Method for efficiently detecting large-size Ds macroscopic inclusions in 54SiCr6 hot-rolled wire rod
By using methods such as post-hot rolling sampling, rapid cooling, low-temperature insulation, straightening and pre-drawing treatment, oil quenching and tempering, hydrochloric acid corrosion and rapid tensile testing in the detection of 54SiCr6 hot-rolled wire rods, problems in the existing technology have been solved It solves the problem of low detection success rate and achieves efficient detection of large-sized Ds macroscopic inclusions, meeting the needs of product quality assessment.
Patent Information
- Application Number
- CN202410776732.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
AI Technical Summary
When existing technology detects large-size Ds macroscopic inclusions inside 54SiCr6 hot-rolled wire rods, the success rate is low and the requirements for the flatness and surface finish of the test sample are high, resulting in inaccurate fracture locations during the detection process and inability to effectively detect them. Inclusions, especially when raw material production steel plants lack rotary bending billet testing machines, make it difficult to meet quality assessment requirements.
Through measures such as sampling immediately after hot-rolled wire rod rolling, rapid cooling, low-temperature insulation, straightening and pre-drawing treatment, oil quenching and tempering, 34% mass concentration hydrochloric acid corrosion and rapid tensile testing, and electron microscopy detection of fractures, the detection accuracy is ensured. Accuracy and efficiency.
It improves the detection success rate of large-sized Ds macroscopic inclusions inside 54SiCr6 hot-rolled wire rods, meets the needs of product quality stability and market competitiveness, and achieves efficient detection without rotating bending billet testing machines.
Smart Images

Figure BDA0004895900670000091 
Figure HDA0004895900720000011 
Figure HDA0004895900720000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and steel rolling, and is a method for efficiently detecting large-sized Ds-type macroscopic inclusions inside a 54SiCr6 hot-rolled wire rod. Background Art
[0002] Spring steel 54SiCr6 is mainly used to make automobile suspension springs with a stress level of 1950-2050MPa. It has been widely used in the field of new energy vehicles and has the performance characteristics of high working stress and high fatigue life. The main quality control points of its products are: zero surface defects, no total decarburization, shallow total decarburization, and no large-sized Ds-type macro inclusions. Generally, the size of such inclusions is required to be no larger than 15μm.
[0003] The current mainstream method for detecting large-sized Ds-type macroscopic inclusions inside 54SiCr6 hot-rolled wire rods relies on a rotating bending billet testing machine, which uses a four-point contact sample to perform small and fast up and down work, so that internal cracks are initiated at large-sized inclusions, and the cracks eventually form fractures after expansion, and then large-sized Ds-type macroscopic inclusions are detected. However, this method has extremely high requirements for the flatness and surface finish of the test sample, and to ensure that the sample is defect-free, high-precision eddy current flaw detection must be performed before sample preparation. Otherwise, a large number of fractures due to poor sample surface or poor flatness will occur during the detection process, resulting in the cross section being located in a place without Ds-type macroscopic inclusions, and the large-sized Ds-type macroscopic inclusions inside the 54SiCr6 hot-rolled wire rod cannot be effectively detected. The current success rate of industry testing is about 25%. In addition, steel mills that produce raw materials generally do not have this equipment.
[0004] The purpose of the present invention is to provide a method for efficiently detecting large-sized Ds-type macro inclusions inside 54SiCr6 hot-rolled wire rods without a rotating bending billet testing machine, so as to meet the quality level assessment requirements of steel mills producing raw materials for large-sized Ds-type macro inclusions inside 54SiCr6 hot-rolled wire rods before leaving the factory, ensure product quality stability, and enhance product market competitiveness. Summary of the invention
[0005] The object of the present invention is to provide a method for efficiently detecting large-sized Ds-type macroscopic inclusions inside 54SiCr6 hot-rolled wire rods, which can efficiently detect large-sized Ds-type macroscopic inclusions inside 54SiCr6 hot-rolled wire rods by taking samples immediately after hot-rolled wire rods are rolled, rapidly cooling, and heat-insulating at low temperatures to retain rolling internal stress and gas H to the maximum extent, straightening and pre-drawing treatment to increase the internal stress of the rolled material, oil quenching and tempering to high tensile strength to amplify the influence of macroscopic inclusions on mechanical properties, heat-insulating at 30°C to increase H in 34% mass concentration hydrochloric acid corrosion, rapid tensile testing, and electron microscope fracture detection.
