Design and preparation method of Ti-Mo-based alloy with good strength and plasticity matching

By designing Ti-11Mo-5Al-4V-3.5Cr metastable beta titanium alloy in titanium alloy, combined with arc melting, water quenching, cold rolling and hot rolling, the problem of low tensile strength and elongation of titanium alloy is solved. Material properties of high strength and high plasticity are achieved.

CN118762779APending Publication Date: 2024-10-11NANJING UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410740854.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing titanium alloys are difficult to meet the tensile strength requirements higher than 1200MPa, and their elongation is low, which limits the application of high-strength beta titanium alloys.

Method used

A metastable beta titanium alloy was designed. By selecting the Ti-Mo-Al-V-Cr system in the titanium alloy system, and using the phase stability diagram and Mo equivalent calculation method, it was determined that the Mo equivalent was between 8% and 30%. The alloy composition is Ti-11Mo-5Al-4V-3.5Cr. It adopts arc melting, water quenching, cold rolling and solution treatment processes, combined with hot rolling treatment, to form a metastable beta titanium alloy with high strength and high plasticity.

Benefits of technology

The high yield strength and maximum tensile strength of titanium alloy are achieved up to 1296MPa, the maximum elongation reaches 18.8%, and the high-strength plastic matching performance of the material is maintained under the optimized processing method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118762779A_ABST
    Figure CN118762779A_ABST
Patent Text Reader

Abstract

The invention discloses design and preparation of a metastable beta titanium alloy with high strength and plasticity matching, and belongs to the field of alloy design and preparation. Based on a Ti-Mo-Al-V-Cr titanium alloy system, isomorphous elements Mo and V and an eutectoid element Cr can significantly strengthen a beta matrix and refine the grain size, and Al serving as an alpha stable element also has a strengthening effect on the alloy, especially alpha nano precipitation. According to the method, a TWIP deformation zone of a Bo-Md phase diagram is selected, and the deformation zone generally shows high yield and good plasticity. According to the Mo equivalent calculation criterion, high Mo content shows high yield. Component design is carried out by utilizing two design criteria of a Bo-Md stable phase diagram and Mo equivalent, and the designed alloy is Ti-11Mo-5Al-4V-3.5 Cr. The raw materials of the alloy are proportioned according to the proportion and are smelted in a vacuum arc furnace to prepare the alloy. And through cold rolling, hot rolling and hot rolling short-time tempering, the metastable beta-state titanium alloy with matched strong plasticity is designed and manufactured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal materials and relates to a design of a metastable β-state titanium alloy with high strength and high plasticity and a preparation method thereof. Background Art

[0002] Titanium and titanium alloys are another important structural metal material after steel and aluminum alloys, and are known as the "third metal" and "flight metal". Titanium alloys have the advantages of low density, high specific strength, high temperature resistance, excellent corrosion resistance, and good biocompatibility. They are widely used in aerospace, marine engineering, biomedicine, and automobiles.

[0003] At present, two-phase structure titanium alloys represented by TC4 are difficult to meet the tensile strength requirements of more than 1200MPa; on the other hand, the rapid development of the aviation industry has put forward higher requirements for the plasticity of high-strength structural titanium alloys. β-titanium alloy has good aging strengthening effect, strong hardenability, excellent cold and hot processing performance, and can obtain excellent mechanical properties through reasonable deformation heat treatment process, and has gradually become an ideal material for high-strength structural titanium alloys. In the past few decades, domestic and foreign researchers have focused on improving the strength-plasticity matching of alloys by adjusting the chemical composition of titanium alloys and optimizing the alloy heat treatment process, in order to obtain structural β-titanium alloys with high strength and reasonable plasticity. At present, the high-strength titanium alloys on various aerospace vehicles are mainly near-β-type, with a strength of 1400-1500MPa, but the elongation is usually less than 10%, and the uniform elongation is even less than 0.2%. Therefore, optimizing the alloy deformation heat treatment process can only improve the strength-plasticity matching of the alloy to a certain extent, and cannot fundamentally solve the current situation of low elongation of β-titanium alloys, which greatly limits the application of high-strength β-titanium alloys. Therefore, how to prepare ultra-high strength and toughness β titanium alloy has become an important research topic in the field of titanium alloy research. Summary of the invention

[0004] The purpose of the present invention is to provide a method for designing, preparing and processing a metastable β titanium alloy having excellent properties of high strength and high plasticity.

