temperature was set higher than the temperature of the epitaxial growth process. According to the results, the shorter the waiting time, the higher the temperature of the upper dome 12, and the longer the waiting time, the lower the temperature of the upper dome 12. That is, the overall Figure 6 The results and Figure 3 As a result, the higher the temperature of the upper dome 12, the thicker the first film thickness is, and the lower the temperature of the upper dome 12, the thinner the first film thickness is, and the relationship between temperature and film thickness is integrated. Therefore, it is inferred that if the temperature of the upper dome 12 is controlled, the film thickness can be suppressed. Figure 3 The first film thickness deviation is shown. In addition, the infrared radiation temperature sensor capable of measuring the quartz surface is set to a different measurement wavelength from the infrared radiation temperature sensor 4. Specifically, the detection range of the infrared radiation temperature sensor 4 is 0.9 to 0.97 μm, while 4.8 to 5.2 μm is used.

[0057] Figure 7 This is a graph showing the results of measuring the relationship between the standby time and the relative temperature of the upper dome 12 from the first to the third epitaxial growth process when the manufacturing apparatus A using the same epitaxial wafer used in the above confirmation experiment was used to perform the cleaning process and the epitaxial growth process three times under the same conditions. According to the results, the temperature of the upper dome 12 deviated only in the case of the first epitaxial growth process, and the temperature of the upper dome 12 in the second and third epitaxial growth processes was almost constant. Therefore, it is speculated that if the temperature of the upper dome 12 in the first epitaxial growth process, that is, the standby time after the cleaning process, is mainly controlled, the relative temperature of the upper dome 12 can be suppressed. Figure 3 Furthermore, the waiting time may be set so that the temperature of the upper dome 12 is less than ±10 degrees, preferably less than ±5 degrees, during the entire epitaxial growth process using the infrared radiation temperature sensor capable of measuring the quartz surface.

[0058] Such a deviation in the film thickness after the first epitaxial growth process due to the temperature of the upper dome 12 can be inferred to be caused by the following reasons. That is, it can be inferred that when the standby time is short, the output of the halogen lamp 15 is suppressed by PID control, but the temperature of the upper dome 12 is high, and the actual surface temperature of the silicon wafer W is higher than the temperature detected by the infrared radiation temperature sensor 4 due to the radiation heat from the upper dome 12. Therefore, the actual film thickness is thicker than the target film thickness. In contrast, when the standby time is long, the temperature of the upper dome 12 is sufficiently reduced, and the influence of the radiation heat from the upper dome 12 is extremely small. Therefore, it can be inferred that the deviation between the actual surface temperature of the silicon wafer W and the surface temperature of the silicon wafer W detected by the infrared radiation temperature sensor 4 becomes smaller, and becomes the surface temperature corresponding to the output of the halogen lamp 15 controlled by PID, and thus becomes the target film thickness.

[0059] Through the above confirmation experiment, in the epitaxial wafer manufacturing apparatus A of the present embodiment, it is not necessary to prepare a plurality of process recipes for epitaxial growth processing, and the waiting time can be reduced by setting the waiting time to a unique value of the epitaxial wafer manufacturing apparatus A. Figure 3 The deviation of the film thickness after the first epitaxial growth process and the film thickness after the second and subsequent epitaxial growth processes shown in the figure. The waiting time is expected to be different according to the individual differences of the manufacturing device A of the epitaxial wafer and the conditions of the process recipe. Therefore, for each manufacturing device A of the epitaxial wafer and each process recipe, the film thickness of the epitaxial layer during the first epitaxial growth process and the film thickness during the second and subsequent epitaxial growth processes under the condition of setting multiple waiting times are obtained in advance through experiments or computer simulations, and the range of the waiting time when the increase and decrease rate of these film thicknesses falls within the prescribed allowable range is obtained in advance. In addition, during actual production, the range of the waiting time obtained in this way is used to control by the controller 5 so that when the time after the cleaning process is completed is within the range of the waiting time, the input of the next wafer is allowed, and when the time after the cleaning process is completed is not within the range of the waiting time, the input of the next wafer is prohibited. Furthermore, the upper dome temperature can also be obtained in advance in the same manner, and the range of the waiting time when the upper dome temperature falls within the prescribed allowable range is obtained. By stabilizing the temperature of the upper dome of quartz in the equipment state, the output of the halogen lamp 15 can be further stabilized. The permission and prohibition of the next wafer loading can be performed by controlling the wafer transport mechanism (not shown) by the controller 5. The predetermined range of the increase or decrease rate is preferably less than ±0.5%, more preferably less than ±0.2%. Here, ± indicates the increase and decrease direction.

