High-color-fastness regenerated environment-friendly fabric and preparation method thereof
By adding the steps of setting and drying and reducing the number of soapings in the production process of recycled environmentally friendly fabrics, the problem of insufficient color fastness of dark series fabrics is solved, dyeing efficiency and stability are improved, production costs are reduced, and consumer satisfaction is satisfied demand and promote environmental protection.
Patent Information
- Application Number
- CN202410993443.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
When dyeing recycled environmentally friendly fabrics, the color fastness of dark series colors is poor. There are many dyes attached to the surface, making it difficult to meet the standards for wearing and use. In addition, traditional processes increase energy consumption and sewage costs.
Through the steps of front processing, dyeing, washing, setting drying, soaping and post-processing of recycled environmentally friendly yarn fabrics, the dyes are ensured to be fully fixed and the color fastness is increased, especially for dark series fabrics, soaping The number of times is reduced, which reduces energy and resource consumption.
It improves the color fastness of recycled environmentally friendly fabrics, has good stability, reduces production costs, meets consumer requirements for fabrics, and saves energy resources.
Smart Images

Figure BDA0004959482570000061 
Figure BDA0004959482570000081 
Figure BDA0004959482570000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabric production and processing, and in particular to a high color fastness recycled environmentally friendly fabric and a preparation method thereof. Background Art
[0002] Polyester fabric is a kind of chemical fiber clothing fabric commonly used in daily life. Its biggest advantage is its good wrinkle resistance and shape retention. Therefore, it is suitable for outerwear, various bags, tents and other outdoor products. In recent years, with the deepening of the concept of recycling and environmental protection, recycled environmentally friendly fabrics have emerged. The raw materials of recycled environmentally friendly fabrics are taken from waste plastic bottles and waste clothes, and processed into recycled environmentally friendly fabrics through multiple processes. Compared with original yarns, the dark series colors of recycled environmentally friendly yarns, such as black, dark navy blue, and dark coffee, have poor dye absorption performance, more dyes attached to the surface, and the washing fastness, perspiration fastness, water fastness and friction fastness do not meet the requirements of wearing and use. In order to improve color fastness, the following two processes are generally adopted for improvement: 1. Reduction cleaning treatment is performed, but the color fastness of the fabric after reduction cleaning treatment is unstable. Sometimes it can reach level 3-4 (the national standard is level 3-4), but in many cases it is only level 2-3 or level 3, which directly leads to the fading of the fabric during wearing and use, and cannot meet the use requirements of consumers; 2. Use imported high-fastness dyes for dyeing, but its production cost will increase significantly, which is not conducive to promotion and use. Summary of the invention
[0003] The purpose of the present invention is to provide a recycled environmentally friendly fabric with high color fastness and a preparation method thereof. The recycled environmentally friendly fabric prepared by the method of the present invention has high color fastness, good color fastness stability and low cost.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a method for preparing a recycled environmentally friendly fabric with high color fastness, comprising the following steps:
[0006] Providing grey fabric, wherein the grey fabric is woven from recycled environmentally friendly yarn;
[0007] The grey cloth is sequentially subjected to pre-treatment, dyeing, washing, shaping and drying, soaping and post-treatment to obtain the recycled environmentally friendly fabric with high color fastness.
[0008] Preferably, the regenerated environmentally friendly yarn includes regenerated polyester yarn or regenerated nylon yarn.
[0009] Preferably, the front-end treatment includes barrel matching, sewing and rolling, and flattening in sequence; the conditions for the flattening include: a temperature of 80-90°C and a vehicle speed of 50-60 yards per hour; based on 2500 meters of grey cloth, the mass of the alkaline reagent used for the flattening is 8kg.
[0010] Preferably, the dyeing conditions include: a holding temperature of 130° C., a holding time of 3 hours, a time required to uniformly increase the temperature from room temperature to the holding temperature of 1 hour, and a time required to uniformly decrease the temperature from the holding temperature to 60° C. of 1 hour.
[0011] Preferably, the recycled environmentally friendly fabric with high color fastness includes dark series fabrics or light series fabrics; the colors of the dark series fabrics include black, dark navy blue, dark coffee, dark red or dark green; the colors of the light series fabrics include white, natural white, off-white or beige.
