Method for testing shear resistance between asphalt and ice layer
By simulating the shear performance test between the asphalt and the ice layer in the laboratory, and using the UTM microcomputer-controlled universal testing machine to conduct the interlayer oblique shear test, the problem of the lack of effective testing methods in the existing technology is solved, and the asphalt pavement is provided with a Winter shear performance data helps optimize material formulas and improve driving safety.
Patent Information
- Application Number
- CN202410803556.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-11
AI Technical Summary
The existing technology lacks effective testing methods to evaluate the shear resistance between asphalt and ice layers, resulting in insufficient research on the driving safety and service life of road asphalt pavements in winter.
Using a method including asphalt specimen preparation, cube mold setting, ice layer mixture preparation and shear force testing, the interlayer oblique shear test was carried out through the UTM microcomputer-controlled universal testing machine, and the peak load and angle during shear failure were recorded. The shear force between the asphalt and the ice layer is calculated.
It provides accurate simulation and evaluation of the shear performance of asphalt pavement materials in winter icing environments under laboratory conditions, fills the gaps in existing technology, provides scientific basis for material formula adjustment and additive selection, and improves driving safety and Maintenance costs are reduced.
Smart Images

Figure CN118758778A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of asphalt pavement deicing and anti-stripping, and in particular relates to a method for testing the shear resistance between asphalt and an ice layer. Background Art
[0002] With the rapid expansion of my country's highway network, asphalt pavement has played an important role in pavement construction due to its excellent performance and economy. However, in winter and early spring, severe weather conditions such as snowfall, freezing rain and frost frequently occur in northern and southwestern my country, resulting in widespread icing of the road surface, forming a slippery ice layer, which seriously reduces the anti-skid performance of the road surface and poses a major threat to driving safety. In addition, icing can also cause the peeling of pavement materials, which in turn affects the service life and maintenance costs of the road.
[0003] At present, the research on road snow and ice removal mainly focuses on the physical removal method of ice layer, while the research on the adhesion mechanism between asphalt and ice layer is relatively small. In addition, due to the limitation of experimental conditions, the existing research focuses on the numerical simulation calculation of aircraft icing and the application of anti-icing technology, while the research on the adhesion performance between road asphalt and ice layer, especially the shear resistance, has not been fully characterized due to the lack of effective testing methods.
[0004] The shear resistance of asphalt pavement is one of the key indicators for testing its performance under icy conditions. In order to better understand and improve the driving safety of asphalt pavement in winter, it is necessary to develop a new test method to accurately evaluate the shear resistance between asphalt and ice. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned shear resistance test, namely, the lack of research data on the adhesion mechanism between asphalt and ice layer, the limitations of previous studies that mainly focused on aircraft icing while ignoring road asphalt, and the lack of an effective method for testing the shear resistance between asphalt and ice layer, and to provide a method for testing the shear resistance between asphalt and ice layer.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A method for testing the shear resistance between asphalt and ice layer, characterized by comprising the following steps:
[0008] Step 1: Preparation of asphalt specimens: Heat the asphalt to be tested to a fluid state. The asphalt can be base asphalt or modified asphalt. Apply the asphalt heated to a fluid state evenly on the top surface of the stainless steel plate, and then place it at room temperature until the asphalt is completely cooled and solidified to form an asphalt specimen.
[0009] Step 2: Preparation of a cubic mold: Use the asphalt specimen formed in step 1 as the bottom plate, with the coated surface of the bottom plate facing upwards, and place four stainless steel plates of the same material and size around the bottom plate in four directions to form a cubic mold without a top surface. The four stainless steel plates serve as side plates of the cubic mold, and a layer of paraffin is coated on the inner sides of the four side plates;
[0010] Step 3: Prepare the ice layer mixture, mix crushed ice and water evenly to form a mixture, and fill the mixture evenly into the cube mold three times. After filling, the surface of the mixture must be flush with the top of the stainless steel plate to form a flat cube ice layer;
[0011] Step 4: The ice layer solidifies. The filled and cube-shaped mold is cooled to allow the mixture to initially solidify into ice. The other four stainless steel plates except the bottom plate are then removed to form a cube structure with only the bottom plate and the ice layer. The structure is then placed in the refrigerator to complete the hardening process of the ice layer.
[0012] Step 5: Shear force test: Perform an interlayer oblique shear test on the hardened ice layer, record the load values corresponding to different interface displacements during the shear process, and lock the peak load F at shear failure.
