Method for testing circularity of non-circular cross-section fiber

By mixing non-circular cross-section fibers and circular cross-section fibers in different proportions, and using a microscope and the least squares method to calculate their circularity, the problem of difficulty in measuring non-circular cross-section fibers is solved, and quantitative analysis of fiber blended products is achieved. and environmental benefits.

CN118758935APending Publication Date: 2024-10-11JIANG SU CHENG XIN JIAN YAN JIAN CE REN ZHENG GU FEN YOU XIAN GONG SI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411143190.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

When measuring the circularity of non-circular cross-section fibers, the existing technology has problems such as high technical difficulty in cross-section slicing, image distortion, and low measurement accuracy, resulting in low efficiency in quantitative analysis of fiber content.

Method used

By mixing non-circular cross-section fibers and circular cross-section fibers in different mass ratios to form a fiber suspension, use a microscope to measure the projection width and number of roots, establish a nonlinear model, and apply the least squares method to calculate the circular shape of non-circular cross-section fibers. Spend.

Benefits of technology

It achieves objective scientific characterization of non-circular cross-section fibers, solves the problem of quantitative analysis of non-circular cross-section fiber and circular cross-section fiber blended products, and has the advantages of energy saving and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_14
    Figure QLYQS_14
  • Figure QLYQS_17
    Figure QLYQS_17
  • Figure QLYQS_22
    Figure QLYQS_22
Patent Text Reader

Abstract

The invention relates to a method for testing the circularity of non-circular cross-section fibers, which comprises the following steps of: selecting different types of non-circular cross-section fibers and circular cross-section fibers, obtaining small fiber fragments through a Hastelloy slicer, proportioning fiber mixtures with different mass proportions, obtaining a mass proportion value of the circular cross-section fibers, dispersing the fibers in a certain amount of solvent, and obtaining the circularity of the non-circular cross-section fibers; using a microscope to observe the mixture of the small fiber fragments, respectively measuring the projection widths and the number of the non-circular cross-section fibers and the circular cross-section fibers, calculating the actual measurement value of the mass of the circular cross-section fibers, and calculating the actual measurement value of the mass of the circular cross-section fibers by defining the circularity of the non-circular cross-section fibers. And establishing a nonlinear model between the mass ratio value of the circular fiber and the measured value, and calculating the characteristic parameter of the nonlinear model by applying a least square method, namely the circularity of the non-circular cross-section fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber circularity testing, and in particular to a method for testing the circularity of a fiber with a non-circular cross section. Background Art

[0002] Circularity is an important concept in image processing, generally used for feature extraction and description, and is represented by the area multiplied by 4π divided by the square of the perimeter.

[0003] The circularity of a fiber refers to the degree to which the shape of the fiber's cross section is close to a circle. It is evaluated by measuring the deviation between the shape of its cross section and the ideal circle. The circularity of a fiber has an important influence on its physical properties and application performance.

[0004] FZ / T 01101-2008 "Physical method for determination of fiber content in textiles" includes manual splitting method and microscopic method. The microscopic method stipulates that for circular cross-section fibers, the fiber diameter is measured, and for non-circular cross-section fibers, the fiber cross-sectional area is measured, and the fiber content is calculated through relevant formulas. In practical applications, there are problems such as high difficulty in fiber cross-sectional slicing technology, distortion of fiber cross-sectional images, low accuracy in fiber cross-sectional area measurement, and low test efficiency when measuring fiber cross-sectional area. Therefore, there are great technical barriers in practical applications. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a method for testing the circularity of non-circular cross-section fibers to solve the problem of quantitative analysis of blended products of non-circular cross-section fibers and circular cross-section fibers.