[0005] Ingredients Design:

[0006] There are three main design methods commonly used for titanium alloys: Mo equivalent method, d-electron theoretical alloy design method and electron concentration method. In the late 1980s, Japanese scholar Morinaga proposed to select two parameters of elements with d electron orbitals, namely the binding energy Md of d electrons (reflecting electronegativity) and the number of d electron binding Bo (reflecting the d orbital electron binding strength), to characterize the comprehensive influence of factors such as element atomic size, electronegativity and binding energy. For alloys with specific compositions, the Bo and Md values ​​of each alloying element are taken as the weighted average according to their atomic percentage, which is the alloy's and The titanium alloy designed by the present invention and The value is located in the TWIP deformation zone, which will exhibit excellent yield strength, strain hardening rate and elongation; the Mo equivalent between 8% and 30% is called metastable β-type titanium alloy, which has higher strength and plasticity in the solid solution state.

[0007] According to the above two-phase principle, the technical route adopted in designing this invention is as follows:

[0008] Step 1, in the titanium alloy system, there are α-stabilizing elements and β-stabilizing elements, Mo and V are β-isomorphic elements, and Cr is a eutectoid element that can significantly strengthen the β matrix and refine the grain size. Al is an α-stabilizing element, which is conducive to the precipitation of α-nanophase. The α-nanoprecipitate has high hardness and has a strengthening effect on the alloy, which is determined to be a Ti-Mo-Al-V-Cr system;

[0009] Step 2, In the phase stability diagram, different and The values ​​are used to divide different deformation zones. The present invention selects the TWIP deformation zone. The TWIP deformation zone usually exhibits lower yield strength, significant strain hardening and better elongation.

[0010] Step 3, maintaining the Mo equivalent between 8% and 30% according to the Mo equivalent calculation method;

[0011] Step 4, based on the two criteria of step 2 and step 3, reversely infer the specific composition of the titanium alloy, and determine that the titanium alloy of the present invention is Ti-11Mo-5Al-4V-3.5Cr. is 2.7728, is 2.3420, and Mo equivalent is 14.28;

[0012] Preparation and conventional processing methods:

[0013] The technical route adopted to prepare high-strength and plastic-matched titanium alloy is as follows:

[0014] Step 1, preparing a Ti-11Mo-5Al-4V-3.5Cr alloy ingot by an arc melting method;

[0015] Step 2, the ingot is placed in a muffle furnace, heated to 1000°C and kept at this temperature for 3 hours, and then quickly water quenched;

[0016] Step 3, using an electric spark cutting machine to cut the ingot from step 2 into cubic blocks with a size of 15*15*6mm;

[0017] Step 4, cold rolling the cubic block obtained in step 3, with a pressing amount of 0.1 mm each time and a total cold rolling deformation of 80%;

[0018] Step 5, taking the alloy sheet with a thickness of 1.2 mm obtained in step 4, and cutting a bone-shaped tensile specimen using an electric spark cutting machine;

[0019] Step 6, placing the tensile specimen in a muffle furnace for solution treatment and rapidly quenching with water;

[0020] Preferably, the metastable β alloy is expressed as Ti-11Mo-5Al-4V-3.5Cr in terms of mass ratio (wt%), wherein the Mo element accounts for 11% (wt%), the Al element accounts for 5% (wt%), the V element accounts for 4% (wt%), the Cr element accounts for 3.5% (wt%), and the remaining component is Ti.

[0021] Preferably, in step 1, the specific steps are as follows: according to the target alloy composition, 99.99% high-purity raw materials are polished to remove surface oxide scale, and the total mass is prepared to be 20 to 25 g. The raw materials are placed in a high vacuum arc melting furnace, and the alloy is homogenized by arc melting and homogenized 6 times to obtain an alloy ingot.

[0022] Preferably, in step 2, the ingot obtained in step 1 is placed in a quartz tube, the quartz tube is evacuated to a vacuum state and sealed, the ingot is placed in a muffle furnace, the temperature is raised to 1000° C. with the furnace, and the temperature is kept for 3 hours, followed by water quenching.

[0023] Preferably, in step 4, room temperature rolling is performed, with positive and negative rolling alternately performed, with a reduction of 0.1 mm in each rolling pass, and nearly 50 passes in total, until the sample thickness reaches 80% of the total deformation.