[0060] As described above, the film thickness during the first epitaxial growth process and the film thickness during the second and subsequent epitaxial growth processes in the multi-station process are strongly correlated with the temperature of the upper dome 12, so it can be Figure 6 As shown in FIG. 1 , the temperature of the upper dome 12 is measured for a plurality of waiting times, and the range of waiting time in which the variation rate of the temperature of the upper dome 12 during the first epitaxial growth process and the temperature of the upper dome 12 during the second and subsequent epitaxial growth processes falls within a predetermined range is obtained in advance. Alternatively, the film thickness during the first epitaxial growth process and the film thickness during the second and subsequent epitaxial growth processes in the multi-station process also have a strong correlation with the output of the halogen lamp 15, so it is also possible to Figure 5 As shown, the output of the halogen lamp 15 is measured for a plurality of waiting times, and a range of waiting times in which the variation rate between the output of the halogen lamp 15 in the first epitaxial growth process and the output of the halogen lamp 15 in the second and subsequent epitaxial growth processes falls within a predetermined range is obtained in advance.

[0061] Figure 5 The output variation rate of the halogen lamp 15 shown is Figure 3 The results of the increase and decrease rate of the epitaxial film shown are shown in Table 1. In addition, the variation rate of the output of the halogen lamp 15 is defined as (the output of the halogen lamp 15 during the second and subsequent epitaxial growth processes - the output of the halogen lamp 15 during the first epitaxial growth process) ÷ (the output of the halogen lamp 15 during the first epitaxial growth process). In addition, the increase and decrease rate of the film thickness of the epitaxial layer is based on the above definition, and the increase and decrease rate of the film thickness between the first and second times is shown in Table 1.

[0062]

Table 1

[0063] Standby time Halogen lamp output fluctuation rate Epitaxial film thickness increase / decrease rate 0 seconds 1.64% 0.55% 60 seconds 1.25% 0.42% 120 seconds 0.50% 0.18% 180 seconds 0.25% 0.03% 240 seconds -0.49% 0.13% 300 seconds -0.98% 0.16% .

[0064] Figure 5 In the results of the epitaxial wafer manufacturing device A shown in the figure, the variation rate is 1.64% when the standby time is 0 seconds, 1.25% when the standby time is 60 seconds, 0.50% when the standby time is 120 seconds, 0.25% when the standby time is 180 seconds, -0.49% when the standby time is 240 seconds, and -0.98% when the standby time is 300 seconds. Figure 3The increase and decrease rate of the first and second film thicknesses shown is 0.55% when the standby time is 0 seconds, 0.42% when the standby time is 60 seconds, 0.18% when the standby time is 120 seconds, 0.03% when the standby time is 180 seconds, 0.13% when the standby time is 240 seconds, and 0.16% when the standby time is 300 seconds. If the allowable range of the increase and decrease rate of the film thickness of the epitaxial layer is set to less than 0.20%, the deviation of the film thickness is suppressed when the variation rate of the output of the halogen lamp 15 is within the range of ±0.98%.