[0012] Preferably, when the recycled environmentally friendly fabric with high color fastness is a dark series fabric, the number of times of washing with water and washing with soap is independently 2 to 3 times; when the recycled environmentally friendly fabric with high color fastness is a light series fabric, the number of times of washing with water and washing with soap is both 1 time.
[0013] Preferably, the time for each soap washing is 30 minutes; based on 2500 meters of grey cloth, the mass of the alkaline reagent used for each soap washing is 20 kg.
[0014] Preferably, the conditions for shaping and drying include: a temperature of 170° C. and a vehicle speed of 60 yards per hour.
[0015] Preferably, the post-processing includes dehydration, opening the width and secondary shaping in sequence; the conditions of the secondary shaping include: temperature of 170°C and vehicle speed of 60 yards per hour; the secondary shaping is carried out in the presence of citric acid and antistatic solvent, based on 2500 meters of grey cloth, the amount of citric acid used is 12 kg, and the amount of antistatic solvent used is 5 kg.
[0016] The present invention provides a recycled environmentally friendly fabric with high color fastness prepared by the preparation method described in the above technical scheme.
[0017] The present invention provides a method for preparing a recycled environmentally friendly fabric with high color fastness, comprising the following steps: providing a grey fabric, the grey fabric being woven from recycled environmentally friendly yarn; sequentially performing pre-treatment, dyeing, washing, shaping and drying, soaping and post-treatment on the grey fabric to obtain the recycled environmentally friendly fabric with high color fastness. The present invention adds a shaping and drying step after dyeing and washing, thereby ensuring that the dye can be fully fixed on the fabric, and then after subsequent soaping and post-treatment, the dyeing color fastness is more stable, greatly improving the dyeing color fastness, and is particularly suitable for recycled environmentally friendly fabrics of dark series (colors such as black, dark navy blue, dark coffee, dark red or dark green), thereby meeting the wearing and use requirements of consumers. In the traditional process, soaping is performed 6 to 7 times directly after washing to clean the cloth surface to remove excess dyes, but no matter how many times the soaping is performed, there are still some residual dyes attached to the surface of the cloth, so the color fastness after dyeing is unstable, not only failing to meet the color fastness standard, but also consuming a large amount of water, electricity or steam and other resources, and increasing the sewage discharge cost. The method of the present invention not only improves color fastness, but also greatly improves dyeing efficiency (for example, dark series recycled environmentally friendly fabrics only need to be soaped 2 to 3 times), reduces energy consumption, saves energy resources, and is more environmentally friendly. The results of the embodiment show that the method of the present invention improves the color fastness of dark series recycled environmentally friendly fabrics to the 3-4 level standard specified by the national standard, and greatly reduces the production cost, which is more conducive to promotion and use. DETAILED DESCRIPTION
[0018] The present invention provides a method for preparing a recycled environmentally friendly fabric with high color fastness, comprising the following steps:
[0019] Providing grey fabric, wherein the grey fabric is woven from recycled environmentally friendly yarn;
[0020] The grey cloth is sequentially subjected to pre-treatment, dyeing, washing, shaping and drying, soaping and post-treatment to obtain the recycled environmentally friendly fabric with high color fastness.
[0021] In the present invention, unless otherwise specified, the raw materials and reagents used are commercially available products well known to those skilled in the art.
[0022] The present invention provides a grey cloth, which is woven from recycled environmentally friendly yarn. In the present invention, the recycled environmentally friendly yarn preferably includes regenerated polyester yarn or regenerated nylon yarn, more preferably regenerated polyester yarn; in an embodiment of the present invention, the regenerated polyester yarn used is specifically a regenerated polyester yarn produced by Zhejiang Jiaren New Materials Co., Ltd., and the model is 75D / 72F DTY low-elastic yarn or 66D / 36F FDY filament. In the present invention, the organizational structure of the grey cloth preferably includes plain or twill, and the twill is specifically 1 / 2 twill or 1 / 3 twill. The present invention preferably performs warping, sizing, beaming and reeding in sequence according to the organizational structure requirements of the grey cloth, and then completes the weaving of the grey cloth through a water jet loom or an air jet loom; the water jet loom is preferably a 408 type water jet loom, and the air jet loom is preferably a 610 type air jet loom.