[0024] Preferably, in step 6, the cut tensile specimen is placed in a quartz tube, the quartz tube is evacuated to a vacuum state and sealed, and then placed in a muffle furnace heated to the solution temperature, kept warm for 30 minutes, and quickly water quenched.

[0025] Optimized processing methods:

[0026] Step 1. Perform the same operation as steps 1 to 3 in the preparation and processing method to obtain a 15*15*6mm cube;

[0027] Step 2. Place the cubes in step 1 at 750°C for 10 minutes;

[0028] Step 3. The heated cubic block in step 2 is hot rolled at 750°C, with a pressing amount of 0.1 mm each time and a total deformation of 80%;

[0029] Step 4. Take the 1.2 mm alloy sheet obtained in step 3 and cut out a bone-shaped tensile specimen using an electric spark cutting machine;

[0030] Step 5. Place the tensile specimen in a muffle furnace for short-term tempering at 800°C.

[0031] Preferably, in step 2, the phase transition temperature of the alloy of the present invention is 788±5°C, and the temperature of the muffle furnace is raised to 750°C, which is slightly lower than the phase transition temperature.

[0032] Preferably, in step 3, hot rolling is performed at 750° C., the temperature is kept at 750° C. for 1 min, the thickness is rolled by 0.1 mm, the rolling process time is 15 to 25 s, and the front and back sides are rolled alternately and evenly.

[0033] Preferably, in step 5, the cut tensile specimen is placed in a quartz tube, the quartz tube is evacuated to a vacuum state and sealed, and then placed in a muffle furnace heated to the tempering temperature, kept warm for a short time, and quickly water quenched.

[0034] Compared with the prior art, the present invention has the following advantages:

[0035] 1. The present invention is used for the first time Based on the two principles of phase stability diagram and Mo equivalent calculation, the reverse design is based on the metastable β titanium alloy with (Ti-Mo-Al-V-Cr) as the main component. and The value is located at The TWIP deformation zone of the phase stability diagram usually shows lower yield strength, significant strain hardening and good elongation. The Mo value is 14.28, which is a metastable β-type titanium alloy. The metastable β-type titanium alloy has higher strength and plasticity in the solid solution state.

[0036] 2. The metastable β titanium alloy of the present invention can have good plasticity under the condition of retaining high yield after high temperature recrystallization under room temperature rolling. After recrystallization at 1000°C for 30 minutes, the tensile yield strength is 1227MPa, the maximum tensile strength is 1296MPa, and the maximum elongation is 18.8%. The titanium alloy with high strength and plasticity matching is obtained, and the room temperature rolling and solution test are easy and simple to operate.

[0037] 3. In the optimization processing method, the present invention demonstrates a hot rolling treatment method. The rolling temperature is slightly lower than the phase transition temperature. During the rolling process, the second item precipitated will hinder the recrystallization of the grains and improve the material properties. After hot rolling at 750°C, the yield strength is 1131MPa, the maximum tensile strength is 1309MPa, and the maximum elongation is 18.1%. After water quenching at 800°C for 5 minutes, the yield strength is 1093MPa, the maximum tensile strength is 1184MPa, and the maximum elongation is 22.5%. Compared with hot rolling after solid solution, it has better maximum tensile strength. High temperature short-time tempering still maintains a yield of 1093MPa, and the maximum elongation is increased by 4%. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 yes Phase stability diagram, according to and Different values ​​are used to divide different deformation zones. The present invention selects the experimental point B2 in the TWIP deformation zone. The composition is designed to be Ti-11Mo-5Al-4V-3.5Cr metastable β titanium alloy.

[0039] Figure 2 This is the true stress-strain curve of the Ti-11Mo-5Al-4V-3.5Cr metastable β titanium alloy in the cast state. The tensile yield strength is 885MPa, the maximum tensile strength is 901MPa, and the maximum elongation is 16.3%.

[0040] Figure 3 This is the true stress-strain curve after room temperature rolling and solution treatment. After room temperature rolling, high temperature recrystallization is carried out at 1000°C for 30 minutes. The material has a tensile yield strength of 1227MPa, a maximum tensile strength of 1296MPa, and a maximum elongation of 18.8%.