[0006] The object of the present invention is achieved in that: A method for testing the circularity of a fiber with a non-circular cross section comprises the following steps: Step 1, selecting a non-circular cross-section fiber to be tested; Step 2: Select circular cross-section fiber; Step 3: Use a Hastelloy slicer to cut short fiber segments of 0.2-0.4 mm in length from the non-circular cross-section fibers and circular cross-section fibers of different types to be tested, and weigh a certain mass of the non-circular cross-section fibers. and circular cross-section fibers , mixed into a series of fiber mixtures with different mass ratios to obtain the mass percentage of circular cross-section fibers : Step 4: Put the fiber mixture of different mass proportions in step 3 into a watch glass, add an appropriate amount of solvent, stir thoroughly to form a uniformly mixed fiber suspension, take a certain amount of the suspension with a pipette, transfer it to a glass slide, and prepare a sample observation slide; Step 5: Place the sample observation film on the microscope stage and measure the projection width of the relevant fibers respectively. , and the number of roots , , calculate the measured mass percentage of circular cross-section fiber : Step 6: Define the circularity of non-circular cross-section fibers ; Step 7: Establish the circular cross-section fiber ratio and measured values The nonlinear model between them is used to obtain the model parameters by applying the least squares method. , that is, the circularity of fibers with non-circular cross-sections.

[0007] Preferably, the non-circular cross-section fiber in step 1 is selected from cotton fiber, hemp fiber or regenerated cellulose fiber.

[0008] Preferably, the hemp fiber is flax, hemp or ramie, and the regenerated cellulose fiber is viscose or modal.

[0009] Preferably, the circular cross-section fiber in step 2 is selected from lyocell fiber, polyester, cashmere or sheep wool, and the circularity is set to 1.

[0010] Preferably, the cotton fibers in step one include non-mercerized cotton and mercerized cotton, and mercerized cotton with different mercerization degrees has different degrees of roundness.

[0011] Preferably, in step 3, the mass percentage of the circular cross-section fiber is The calculation formula is: ; In the formula, is the mass percentage of circular cross-section fiber, %.

[0012] Preferably, in step 5, the measured mass percentage of the circular cross-section fiber is The calculation formula is as follows: ; Where: is the measured mass of the fiber with non-circular cross section, mg; is the measured mass of the circular cross-section fiber, mg; is the measured mass percentage of circular cross-section fiber, %.

[0013] Preferably, in step 6, the circularity of the non-circular cross-section fiber is defined according to the following formula: : ; Where: It is the circularity of non-circular cross-section fibers, ranging from 0 to 1.

[0014] Preferably, in step seven, according to the following formula, Get model parameters .

[0015] The beneficial effects of the present invention are: The present invention measures the projected width and number of fibers of non-circular cross-section and circular cross-section respectively by mixing non-circular cross-section and circular cross-section fibers in different mass proportions, defines the circularity of fibers of non-circular cross-section, establishes a nonlinear model between the ratio value and the measured value of circular cross-section fibers, and applies the least square method to obtain the characteristic parameter circularity of fibers of non-circular cross-section. The present invention innovatively establishes a circularity test method for fibers of non-circular cross-section. On the one hand, it provides an objective and scientific characterization method for the circularity of fibers of non-circular cross-section, and on the other hand, it helps to solve the quantitative analysis problem of blended products of fibers of non-circular cross-section and circular cross-section, and this solution has the advantages of energy saving and environmental protection. It is not limited to evaluating the circularity of fibers with non-circular cross-sections. Mercerized cotton with different mercerization degrees has different circularity. By measuring the circularity of mercerized cotton with different mercerization processes (alkali mercerization, liquid ammonia mercerization, yarn mercerization, fabric mercerization, double mercerization), it can be used to evaluate the mercerization degree of mercerized cotton with different mercerization processes. It is not limited to evaluating the circularity of non-circular cross-section fibers, but is also applicable to the quantitative analysis of blended products of non-circular cross-section fibers and circular cross-section fibers. DETAILED DESCRIPTION

[0016] The present invention relates to a method for testing the circularity of a fiber with a non-circular cross section, comprising the following steps: Step 1: Select the non-circular cross-section fiber to be tested. The non-circular cross-section fiber is selected from cotton fiber, hemp fiber (flax, hemp, ramie), regenerated cellulose fiber (viscose, modal), etc. The circularity is between 0-1; Step 2: Select circular cross-section fibers, such as lyocell fibers, polyester fibers (polyester), cashmere fibers, sheep wool, etc., and set the circularity to 1; Step 3: Use a Hastelloy slicer to cut short fiber segments of 0.2-0.4 mm in length from the non-circular cross-section fibers and circular cross-section fibers of different types to be tested, and use a 1 / 10,000 balance to weigh a certain mass of the non-circular cross-section fibers. and circular cross-section fibers , mixed into a series of fiber mixtures with different mass ratios, the following formula is used to calculate the mass percentage of circular cross-section fiber : ; In formula (1), is the mass percentage (%) of circular cross-section fiber.