[0023] After obtaining the grey cloth, the present invention sequentially performs pre-treatment, dyeing, washing, shaping and drying, soaping and post-treatment on the grey cloth to obtain the high color fastness recycled environmentally friendly fabric. In the present invention, the pre-treatment preferably includes sequentially performing barrel matching, sewing and rolling, and flattening. In the present invention, the barrel matching preferably includes: configuring the number of grey cloths according to the number of finished products to be produced and the dyeing shrinkage of different varieties (pay attention to observe whether the ends of the cloth are dirty, such as oil stains and rust, when matching barrels). In the present invention, the sewing and rolling preferably includes: using a sewing machine to sew and connect the ends of each roll of grey cloth and rewind them onto the A1 frame (when sewing the ends, ensure that the cloth surface is flat to prevent breakage; maintain a uniform speed when rolling, and observe whether the cloth surface is wrinkled, weft skewed, and oily). In the present invention, the conditions for running flat width include: the temperature is preferably 80-90°C, more preferably 80-85°C; the vehicle speed is preferably 50-60 yards / hour, more preferably 50-55 yards / hour; based on 2500 meters of grey cloth, the mass of the alkali reagent used for running flat width is preferably 8kg; in an embodiment of the present invention, the alkali reagent used for running flat width is specifically purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.
[0024] In the present invention, dyeing is performed after the front treatment is completed. In the present invention, the dyeing conditions include: the insulation temperature is preferably 130°C, and the insulation time is preferably 3 hours; the time required for uniform heating from room temperature to the insulation temperature is preferably 1 hour, and the time required for uniform cooling from the insulation temperature to 60°C is preferably 1 hour. The present invention preferably selects the type of dye used for dyeing according to actual color needs; in an embodiment of the present invention, the dye used for dyeing (such as disperse blue, disperse orange, disperse red, leveling agent, glacial acetic acid) is specifically purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd. Specifically, the high color fastness recycled environmentally friendly fabric of the present invention preferably includes dark series fabrics or light series fabrics; the color of the dark series fabrics preferably includes black, dark navy blue, dark coffee, dark red or dark green; the color of the light series fabrics preferably includes white, natural white, off-white or beige. In an embodiment of the present invention, after the running flat width is completed, it is preferably carried out in sequence to beat the cloth into the cylinder and beat the material at room temperature, and then dyeing is achieved by heating, keeping warm and cooling in the above-mentioned manner. The cloth feeding into the cylinder of the present invention is preferably based on a cylinder of 2500 meters of cloth (before beating the cloth, observe whether there are foreign objects at the cylinder mouth to prevent scratching the cloth surface, and observe whether the cloth surface is clean and flat during beating), and ensure that the number of cloths in the two tubes is consistent to prevent tube difference and beat the cloth at a uniform speed. The normal temperature beating of the present invention preferably includes: the beating machine prepares the dye according to the specified formula (the beating machine should pay attention to observe whether the dye is dissolved and evenly dissolved when working), and manually feeds the material into the cylinder at a uniform speed. In the present invention, after the normal temperature punching is completed, the cylinder door is preferably closed, and the temperature is automatically raised by computer control, and the temperature is raised uniformly from normal temperature to the insulation temperature (when closing the cylinder door, make sure that the cylinder door is closed tightly to prevent material leakage, and pay attention to observe the heating situation to prevent excessive heating); the present invention allows the dye to fully penetrate into the grey cloth through insulation to achieve the dyeing effect (pay attention to observe whether the temperature meets the standard during the insulation process, observe the dyeing situation of the grey cloth, and ensure that the insulation time meets the requirements); when cooling down in the present invention, pay attention to prevent excessive cooling from causing color difference of the cloth, and ensure that the cooling time meets the requirements.
[0025] In the present invention, the dyeing is completed and then washed. In the present invention, when the high color fastness recycled environmentally friendly fabric is a dark series fabric, the number of times of washing is preferably 2 to 3 times; when the high color fastness recycled environmentally friendly fabric is a light series fabric, the number of times of washing is preferably 1. In the embodiment of the present invention, after the dyeing is completed (i.e. the temperature drops to 60°C), the dye is preferably discharged, and circulating water is injected to wash the fabric surface and take away the excess dye (when washing the fabric surface, the water should be clear before stopping the washing to prevent unclean water from causing the fabric surface to be stained). Usually, the light series fabric is washed once, and the dark series fabric is washed 2 to 3 times.