[0013] In step one, for base asphalt, the heating temperature is 150°C, for modified asphalt, the heating temperature is 180°C, and the heating time is 40 minutes.
[0014] In step 1, the stainless steel plate coated with asphalt is 15 cm×15 cm.
[0015] In step three, the mixture is formed by mixing crushed ice and water in a mass ratio of 9:1. The mixture is evenly filled into the mold three times, each time filling to a height of about 5 cm, and gently tamped 10 times with a glass rod.
[0016] To make the mixture in the cube mold initially solidify, the mold needs to be refrigerated at -10°C for 30 minutes; to make the mixture in the cube mold further harden, the mold after initial solidification needs to be placed in the refrigerator and refrigerated at -5°C for 24 hours.
[0017] In step 5, the measuring range of the UTM microcomputer-controlled universal testing machine is 50 kN, and the loading rate is set to 10 mm / min.
[0018] A method for preparing a test piece for testing the shear performance between an asphalt mixture and an ice layer comprises the following steps:
[0019] Step 1: Asphalt mixture preparation: Prepare asphalt mixture according to standard methods and make Marshall specimens according to the Marshall test method;
[0020] Step 2: Specimen cutting: Cut the Marshall specimen into a cube with a side length of 6 cm;
[0021] Step 3: Preparation of hollow cube: Place the cut cube specimen with the top surface facing upwards, and use 4 stainless steel plates with a side length of 6 cm to surround the specimen to form a hollow cube without a top surface. The front, back, left, and right stainless steel plates facing inwards also need to be evenly coated with a layer of paraffin wax;
[0022] Step 4: Preparation and condensation of ice layer: Use crushed ice and water to mix evenly to form a mixture, and fill the mixture evenly into the cube mold three times. After filling, the surface of the mixture must be flush with the top of the stainless steel plate to form a flat cube ice layer; cool the filled and cube-shaped mold to allow the mixture to initially condense into ice, then remove the other four stainless steel plates except the bottom plate to form a cube structure with only the bottom plate and the ice layer, and continue to put the structure into the refrigerator to complete the hardening process of the ice layer.
[0023] A method for calculating the shear force between asphalt and an ice layer, using the peak load F and shear angle θ recorded during shear failure, and calculating the shear force F2 between the asphalt and ice layer through the formula 2Fsinθ=F2, where F is the peak load during shear failure, and θ is the angle in the shear test.
[0024] An application of asphalt pavement deicing and anti-stripping technology uses a test method for the shear resistance between asphalt and ice layers.
[0025] A method for optimizing the winter performance of an asphalt pavement material adjusts the formulation of the asphalt pavement material or selects a suitable additive based on data obtained from a test method for the shear resistance between asphalt and an ice layer.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention discloses a method for testing the shear resistance between asphalt and ice layer, which can accurately simulate and evaluate the shear resistance of asphalt pavement materials in winter icing environment under laboratory conditions, effectively filling the gap in the existing technology in the study of asphalt-ice layer adhesion mechanism; at the same time, the test method proposed by the present invention can provide accurate shear resistance data of asphalt pavement materials under winter icing conditions, providing a scientific basis for material formulation adjustment or additive selection, thereby helping to develop asphalt pavement materials that are more suitable for winter conditions and breaking the limitations of asphalt research.
[0028] Furthermore, the specific temperature and time of asphalt heating are adjusted according to the specific type of asphalt and the required flow state to ensure that the asphalt can be evenly distributed during the coating process to form a defect-free asphalt layer and provide accurate test data for shear force testing.
[0029] Furthermore, the step of applying paraffin is to prevent adhesion between the stainless steel plate and the ice layer during the subsequent ice layer preparation process, thereby ensuring the repeatability of the test and the accuracy of the results, so as to improve the effectiveness of the shear force test between the asphalt and the ice layer.
[0030] Furthermore, the loading rate during the shear force test is selected based on actual road usage conditions and ice layer material properties to ensure that the test results can truly reflect the shear resistance between the asphalt and ice layer, providing a guarantee for the implementation of the shear force test method between the asphalt and the ice layer of the present invention.
[0031] Furthermore, the filling and tamping steps of the mixture need to ensure that there are no air gaps between the mixture and the asphalt layer and inside the mixture, so as to simulate the contact state between the asphalt and the ice layer under actual road conditions, improve the realistic simulation of the test, and further ensure the effectiveness of the test experiment.