[0006] In order to achieve the above technical purpose, the present invention provides a method for efficiently detecting large-sized Ds-type macroscopic inclusions inside 54SiCr6 hot-rolled wire rods, the process comprising: sampling the hot-rolled wire rods immediately after rolling, rapid cooling, low-temperature insulation, straightening & pre-drawing treatment, oil quenching and tempering to the target tensile strength, insulation at 30°C in 34% mass concentration hydrochloric acid corrosion, rapid tensile test, and electron microscope fracture detection, the steps are as follows:
[0007] (1) Take a 30-45 cm tensile sample immediately after hot-rolled wire rod rolling;
[0008] (2) The above sample is rapidly cooled to below 120°C within 5 to 10 minutes;
[0009] (3) The above sample is then placed in a foam insulation box with ice cubes and taken out after being kept warm to below 10°C;
[0010] (4) The above specimen is then straightened using a straightening machine and subjected to a single-side pre-drawing process until the diameter of the specimen is reduced by at least 0.15 mm;
[0011] (5) The above samples are then subjected to oil quenching at 875±5℃ for ≤5 min and tempering at 425±5℃ for ≤10 min. The tensile strength of the samples after heat treatment is controlled within the range of 1950-2050 MPa.
[0012] (6) After the tempering and heat preservation of the above-mentioned sample, put it into 34% mass concentration hydrochloric acid etchant and keep it at 30℃ for 15 to 20 minutes;
[0013] (7) The above specimens are then taken out and immediately subjected to tensile testing;
[0014] (8) The tensile fracture of the above-mentioned specimens was examined for fracture source using a field emission electron microscope to detect large-sized Ds-type macroscopic inclusions inside the 54SiCr6 hot-rolled wire rod.
[0015] Furthermore, the chemical composition of the 54SiCr6 hot-rolled wire rod, calculated by mass percentage, is C: 0.53%~0.59%, Si: 1.30%~1.60%, Mn: 0.60%~0.80%, P≤0.015%, S≤0.015%, Cr: 0.60%~0.80%, Ni: ≤0.10%, Cu≤0.08%, and the rest is iron and unavoidable impurities.
[0016] The present invention takes measures such as sampling immediately after hot-rolled wire rod rolling, rapid cooling, low-temperature heat preservation to retain rolling internal stress and gas H to the maximum extent, straightening and pre-drawing treatment to increase the internal stress of rolled materials, oil quenching and tempering to high tensile strength, amplifying the influence of macroscopic inclusions on mechanical properties, heat preservation at 30°C in 34% mass concentration hydrochloric acid corrosion to increase H, rapid tensile test, and electron microscope fracture detection to make 54SiCr6 hot-rolled wire rods in high internal stress and high H state, ensure that the 54SiCr6 hot-rolled wire rods are broken at the place containing Ds-type macroscopic inclusions during tensile test, and can efficiently detect large-size Ds-type macroscopic inclusions inside the 54SiCr6 hot-rolled wire rods. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the morphology of large-sized Ds-type inclusions inside the φ14mm 54SiCr6 hot-rolled wire rod in Example 1;
[0018] Figure 2 This is the morphology of large-sized Ds-type inclusions inside the φ15mm54SiCr6 hot-rolled wire rod of Example 2;
[0019] Figure 3 This is the morphology of large-sized Ds-type inclusions inside the φ16mm54SiCr6 hot-rolled wire rod of Example 3;
[0020] Figure 4 This is the electron microscope morphology of the fracture surface of the φ14mm54SiCr6 hot-rolled wire rod of the comparative example;
[0021] Figure 5 This is the electron microscope morphology of the fracture surface of the comparative example 2φ15mm54SiCr6 hot-rolled wire rod;
[0022] Figure 6 This is the electron microscope morphology of the fracture surface of the comparative example 7φ16mm54SiCr6 hot-rolled wire rod.