[0065] DESCRIPTION OF SYMBOLS A ... manufacturing device for epitaxial wafer 1 ... epitaxial growth furnace

[0066] 11…Cavity

[0067] 12…Upper side vault

[0068] 13…Lower side vault

[0069] 14…Arch mounting body

[0070] 15…Halogen lamp

[0071] 16…Carrier

[0072] 16a…Periphery

[0073] 17…Carrier rotation axis

[0074] 18…Support arm

[0075] 19…Lifting pin

[0076] 20…Lifting arm

[0077] 21…Driver

[0078] 22…Gas supply port

[0079] 23…Gas exhaust port

[0080] 24…Driver

[0081] 3…Gas supply system

[0082] 4…Infrared radiation temperature sensor 5…Controller

[0083] W…Silicon wafer.

Claims

1. A method for manufacturing an epitaxial wafer, Wafers are placed one at a time into a chamber of an epitaxial growth furnace having a quartz upper dome at the top. The surface temperature of the wafer is measured by a non-contact temperature sensor, and the output of a heater for heating the chamber is controlled so that the measured temperature falls within a predetermined temperature range. Supplying a reaction gas into the chamber, while causing a vapor phase growth of an epitaxial layer on the surface of the wafer, After the epitaxial growth process is performed multiple times in succession, a cleaning process is performed to remove the deposits deposited in the aforementioned chamber. In the method for manufacturing the epitaxial wafer, Regarding the waiting time from the completion of the aforementioned cleaning treatment until the first chip is put into the aforementioned chamber, the range of the aforementioned waiting time in which the rate of change of the temperature of the aforementioned upper dome when the first epitaxial growth treatment is carried out after the completion of the aforementioned cleaning treatment and the temperature of the aforementioned upper dome when the second and subsequent epitaxial growth treatments are carried out fall within the specified range is calculated in advance, the waiting time from the completion of the aforementioned cleaning treatment until the first chip is put into the aforementioned chamber is set to the aforementioned waiting time falling within the specified range, and the epitaxial growth treatment is carried out.

2. The method for manufacturing an epitaxial wafer according to claim 1, It is characterized in that The standby time is a time during which the variation rate of the output of the heater when the first epitaxial growth process is performed after the cleaning process is completed and the output of the heater when the second and subsequent epitaxial growth processes are performed falls within a range of ±0.5%.

3. The method for manufacturing an epitaxial wafer according to claim 1 or 2, It is characterized in that The non-contact temperature sensor detects the temperature of the surface of the wafer from the outside of the epitaxial growth furnace through the upper dome made of quartz.

4. The method for producing an epitaxial wafer according to claim 1 or 2, It is characterized in that The non-contact temperature sensor is an infrared radiation temperature sensor.

5. An epitaxial wafer manufacturing device, comprising: A monolithic epitaxial growth furnace having at least a quartz upper dome, A carrier for mounting a chip, A gas supply system for supplying reaction gas or cleaning gas into the chamber of the epitaxial growth furnace, A heater for heating the cavity, an infrared radiation temperature sensor for detecting the temperature of the upper dome and detecting the temperature of the surface of the wafer from outside the chamber through the upper dome, and a controller that controls the output of the heater so that the temperature detected by the infrared radiation temperature sensor becomes within a predetermined temperature range and controls the gas supply system, In the epitaxial wafer manufacturing apparatus, The aforementioned controller is, Regarding the waiting time from the completion of the cleaning process until the first wafer is introduced into the chamber, a range of the waiting time in which the rate of change of the temperature of the upper dome when the first epitaxial growth process is performed after the cleaning process is completed and the temperature of the upper dome when the second and subsequent epitaxial growth processes are performed falls within a predetermined range is calculated and stored in advance, The gas supply system is controlled so that a cleaning process is performed to remove the deposits deposited in the chamber after the epitaxial growth process is performed multiple times in succession. The waiting time from the completion of the cleaning process until the first wafer is placed in the chamber is set to the waiting time falling within the prescribed range. Until the time after the completion of the cleaning process reaches the standby time, the first wafer input is prohibited. If the time after the completion of the cleaning process exceeds the standby time, the first wafer input is allowed.