[0017] Step 4: put the fiber mixture of different mass proportions in step 3 into a watch glass, add appropriate amount of liquid paraffin and dispersant, stir thoroughly to form a uniformly mixed fiber suspension, take a certain amount of the suspension with a pipette, transfer it to a glass slide, and prepare a sample observation slide; Step 5: Place the sample observation film on the microscope stage and measure the projection width of the relevant fibers respectively. , and the number of roots , , the following formula is used to calculate the measured mass percentage of circular cross-section fiber : ; In formula (2-4): is the measured mass of the fiber with non-circular cross section (mg); is the measured mass of the circular cross-section fiber (mg); is the measured mass percentage (%) of circular cross-section fibers.

[0018] Step 6: Define the circularity of non-circular cross-section fibers according to the following formula: : ; In formula (5): It is the circularity of non-circular cross-section fibers, ranging from 0 to 1.

[0019] Step 7: Establish the circular cross-section fiber ratio and measured values The nonlinear model between them is used to obtain the model parameters by applying the least squares method. , that is, the circularity of non-circular cross-section fibers: . Example 1

[0020] The present invention relates to a method for testing the circularity of a fiber with a non-circular cross section, comprising the following steps: Step 1, selecting cotton fiber as the non-circular cross-section fiber to be tested; Step 2, selecting polyester as the circular cross-section fiber; Step 3: Use a Hastelloy slicer to cut short fiber segments of 0.4 mm in length from the cotton fiber and the polyester fiber, respectively, and use a 1 / 10,000 balance to weigh a certain mass of the cotton fiber and the polyester fiber, respectively, and mix them into a series of fiber mixtures with different mass ratios, and record the mass percentage of the polyester fiber; Step 4: put the fiber mixture of different mass proportions in step 3 into a watch glass, add appropriate amount of liquid paraffin and dispersant, stir thoroughly to form a uniformly mixed fiber suspension, take a certain amount of the suspension with a pipette, transfer it to a glass slide, and prepare a sample observation slide; Step 5: Place the sample observation film on the microscope stage, measure the projection width and number of relevant fibers, and calculate the measured mass percentage of polyester fibers; Step 6: Establish a nonlinear model between the polyester fiber ratio and the measured value, and apply the least squares method to obtain the model parameters , that is, the circularity of cotton fiber is 0.76 (see Table 1).

[0021] Table 1 Cotton fiber / polyester Example 2

[0022] The present invention relates to a method for testing the circularity of a fiber with a non-circular cross section, comprising the following steps: Step 1, selecting mercerized cotton as the non-circular cross-section fiber to be tested; Step 2, selecting polyester as the circular cross-section fiber; Step 3: Use a Hastelloy slicer to cut short fiber segments of 0.4 mm in length from the mercerized cotton fiber and the polyester fiber, respectively, and use a 1 / 10,000 balance to weigh a certain mass of the mercerized cotton fiber and the polyester fiber, respectively, and mix them into a series of fiber mixtures with different mass ratios, and record the mass percentage of the polyester fiber; Step 4: put the fiber mixture of different mass proportions in step 3 into a watch glass, add appropriate amount of liquid paraffin and dispersant, stir thoroughly to form a uniformly mixed fiber suspension, take a certain amount of the suspension with a pipette, transfer it to a glass slide, and prepare a sample observation slide; Step 5: Place the sample observation film on the microscope stage, measure the projection width and number of relevant fibers, and calculate the measured mass percentage of polyester fibers; Step 6: Establish a nonlinear model between the polyester fiber ratio and the measured value, and apply the least squares method to obtain the model parameters , that is, the roundness of mercerized cotton is 0.92 (see Table 2).