[0032] Furthermore, the method for preparing test specimens for shear resistance testing between asphalt mixture and ice layer disclosed in the present invention provides key test conditions for shear force testing between asphalt and ice layer to obtain key test data, further providing guarantee for shear force testing between asphalt and ice layer.
[0033] Furthermore, the method for calculating the shear force between asphalt and ice layer disclosed in the present invention provides important data support for winter maintenance and improvement of asphalt pavement, and further effectively fills the gap in the existing technology in the research of asphalt-ice layer adhesion mechanism.
[0034] Furthermore, the application developed according to the shear resistance test method between asphalt and ice layer disclosed in the present invention helps to deeply understand the adhesion mechanism between asphalt and ice layer, has guiding significance for the development of new asphalt pavement materials or additives, and can significantly improve the driving safety of asphalt pavement under low temperature conditions.
[0035] Furthermore, the present invention optimizes the winter performance of asphalt pavement materials, helps reduce traffic accidents and maintenance costs caused by road icing, and has significant economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a flow chart of the asphalt-ice layer shear resistance testing method of the present invention;
[0037] Figure 2 FIG. 1 is a diagram showing the preparation process of the ice layer mixture of the present invention;
[0038] Figure 3 Diagram of steps for constructing a cube mold for the present invention. DETAILED DESCRIPTION
[0039] In order to further understand the content of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the embodiments are only for explaining the present invention and are not intended to limit it.
[0040] See also Figure 1 , Figure 2 , Figure 3 , the asphalt-ice layer shear resistance test method includes the following steps:
[0041] (1) Preparation of asphalt specimens:
[0042] The asphalt is heated to a fluid state and then applied to the stainless steel plate, and then cooled to room temperature until the asphalt on the stainless steel plate is completely solidified.
[0043] (2) Create a cube mold:
[0044] like Figure 3 As shown, four stainless steel plates of exactly the same size are prepared, the stainless steel plate coated with asphalt is used as the bottom plate, and four stainless steel plates are used as side plates. Paraffin is coated on the inner sides of the four side plates, and the four side plates are placed on the four surfaces of the bottom plate respectively. The four side plates are perpendicular to the bottom plate and fit tightly to each other.
[0045] (3) Ice layer preparation:
[0046] like Figure 2 As shown, crushed ice and water are mixed evenly in a mass ratio of 9:1 to form a mixture, and the mixture is evenly filled into the above-mentioned cubic mold three times. After filling, the surface of the mixture needs to be flush with the top of the stainless steel plate to form a flat cubic ice layer; after filling, the mold is placed in a refrigerator for refrigeration. After the mixture is initially condensed into ice, the four side panels are removed and the mixture is continued to be placed in the refrigerator for refrigeration until the mixture is completely hardened.
[0047] (4) Shear force test:
[0048] The UTM microcomputer-controlled universal testing machine is used to carry out interlayer oblique shear test on the hardened ice layer. The testing machine automatically records the load values corresponding to the displacements of different interfaces during the shear process and locks the peak load at the time of shear failure.
[0049] In a specific embodiment of the present invention, each step of the asphalt-ice layer shear resistance testing method will be described in detail, including parameter settings, operation procedures and results.
[0050] Example 1
[0051] (1) Preparation of asphalt specimens:
[0052] Select base asphalt or modified asphalt as the experimental material, put the asphalt sample into an oven preheated to 150℃ or 180℃ and heat it for 40 minutes until the asphalt reaches a fully fluid state.
[0053] Apply the heated asphalt evenly on a 15cm×15cm stainless steel plate to ensure uniform coating thickness without bubbles and cracks, then cool at room temperature for 2 hours until the asphalt is completely solidified.
[0054] (2) Construction of cube mold:
[0055] Use a stainless steel plate of the same material as the base plate to build a cube mold without a top surface around the asphalt specimen, ensuring that the sides of the mold are vertical and fit tightly.
[0056] Paraffin wax was evenly coated on the inner side of the four stainless steel plates constituting the cube mold to reduce adhesion to the ice layer and improve the repeatability of the experiment.
[0057] (3) Preparation of ice layer mixture:
[0058] The pre-crushed ice residue was mixed with distilled water in a mass ratio of 9:1 and stirred thoroughly with a stirrer for 5 minutes until a uniform ice-water mixture was formed.
[0059] (4) Filling and leveling of ice layer:
[0060] The ice-water mixture was evenly filled into the cubic mold three times, each time to a height of about 5 cm, and gently tamped with a glass rod to ensure that the mixture was in full contact with the asphalt layer and there was no air gap.