[0026] In the present invention, after the washing is completed, shaping and drying are performed. In the present invention, the conditions for shaping and drying preferably include: the temperature is preferably 170°C; the vehicle speed is preferably 60 yards / hour. In an embodiment of the present invention, after the washing, the grey cloth in the cylinder is preferably beaten out and put into the cloth drop barrel, and then pushed onto the dehydration and width-opening machine for dehydration and width-opening. After completion, shaping and drying are performed under the aforementioned limited conditions (pay attention to observe whether the vehicle speed and temperature meet the standards during shaping and drying, and observe whether the cloth surface has dyeing problems, wrinkles, and dirt such as oil stains).
[0027] In the present invention, soap washing is performed after the shaping and drying. In the present invention, when the recycled environmentally friendly fabric with high color fastness is a dark series fabric, the number of soap washings is preferably 2 to 3 times; when the recycled environmentally friendly fabric with high color fastness is a light series fabric, the number of soap washings is preferably 1 time. In the present invention, based on 2500 meters of grey cloth, the mass of the alkaline reagent used for each soap washing is preferably 20 kg; the feeding time of the alkaline reagent of the present invention is preferably 20 minutes, and the present invention prevents the fabric from being burned by slowly and evenly adding the alkaline reagent; the time of each soap washing of the present invention is preferably 30 minutes, and the time of soap washing is counted from the completion of feeding (soap washing makes the color fastness of the cloth surface more stable, usually the light series fabric is soaped once, and the dark series fabric is soaped 2 to 3 times). In an embodiment of the present invention, the alkaline reagent used for soap washing is specifically purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.
[0028] After the soaping, the present invention performs post-processing. The post-processing of the present invention preferably includes dehydration, opening and secondary shaping in sequence. In the embodiment of the present invention, the soaped cloth is specifically introduced into a washing machine, and the alkali agent is washed away while opening the width (keep the water tank clean before washing and introduce circulating water, pay attention to observe whether the water in the water tank is turbid during the washing process, and observe whether the cloth surface is clean when the cloth falls into the barrel). In the present invention, the conditions for the secondary shaping include: the temperature is preferably 170°C, and the vehicle speed is preferably 60 yards / hour; the secondary shaping is preferably carried out under the conditions of citric acid and antistatic solvent, and based on 2500 meters of grey cloth, the amount of citric acid is preferably 12kg; the amount of antistatic solvent is preferably 5kg (pay attention to observe whether the temperature and vehicle speed meet the standards during the secondary shaping, whether the citric acid and antistatic solvent are added accurately, whether the width measured by the rear head is uniform, and whether the color is consistent and whether there is color difference). In the embodiment of the present invention, the antistatic solvent is specifically purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.
[0029] The present invention provides a recycled environmentally friendly fabric with high color fastness prepared by the preparation method described in the above technical scheme.