[0023] Figure 7 This is the macroscopic morphology of the fracture of the comparative example 9φ14mm54SiCr6 hot-rolled wire rod; DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0025] Based on the actual production of 54SiCr6 Taking hot-rolled wire rod as an example, the composition of 54SiCr6 is: C: 0.55%, Si: 1.40%, Mn: 0.67%, P: 0.010%, S: 0.008%, Cr: 0.67%, Ni: 0.005%, Cu: 0.010%, and the rest is iron and unavoidable impurities.
[0026] Example 1: φ14mm specification 54SiCr6
[0027] (1) Take 10 40cm tensile samples from the 54SiCr6 hot-rolled wire rod immediately after rolling;
[0028] (2) The above sample is rapidly cooled to 110°C by air;
[0029] (3) The above sample is then placed in a foam insulation box with ice cubes and taken out after being kept warm to 8°C;
[0030] (4) The above specimens are then straightened using a straightening machine and pre-drawn to
[0031] (5) The above samples were then oil quenched at 875°C for 3 min and tempered at 425°C for 7 min;
[0032] (6) After the tempering and heat preservation of the above sample, put it into 34% mass concentration hydrochloric acid etchant at 30℃ for 17 minutes;
[0033] (7) The above-mentioned samples were then taken out and immediately subjected to a tensile test in accordance with GB / T 228.1 Metallic materials tensile test Part 1: Room temperature test method. The tensile strength of the samples was 1987 MPa.
[0034] (8) The tensile fracture of the above specimens was examined for fracture source using a field emission electron microscope.
[0035] (9) This method was used to repeatedly test 10 rods. The results are shown in Table 1. The probability of detecting DS inclusions in the 54SiCr6 hot-rolled wire rod sample is 80%. The electron microscopy morphology of DS inclusions in sample 2 is shown in Table 1. Figure 1 shown.
[0036] Table 1
[0037] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? yes yes no yes yes yes no yes yes yes
[0038] Example 2: φ15mm specification 54SiCr6
[0039] (1) Take 10 45 cm tensile specimens immediately after hot rolling.
[0040] (2) The above sample is rapidly cooled to 80°C by air;
[0041] (3) The above sample is then placed in a foam insulation box with ice cubes and taken out after being kept warm to 6°C;
[0042] (4) The above specimens were then straightened using a straightening machine and pre-drawn to 14.65 mm;
[0043] (5) The above samples were then oil quenched at 871°C for 5 min and tempered at 430°C for 10 min;
[0044] (6) After the tempering and heat preservation of the above sample, put it into 34% mass concentration hydrochloric acid etchant at 30℃ for 20 minutes;
[0045] (7) The above-mentioned samples were then taken out and immediately subjected to a tensile test in accordance with GB / T 228.1 Metallic materials tensile test Part 1: Room temperature test method. The tensile strength of the samples was 1991 MPa.
[0046] (8) The tensile fracture of the above specimens was examined for fracture source using a field emission electron microscope.
[0047] (9) This method was used to repeatedly test 10 rods. The results are shown in Table 2. The probability of detecting DS inclusions in the 54SiCr6 hot-rolled wire rod sample is 90%. The electron microscopy morphology of DS inclusions in sample 5 is shown in Table 2. Figure 2 Implementation shown.
[0048] Table 2
[0049] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? yes yes yes yes yes yes yes yes no yes
[0050] Example 3: φ16mm specification 54SiCr6
[0051] (1) Take 10 33 cm tensile samples immediately after hot rolling;
[0052] (2) The above sample is rapidly cooled to 97°C by air;
[0053] (3) The above sample is then placed in a foam insulation box with ice cubes and taken out after being kept warm to 10°C;
[0054] (4) The above specimens were then straightened using a straightening machine and pre-drawn to 15.70 mm;
[0055] (5) The above samples were then oil quenched at 879°C for 5 min and tempered at 420°C for 8 min;
[0056] (6) After the tempering and heat preservation of the above sample, put it into 34% mass concentration hydrochloric acid etchant and keep it at 30℃ for 16 minutes;
[0057] (7) The above-mentioned samples were then taken out and immediately subjected to a tensile test in accordance with GB / T 228.1 Metallic materials tensile test Part 1: Room temperature test method. The tensile strength of the samples was 2031 MPa.