[0061] Once filled, use a ruler and spatula to level the surface of the mixture, making sure it is flush with the top of the stainless steel plate to form a regular layer of cubed ice.
[0062] (5) Initial condensation and refrigeration of ice layer:
[0063] Place the filled cube mold in the pre-cooling area of the refrigerator at -10°C for 30 minutes to allow the mixture to begin to freeze.
[0064] After initial solidification, the four side panels of the cube mold were carefully removed, leaving only the ice layer and the bottom panel in contact with the asphalt layer.
[0065] (6) Final hardening of the ice layer:
[0066] The remaining cube structure was placed in the freezer at -5°C for 24 hours to complete the final hardening of the ice layer.
[0067] (7) Implementation of shear force test:
[0068] The hardened ice layer specimens were placed on a UTM microcomputer-controlled universal testing machine and subjected to an interlayer oblique shear test in accordance with ASTM C882 / C882M-13 standards.
[0069] The loading rate is set to 10 mm / min, and the testing machine automatically records the load values corresponding to different interface displacements during the shear process until shear failure occurs between the asphalt and ice layers.
[0070] (8) Calculation and analysis of shear force:
[0071] According to the peak load F and the back shear angle θ recorded during shear failure, the actual shear force F2 between the asphalt and ice layer is calculated using the formula 2Fsinθ=F2.
[0072] The test results are analyzed in detail to evaluate the shear performance of asphalt pavement materials under winter icing conditions, and the formulation or additive selection of asphalt pavement materials is optimized accordingly.
[0073] In this embodiment, through the above steps, we obtain specific data of the shear resistance between asphalt and ice layer. For example, in a typical measurement force F2 is 1732.0N. This result shows that the asphalt pavement material has good anti-retention performance under icing conditions and can meet the requirements of winter driving safety.
[0074] Through the specific implementation of the present invention, not only can the winter performance of asphalt pavement materials be accurately evaluated, but also strong technical support is provided for the scientific selection and reasonable design of asphalt pavement materials, which has significant practical value and social significance.
[0075] Embodiment 2:
[0076] In another specific embodiment of the present invention, it will be demonstrated how to use the asphalt mixture-ice shear resistance test specimen preparation method and the asphalt-ice layer shear force test method to test the shear resistance of the asphalt mixture.
[0077] (1) Preparation of asphalt mixture:
[0078] According to the standard asphalt mixture preparation process, the base asphalt is evenly mixed with aggregates, fillers and other additives to form the required asphalt mixture.
[0079] (2) Preparation of Marshall test pieces:
[0080] The prepared asphalt mixture was used to make a standard Marshall specimen with a diameter of 101.6 mm and a height of 63.5 mm according to the Marshall test method.
[0081] (3) Cutting of cube specimens:
[0082] The Marshall specimen was cut into a cube with a side length of 6 cm. During the cutting process, special attention was paid to keep the top surface uncut to ensure that the top surface was flat.
[0083] (4) Construction of hollow cube:
[0084] Four stainless steel plates with a side length of 6 cm were used to surround the front, back, left and right sides of the cube specimen to form a hollow cube without a top surface, ensuring that all contact surfaces were coated with paraffin to reduce adhesion.
[0085] (5) Preparation and filling of ice layer mixture:
[0086] Crushed ice and pre-cooled water were mixed evenly in a mass ratio of 9:1 to form an ice-water mixture, and the mixture was filled into the hollow cubes by three fillings. After each filling, a glass rod was used to gently tamp to ensure that the mixture was evenly distributed.
[0087] (6) Ice condensation and refrigeration:
[0088] Place the filled cubes in a refrigerator and refrigerate at -10°C for 30 minutes. After initial solidification, remove the outer stainless steel plate and continue to refrigerate at -5°C for 24 hours to complete the hardening of the ice layer.
[0089] (7) Shear force test:
[0090] The hardened asphalt mixture-ice layer specimen was placed on a UTM microcomputer-controlled universal testing machine and an interlayer oblique shear test was carried out in accordance with ASTM C882 / C882M-13 standards. The loading rate was set at 10 mm / min.
[0091] (8) Data recording and shear force calculation:
[0092] The load values corresponding to different interface displacements during the test were recorded until shear failure occurred between the ice layers of the asphalt mixture. The peak load F was recorded, and the shear force F2 between the ice layers of the asphalt mixture was calculated using the formula 2Fsinθ=F2.