[0023] Table 2 Mercerized cotton / polyester Example 3

[0024] The present invention relates to a method for testing the circularity of a fiber with a non-circular cross section, comprising the following steps: Step 1, select viscose as the non-circular cross-section fiber to be tested; Step 2, selecting Lyocell as the circular cross-section fiber; Step 3: Use a Hastelloy slicer to cut short fiber segments of 0.4 mm in length from viscose and lyocell respectively, use a 1 / 10,000 balance to weigh a certain mass of viscose and lyocell respectively, mix them into a series of fiber mixtures with different mass ratios, and record the mass percentage of lyocell; Step 4: put the fiber mixture of different mass proportions in step 3 into a watch glass, add appropriate amount of liquid paraffin and dispersant, stir thoroughly to form a uniformly mixed fiber suspension, take a certain amount of the suspension with a pipette, transfer it to a glass slide, and prepare a sample observation slide; Step 5: Place the sample observation film on the microscope stage, measure the projection width and number of relevant fibers, and calculate the measured mass percentage of Lyocell; Step 6: Establish a nonlinear model between the lyocell ratio and the measured value, and apply the least squares method to obtain the model parameters. , that is, the circularity of viscose fiber is 0.83 (see Table 3).

[0025] Table 3 Viscose / Lyocell

[0026] It can be seen from the test results of Examples 1-3 that the circularity testing method for non-circular cross-section fibers established by the present invention, on the one hand, provides an objective and scientific characterization method for the circularity of non-circular cross-section fibers, and on the other hand, helps to solve the problem of quantitative analysis of blended products of non-circular cross-section fibers and circular cross-section fibers.

[0027] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A method for testing the circularity of a fiber with a non-circular cross section, characterized in that: The following steps are involved: Step 1, selecting a non-circular cross-section fiber to be tested; Step 2: Select circular cross-section fiber; Step 3: Use a Hastelloy slicer to cut short fiber segments of 0.2-0.4 mm in length from the non-circular cross-section fibers and circular cross-section fibers of different types to be tested, and weigh a certain mass of the non-circular cross-section fibers. and circular cross-section fibers , mixed into a series of fiber mixtures with different mass ratios, and the mass percentage P of the circular cross-section fiber is obtained. : Step 4: Put the fiber mixture of different mass proportions in step 3 into a watch glass, add an appropriate amount of solvent, stir thoroughly to form a uniformly mixed fiber suspension, take a certain amount of the suspension with a pipette, transfer it to a glass slide, and prepare a sample observation slide; Step 5: Place the sample observation film on the microscope stage and measure the projection width of the relevant fibers respectively. , and the number of roots , , calculate the measured mass percentage of circular cross-section fiber : Step 6: Define the circularity of non-circular cross-section fibers : Step 7: Establish the circular cross-section fiber ratio and measured values The nonlinear model between them is used to obtain the model parameters by applying the least squares method. , that is, the circularity of fibers with non-circular cross-sections.

2. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: The non-circular cross-section fiber in step 1 is selected from cotton fiber, hemp fiber or regenerated cellulose fiber.

3. The method for testing the circularity of a fiber with a non-circular cross section according to claim 2, characterized in that: The hemp fiber is flax, hemp or ramie, and the regenerated cellulose fiber is viscose or modal.

4. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: The circular cross-section fiber in step 2 is selected from lyocell fiber, polyester, cashmere or sheep wool, and the circularity is set to 1.

5. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: The cotton fiber in step 1 includes non-mercerized cotton and mercerized cotton, and mercerized cotton with different mercerization degrees has different roundness.

6. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: In the step 3, the mass percentage of the circular cross-section fiber is The calculation formula is: ; In the formula, is the mass percentage of circular cross-section fiber, %.

7. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: Step 5: Measured mass percentage of circular cross-section fiber The calculation formula is as follows: ; Where: is the measured mass of the fiber with non-circular cross section, mg; is the measured mass of the circular cross-section fiber, mg; is the measured mass percentage of circular cross-section fiber, %.

8. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: In step 6, the circularity of the non-circular cross-section fiber is defined according to the following formula: : ; Where: It is the circularity of non-circular cross-section fibers, ranging from 0 to 1.

9. The method for testing the circularity of a fiber with a non-circular cross section according to claim 1, characterized in that: In step seven, according to the following formula, Get model parameters .

Citation Information

Patent Citations

  • Quantitative representation method for physical structure of carbon fiber

    CN109540945A

  • Polyester-cotton fiber blending ratio measurement method based on roundness algorithm

    CN110006898A

  • Quantitative analysis method for fiber content in lyocell fiber blended product

    CN111521612A

  • Cellulosic fiber blended product quantitative analysis method

    CN113063782A

  • Method for measuring degree of fibrillation in fibrous material in powder

    JP2000055904A