[0030] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] The steps for preparing recycled environmentally friendly fabrics with high color fastness are as follows:
[0033] I. Fabric structure: The warp yarn and the weft yarn are interwoven with recycled environmentally friendly yarn; the recycled environmentally friendly yarn is recycled polyester yarn purchased from Zhejiang Jiaren New Materials Co., Ltd., the model is 75D / 72F DTY low-elastic yarn; the interweaving method is plain weave;
[0034] II. Grey fabric weaving: warping, sizing, beaming and reeding are carried out in sequence according to the fabric structure requirements, and then the grey fabric weaving is completed by a 408 type water jet loom;
[0035] III. Dyeing: including pre-treatment, dyeing and post-treatment in sequence, as follows:
[0036] 1. Front-end processing:
[0037] 1. Bucket matching: The number of grey cloths is matched according to the number of finished products to be produced and the dyeing shrinkage of different varieties (when matching the barrels, pay attention to whether there are dirty marks such as oil stains and rust on the cloth head);
[0038] 2. Sewing and rolling: Use a sewing machine to sew the ends of each roll of grey cloth together and roll them back onto the A1 frame (make sure the cloth surface is flat when sewing the ends to prevent breakage; keep a constant speed when rolling, and observe whether there are wrinkles, weft skew, and oil stains on the cloth surface);
[0039] 3. Flattening: Introduce the cloth roll on the A1 frame into the flattening machine at a temperature of 80℃, a speed of 50 yards / hour, and an alkali reagent (purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.) of 8kg (based on 2,500 meters of cloth in one cylinder) (the cloth surface must be flat and introduced at a uniform speed during introduction, and observe whether the amount of alkali reagent meets the requirements. If the amount of alkali reagent is less than 8kg, the machine will automatically add 8kg), and roll the flattened cloth flatly onto the A2 frame (pay attention to check whether the cloth surface is clean and the width is uniform);
[0040] 2. Dyeing in the tank:
[0041] 1. Put the cloth into the cylinder: one cylinder contains 2500 meters of cloth (before beating the cloth, check whether there are any foreign objects at the cylinder mouth to prevent scratching the cloth surface, and check whether the cloth surface is clean and flat during beating), and ensure that the amount of cloth in the two tubes is consistent to prevent tube difference and beating the cloth at a uniform speed;
[0042] 2. Normal temperature punching: The punching machine prepares the dye according to the specified formula (pay attention to whether the dye is dissolved and evenly mixed when the punching machine is working), which is controlled by a computer and the punching is completed in 10 minutes; the specific formula of the dye (disperse blue, disperse orange, disperse red, leveling agent and glacial acetic acid are all purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.) is shown in Table 1:
[0043] Table 1 Dye specific formula
[0044]
[0045] Note: The weight of the grey cloth is 100 grams, and the number of meters of the grey cloth is 2500 meters. According to the above ratio, the amount of 602 dye used is calculated as follows: 100 grams × 2500 meters × 4.05% = 10125 grams; the calculation method for other types of dyes is the same.
[0046] 3. Heating: After the material is charged, close the cylinder door, and the temperature will be automatically raised by computer control, from room temperature to 130°C at a uniform speed, and the heating time is 1 hour (make sure the cylinder door is closed tightly to prevent material from escaping, and pay attention to the temperature rise to prevent the temperature from rising too fast);
[0047] 4. Insulation: After the temperature rises to 130°C, keep it warm for 3 hours to allow the dye to fully penetrate into the grey cloth to achieve the dyeing effect (pay attention to observe whether the temperature meets the standard during the insulation process, observe the dyeing of the grey cloth, and ensure that the insulation time meets the requirements);
[0048] 5. Cooling: The temperature is cooled down from 130℃ to 60℃ at a uniform speed, and the cooling time is 1 hour (pay attention to the cooling situation during cooling to prevent the fabric from being damaged due to excessive cooling, and ensure that the cooling time meets the requirements);
[0049] 6. Water discharge: After the temperature drops to 60℃, the dye is discharged, and circulating water is injected to clean the fabric and take away the excess dye (when washing the fabric, the water should be clear before stopping the washing to prevent the fabric from being stained due to unclean water discharge. Generally, light-colored fabrics are washed once, and dark-colored fabrics are washed 2 to 3 times);
[0050] 7. Forming and drying: take the cloth out of the cylinder and put it into the cloth-dropping barrel, then push it onto the dehydration and width-opening machine for dehydration and width-opening. After completion, form and dry the cloth at a temperature of 170°C and a speed of 60 yards per hour (pay attention to observe whether the speed and temperature meet the standards during the forming and drying process, and also observe whether the cloth has any dyeing problems, wrinkles, or dirt such as oil stains);
[0051] 8. Soap washing: After shaping and drying, the fabric is put into the dyeing vat again, and 20kg of alkaline reagent (purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.) is used to wash the fabric surface according to 2500 meters of grey fabric to make the color fastness of the fabric surface more stable. The washing time is 30 minutes / time (the alkaline reagent is added slowly and evenly by computer control, and the material is beaten in 20 minutes to prevent burning the fabric. The washing time starts from the completion of adding materials; generally, light-colored fabrics are soaped once, and dark-colored fabrics are soaped 2-3 times);
[0052] 3. Post-processing:
[0053] 1. Dehydration and opening: introduce the soaped fabric into the washing machine, wash away the alkaline reagent and open the fabric at the same time (keep the water tank clean before washing and introduce circulating water. During the washing process, pay attention to whether the water in the water tank is turbid, and observe whether the fabric surface is clean when it falls into the bucket);
[0054] 2. Secondary shaping: adjust the shaping machine to a temperature of 170°C and a speed of 60 yards per hour, and add 12kg of citric acid and 5kg of antistatic solvent (purchased from Zhejiang Chuanhua Synthetic Materials Co., Ltd.) to 2500 meters of grey cloth for secondary shaping (pay attention to whether the temperature and speed meet the standards, whether the citric acid and antistatic solvent are added accurately, whether the width measured by the rear head is uniform, and whether the color is consistent and whether there is any color difference during the secondary shaping) to obtain recycled and environmentally friendly fabrics with high color fastness.