[0058] (8) The tensile fracture of the above specimens was examined for fracture source using a field emission electron microscope.
[0059] (9) This method was used to repeatedly test 10 rods. The results are shown in Table 3. The probability of detecting DS inclusions in the 54SiCr6 hot-rolled wire rod sample is 90%. The electron microscopy morphology of DS inclusions in sample 4 is shown in Table 3. Figure 3 shown.
[0060] Table 3
[0061] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? yes yes yes yes no yes yes yes yes yes
[0062] Comparative Example 1:
[0063] Comparative Example 1 only adjusts step (2) of Example 1 to cool the sample to 110°C naturally in air, and the rest is the same as Example 1. All 10 samples of 54SiCr6 hot-rolled wire rods were broken at the position without inclusions. The results are shown in Table 4. The tensile strength is 1988MPa. The fracture electron microscope morphology is shown in Table 4. Figure 4 shown.
[0064] Table 4
[0065] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0066] Comparative Example 2:
[0067] Comparative Example 2 only adjusts step (5) of Example 2 to 900°C oil quenching and heat preservation for 10 min, and 460°C tempering and heat preservation for 15 min. The rest is the same as Example 2. The comparative example 2 obtains All 10 samples of 54SiCr6 hot-rolled wire rods were broken at the position without inclusions. The results are shown in Table 5. The tensile strength is 1895MPa. The fracture electron microscope morphology is shown in Table 5. Figure 5 shown.
[0068] Table 5
[0069] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0070] Comparative Example 3:
[0071] Comparative Example 3 only adjusted step (5) of Example 2 to 871°C oil quenching and heat preservation for 10 min, and 430°C tempering and heat preservation for 10 min. The rest was the same as Example 2. The obtained All 10 samples of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 6 below, and the tensile strength is 1922MPa.
[0072] Table 6
[0073] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0074] Comparative Example 4:
[0075] Comparative Example 4 only adjusted step (5) of Example 2 to 890°C oil quenching and heat preservation for 4 min, and 430°C tempering and heat preservation for 10 min. The rest was the same as Example 2. The obtained All 10 specimens of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 7 below, and the tensile strength is 1850 MPa.
[0076] Table 7
[0077] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0078] Comparative Example 5:
[0079] Comparative Example 5 only adjusted step (5) of Example 2 to 871°C oil quenching and heat preservation for 5 min, and 425°C tempering and heat preservation for 15 min. The rest was the same as Example 2. The obtained All 10 specimens of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 8 below, and the tensile strength is 1900MPa.
[0080] Table 8
[0081] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0082] Comparative Example 6:
[0083] Comparative Example 6 only adjusted step (5) of Example 2 to 871°C oil quenching and heat preservation for 5 min, and 440°C tempering and heat preservation for 5 min. The rest was the same as Example 2. The obtained All 10 specimens of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 9 below, and the tensile strength is 1970 MPa.
[0084] Table 9
[0085] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0086] Comparative Example 7:
[0087] Comparative Example 7 only adjusts step (6) of Example 3. After the tempering and heat preservation of the above sample, it is placed in ordinary pure water at 30°C for 30 minutes. The rest is the same as Example 3. The comparative example 7 obtains All 10 samples of 54SiCr6 hot-rolled wire rods were broken at the position without inclusions. The results are shown in Table 10. The tensile strength is 1984MPa. The fracture electron microscope morphology is shown in Table 10. Figure 6 shown.
[0088] Table 10
[0089] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0090] Comparative Example 8:
[0091] Comparative Example 8 only adjusts step (6) of Example 3. After the tempering and heat preservation of the above sample, put it into 34% mass concentration hydrochloric acid etchant at 30℃ for 10 minutes. The rest is the same as Example 3. The comparative example 8 obtains All 10 specimens of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 11 below, and the tensile strength is 1975MPa.