[0093] (9) Result analysis:
[0094] By analyzing the bending shear test results, the anti-freezing performance of asphalt mixture under winter icing conditions is evaluated. For example, in one test, the peak load F was measured to be 2500N, the shear angle θ was 35°, and the calculated shear force F2 was 1913.2N.
[0095] (10) Material optimization:
[0096] According to the test results, the formula of asphalt mixture is adjusted, such as increasing the amount of anti-stripping agent or changing the ratio of asphalt to aggregate, to improve the shear resistance of asphalt mixture.
[0097] Through the above-mentioned specific implementation mode 2, the present invention can not only test the winter performance of asphalt mixture, but also provide an experimental means to guide the optimization and improvement of asphalt mixture, which has important engineering application value.
[0098] Embodiment 3:
[0099] This embodiment further describes in detail the specific operating steps of a method for testing the shear resistance between asphalt and ice layers, which is particularly suitable for evaluating the performance of different asphalt pavement materials under simulated winter icing conditions.
[0100] (1) Heating and coating of asphalt:
[0101] A specific modified asphalt was selected as the experimental material and heated in an oven preheated to 180°C for 40 minutes until the asphalt was completely fluid.
[0102] The heated asphalt was evenly coated on a 15cm×15cm×1cm stainless steel plate to ensure uniformity and defect-free coverage of the asphalt layer.
[0103] (2) Cooling and solidification of the specimen:
[0104] The stainless steel plate coated with asphalt was placed at room temperature (about 25°C) to cool naturally for 2 hours until the asphalt was completely solidified to form a solid asphalt specimen.
[0105] (3) Preparation of ice layer mixture:
[0106] Ice chips that had been crushed to a diameter of less than 2 mm were mixed with distilled water precooled to 4°C in a mass ratio of 9:1, and stirred thoroughly for 5 minutes using a stirrer until a uniform ice-water mixture was formed.
[0107] (4) Filling and leveling of ice layer:
[0108] The ice-water mixture was evenly filled into the constructed cubic mold three times, each time to a height of about 5 cm, and a glass rod was used to gently tamp to exclude air, ensuring that the mixture was in full contact with the asphalt layer.
[0109] (5) Initial condensation and refrigeration of ice layer:
[0110] Place the filled cube mold in the pre-cooling area of the refrigerator at -10°C for 30 minutes to allow the mixture to begin to freeze.
[0111] (6) Final hardening of the ice layer:
[0112] The four side panels of the cube mold were removed, leaving only the asphalt specimen and the ice layer in contact with it. The structure was then placed in the freezer area of the refrigerator and refrigerated at -5°C for 24 hours.
[0113] (7) Implementation of shear force test:
[0114] The hardened ice layer specimen was placed on a UTM microcomputer-controlled universal testing machine and subjected to an interlayer oblique shear test according to ASTM C882 / C882M-13 standard, with the loading rate set at 10 mm / min.
[0115] (8) Data recording and shear force calculation:
[0116] The load values corresponding to different interface displacements during the test were recorded until shear failure occurred between the asphalt and the ice layer. The peak load F was recorded and the actual shear force F2 between the asphalt and the ice layer was calculated using the formula 2Fsinθ=F2.
[0117] (9) Result analysis and application:
[0118] By analyzing the shear force test results, the shear resistance of the modified asphalt used in winter icing conditions was evaluated. In one test, the peak load F was measured to be 3200N, the shear angle θ was 30°, and the calculated shear force F2 was 1739.75N. This result shows that the modified asphalt tested has good shear resistance and is suitable for winter road maintenance.
[0119] (10) Material performance optimization:
[0120] Based on the test results, the formula of modified asphalt can be adjusted, such as increasing the amount of anti-stripping agent or changing the ratio of asphalt to aggregate, to further improve the winter performance of asphalt pavement materials.
[0121] Through the above-mentioned specific implementation mode 3, the present invention can not only accurately evaluate the winter performance of specific asphalt pavement materials, but also provide an experimental means to guide the optimization and improvement of asphalt pavement materials, which has important practical significance and application value for improving winter road driving safety and reducing maintenance costs.