[0055] Comparative Example 1
[0056] The operation is carried out in accordance with the method of Example 1, except that the step "7. shaping and drying" is omitted, that is, the fabric obtained in the step "6. water discharge" is directly subjected to the step "8. soaping", and the number of soaping is 7 times.
[0057] The fabrics prepared in Example 1 and Comparative Example 1 were subjected to staining tests, and the results are shown in Table 2 and Table 3, respectively. The results show that compared with the fabrics prepared by the conventional process in Comparative Example 1, the fabrics prepared by the method of Example 1 of the present invention all meet the standards, the color fastness is greatly improved, and the actual use requirements of the fabrics are met.
[0058] Table 2 Performance test results of the fabric prepared in Example 1
[0059]
[0060] Table 3 Performance test results of the fabric prepared in Comparative Example 1
[0061]
[0062] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a recycled environmentally friendly fabric with high color fastness, comprising the following steps: Providing grey fabric, wherein the grey fabric is woven from recycled environmentally friendly yarn; The grey cloth is sequentially subjected to pre-treatment, dyeing, washing, shaping and drying, soaping and post-treatment to obtain the recycled environmentally friendly fabric with high color fastness.
2. The preparation method according to claim 1, characterized in that: The regenerated environmentally friendly yarn includes regenerated polyester yarn or regenerated nylon yarn.
3. The preparation method according to claim 1, characterized in that: The front-end treatment includes barrel matching, sewing and rolling, and flattening in sequence; the conditions for the flattening include: a temperature of 80-90° C., a vehicle speed of 50-60 yards per hour; based on 2500 meters of grey cloth, the mass of the alkaline reagent used for the flattening is 8 kg.
4. The preparation method according to claim 1, characterized in that: The dyeing conditions include: a holding temperature of 130° C., a holding time of 3 hours, a time required for uniformly increasing the temperature from room temperature to the holding temperature of 1 hour, and a time required for uniformly decreasing the temperature from the holding temperature to 60° C. of 1 hour.
5. The preparation method according to claim 1 or 4, characterized in that: The high color fastness recycled environmentally friendly fabrics include dark series fabrics or light series fabrics; the colors of the dark series fabrics include black, dark navy blue, dark coffee, dark red or dark green; the colors of the light series fabrics include white, natural white, off-white or beige.
6. The preparation method according to claim 5, characterized in that: When the recycled environmentally friendly fabric with high color fastness is a dark series fabric, the number of times of washing with water and washing with soap is independently 2 to 3 times; when the recycled environmentally friendly fabric with high color fastness is a light series fabric, the number of times of washing with water and washing with soap is both 1 time.
7. The preparation method according to claim 6, characterized in that: The soap washing time for each time is 30 minutes; based on 2500 meters of grey cloth, the mass of the alkaline reagent used for each soap washing is 20 kg.
8. The preparation method according to claim 1, characterized in that: The conditions for the shaping and drying include: a temperature of 170° C. and a vehicle speed of 60 yards per hour.
9. The preparation method according to claim 1, characterized in that: The post-processing includes dehydration, opening the width and secondary shaping in sequence; the conditions of the secondary shaping include: temperature of 170°C and vehicle speed of 60 yards per hour; the secondary shaping is carried out in the presence of citric acid and antistatic solvent, based on 2500 meters of grey cloth, the amount of citric acid used is 12 kg, and the amount of antistatic solvent used is 5 kg.
10. The recycled environmentally friendly fabric with high color fastness prepared by the preparation method according to any one of claims 1 to 9.