[0092] Table 11
[0093] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0094] Comparative Example 9:
[0095] Comparative Example 9 only adjusts step (6) of Example 3. After the tempering and heat preservation of the above sample, it is placed in ordinary pure water at 30°C for 16 minutes. The rest is the same as Example 3. The comparative example 9 obtains All 10 specimens of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 12 below, and the tensile strength is 1986MPa.
[0096] Table 12
[0097] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0098] Comparative Example 10:
[0099] Comparative Example 10 only adjusts step (5) of Example 1. The sample is then oil quenched at 840°C for 7 minutes and tempered at 410°C for 8 minutes. The tensile strength of the sample after heat treatment is controlled at 2089 MPa. The other steps are the same as those of Example 1. The sample obtained in Comparative Example 10 is All 10 samples of 54SiCr6 hot-rolled wire rods were broken at the position without inclusions. The results are shown in Table 13. Among them, 6 samples were broken flush. The macroscopic morphology of the fracture is shown in Table 13. Figure 7 ;
[0100] Table 13
[0101]
[0102] Comparative Example 11:
[0103] Comparative Example 11 only adjusts step (1) of Example 1 After 7 days of storage, 10 40cm tensile samples were taken from the 54SiCr6 hot-rolled wire rods. The other samples were the same as those in Example 1. The samples obtained in Comparative Example 11 were All 10 specimens of 54SiCr6 hot-rolled wire rod broke at the position without inclusions. The results are shown in Table 14 below. The tensile strength is 1989 MPa.
[0104] Table 14
[0105] Test sample number 1 2 3 4 5 6 7 8 9 10 Is the fracture at the location containing DS inclusions? no no no no no no no no no no
[0106] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for efficiently detecting large-sized Ds-type macroscopic inclusions inside 54SiCr6 hot-rolled wire rod, characterized in that: The steps include: (1) Take a 30-45 cm tensile sample immediately after hot-rolled wire rod rolling; (2) The above-mentioned samples are rapidly cooled by air to below 120°C; (3) The above sample is then placed in a foam insulation box with ice cubes and taken out after being kept warm to below 10°C; (4) The above-mentioned specimen is then straightened by a straightening machine and subjected to a single-side pre-drawing; (5) The above samples are then subjected to oil quenching at 875±5℃ for ≤5 min and tempering at 425±5℃ for ≤10 min; (6) After the tempering and heat preservation of the above-mentioned sample is completed, it is placed in a hydrochloric acid etchant with a mass concentration of 34% and kept at 30°C for 15 to 20 minutes; (7) The above specimens are then taken out and immediately subjected to tensile testing; (8) The tensile fracture of the above-mentioned specimens was examined for fracture source using a field emission electron microscope to detect large-sized Ds-type macroscopic inclusions inside the 54SiCr6 hot-rolled wire rod.
2. The method for efficiently detecting large-sized Ds-type macroscopic inclusions in 54SiCr6 hot-rolled wire rod according to claim 1, characterized in that: The chemical composition of the 54SiCr6 hot-rolled wire rod is calculated by mass percentage and the proportion is: C: 0.53% to 0.59%, Si: 1.30% to 1.60%, Mn: 0.60% to 0.80%, P≤0.015%, S≤0.015%, Cr: 0.60% to 0.80%, Ni: ≤0.10%, Cu≤0.08%, and the rest is iron and unavoidable impurities.
3. The method for efficiently detecting large-sized Ds-type macroscopic inclusions in 54SiCr6 hot-rolled wire rod according to claim 1, characterized in that: The rapid air cooling time in step (2) is 5-10 minutes.
4. The method for efficiently detecting large-sized Ds-type macroscopic inclusions in 54SiCr6 hot-rolled wire rod according to claim 1, characterized in that: After step (4) is completed, the sample diameter is reduced by at least 0.15 mm.
5. The method for efficiently detecting large-sized Ds-type macroscopic inclusions in 54SiCr6 hot-rolled wire rod according to claim 1, characterized in that: After step (5) is completed, the tensile strength of the sample is controlled at 1950-2050 MPa.