[0122] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for testing the shear resistance between asphalt and ice layer, characterized in that: The following steps are involved: Step 1: Preparation of asphalt specimens: Heat the asphalt to be tested to a fluid state. The asphalt can be base asphalt or modified asphalt. Apply the asphalt heated to a fluid state evenly on the top surface of the stainless steel plate, and then place it at room temperature until the asphalt is completely cooled and solidified to form an asphalt specimen. Step 2: Preparation of a cubic mold: Use the asphalt specimen formed in step 1 as the bottom plate, with the coated surface of the bottom plate facing upwards, and place four stainless steel plates of the same material and size around the bottom plate in four directions to form a cubic mold without a top surface. The four stainless steel plates serve as side plates of the cubic mold, and a layer of paraffin is coated on the inner sides of the four side plates; Step 3: Prepare the ice layer mixture, mix crushed ice and water evenly to form a mixture, and fill the mixture evenly into the cube mold three times. After filling, the surface of the mixture must be flush with the top of the stainless steel plate to form a flat cube ice layer; Step 4: The ice layer solidifies. The filled and cube-shaped mold is cooled to allow the mixture to initially solidify into ice. The other four stainless steel plates except the bottom plate are then removed to form a cube structure with only the bottom plate and the ice layer. The structure is then placed in the refrigerator to complete the hardening process of the ice layer. Step 5: Shear force test: Perform an interlayer oblique shear test on the hardened ice layer, record the load values corresponding to different interface displacements during the shear process, and lock the peak load F at shear failure.
2. A method for testing the shear resistance between asphalt and ice layer according to claim 1, characterized in that: In step 1, for base asphalt, the heating temperature is 150°C, for modified asphalt, the heating temperature is 180°C, and the heating time is 40 minutes.
3. A method for testing the shear resistance between asphalt and ice layer according to claim 1, characterized in that: In step 1, the stainless steel plate coated with asphalt is 15 cm×15 cm.
4. A method for testing the shear resistance between asphalt and ice layer according to claim 1, characterized in that: In step three, the mixture is crushed ice and water in a mass ratio of 9:1; the mixture is evenly filled into the mold three times, each time filling to a height of about 5 cm, and gently tamped 10 times with a glass rod.
5. The method for testing the shear resistance between asphalt and ice layer according to claim 1, characterized in that: To make the mixture in the cube mold initially solidify, the mold needs to be refrigerated at -10°C for 30 minutes; to make the mixture in the cube mold further harden, the initially solidified mold is further placed in the refrigerator and refrigerated at -5°C for 24 hours.
6. A method for testing the shear resistance between asphalt and ice layer according to claim 1, characterized in that: In step five, the testing machine for performing the interlayer oblique shear test on the hardened ice layer is a UTM microcomputer-controlled universal testing machine, the measuring range of the UTM microcomputer-controlled universal testing machine is 50 kN, and the loading rate is set to 10 mm / min.
7. A method for preparing a test specimen for testing the shear performance between an asphalt mixture and an ice layer, characterized in that: The following steps are involved: Step 1: Asphalt mixture preparation: Prepare asphalt mixture according to standard methods and make Marshall specimens according to the Marshall test method; Step 2: Specimen cutting: Cut the Marshall specimen into a cube with a side length of 6 cm; Step 3: Preparation of hollow cube: Place the cut cube specimen with the top surface facing upwards, and use 4 stainless steel plates with a side length of 6 cm to surround the specimen to form a hollow cube without a top surface. The front, back, left, and right stainless steel plates facing inwards also need to be evenly coated with a layer of paraffin wax; Step 4: Preparation and condensation of ice layer: Use crushed ice and water to mix evenly to form a mixture, and fill the mixture evenly into the cube mold three times. After filling, the surface of the mixture must be flush with the top of the stainless steel plate to form a flat cube ice layer; cool the filled and cube-shaped mold to allow the mixture to initially condense into ice, then remove the other four stainless steel plates except the bottom plate to form a cube structure with only the bottom plate and the ice layer, and continue to put the structure into the refrigerator to complete the hardening process of the ice layer.
8. A method for calculating the shear force between asphalt and ice layer, characterized in that: Using the peak load F and shear angle θ recorded during shear failure, the shear force F2 between the asphalt and ice layer is calculated using the formula 2Fsinθ=F2, where F is the peak load during shear failure and θ is the angle in the sound shear test.
9. An application of asphalt pavement deicing and anti-stripping technology, characterized in that: The method for testing the shear resistance between asphalt and ice layer as described in any one of claims 1 to 6 is used.
10. A method for optimizing the winter performance of asphalt pavement materials, characterized in that: According to the data obtained by the method for testing the shear resistance between asphalt and ice layer according to any one of claims 1 to 8, the formulation of the asphalt pavement material is adjusted or a suitable additive is selected.