[0041] Figure 4 This is the true stress-strain curve of hot rolling at 750℃ and tempering at 800℃ for 5min. High temperature recrystallization at 1000℃ for 30min. After hot rolling at 750℃, the yield strength is 1131MPa, the maximum tensile strength is 1309MPa, and the maximum elongation is 18.1%. After water quenching at 800℃ for 5min, the yield strength is 1093MPa, the maximum tensile strength is 1184MPa, and the maximum elongation is 22.5%.

[0042] Figure 5 This is a TEM image of the alloy of the present invention after hot rolling at 750°C.

[0043] Figure 6 Yes, the XRD patterns after room temperature rolling at 1000℃ solution (1000), hot rolling at 750℃ (750HR), and hot rolling at 750℃ and short time tempering at 800℃ (750HR-800). Specific implementation methods

[0045] The technical solution of the present invention is further described below with specific implementation methods. The following embodiments are all implemented under the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given, but the protection scope of the present invention is not limited to the following embodiments.

[0046] Example 1

[0047] Step 1, Phase stability diagram Figure 1 As shown in Figure 2, the TWIP deformation zone is selected. and The weighted average value of the value is calculated according to its atomic percentage, which is the alloy and The specific calculation formula is as follows:

[0048]

[0049]

[0050] Wherein xi, (Bo)i and (Md)i represent the atomic percentage of alloy element i, Bo and Md values ​​respectively.

[0051] Table 1 Common alloying elements Bo and Md values ​​in β titanium alloys

[0052]

[0053]

[0054] Step 2: Maintain the Mo equivalent between 8% and 30%. The Mo equivalent (MoE) calculation formula is as follows:

[0055] MoE=1.0Mo+0.67V+0.44W+0.28Nb+0.22Ta+2.5Fe

[0056] +1.25Cr+1.25Ni+1.70Mn+1.70Co-1Al

[0057] Step 3, according to the two-phase criterion of step 2 and step 3, reversely infer the specific composition of the titanium alloy, and determine that the titanium alloy of the present invention is Ti-11Mo-5Al-4V-3.5Cr. is 2.7728, is 2.3420, and Mo equivalent is 14.28;

[0058] Example 2

[0059] Step 1: Prepare raw materials according to the titanium alloy composition.

[0060] Ultrasonic cleaning: Use a grinding gun to remove the surface oxide scale of high-purity Ti, Mo, Al, V, and Cr alloys, and prepare a titanium alloy with a total mass of 20 to 25 g according to their mass percentage. Then put it into a container and add alcohol cleaning solution. Use ultrasonic cleaning for 3 minutes. After taking it out, blow off the residual cleaning solvent to obtain the required raw material.

[0061] Step 2: Place the material in a high vacuum arc melting furnace, use high-purity argon to clean the furnace body, reduce the content of adverse gases in the furnace chamber, set the working current to 210A, and perform homogenization smelting on the raw materials. Turn the raw materials over after each smelting, and repeat the smelting six times to obtain a Ti-11Mo-5Al-4V-3.5Cr alloy ingot.

[0062] Step 3, placing the ingot obtained in step 2 in a quartz tube, vacuumizing the quartz tube, then sealing the quartz tube, placing the quartz tube in a muffle furnace, heating the furnace to 1000° C., and keeping the temperature for 3 hours. Quickly taking the quartz tube out of the muffle furnace for water quenching.

[0063] Step 4: Use an electric spark cutting machine to cut the ingot from step 3 into cubic blocks with a size of 15*15*6 mm.

[0064] Step 5: Take out the as-cast tensile specimen and conduct tensile test. The mechanical properties are as follows: Figure 2 shown.

[0065] Step 6: Take the block obtained in step 4 and use a rolling mill for rolling. The sample is rolled for multiple passes, with a pressing amount of 0.1 mm each time, and the positive and negative rolling are alternated, with a total rolling amount of 80%, and finally rolled into an alloy sheet with a thickness of 1.2 mm.

[0066] Step 7, take the alloy sheet obtained in step 6, and use an electric spark cutting machine to cut out a bone-shaped tensile specimen. Place the tensile specimen in a quartz tube, evacuate the quartz tube, and then seal the quartz tube, heat the muffle furnace to 1000° C., place the quartz tube in the muffle furnace and keep it warm for 30 minutes, and quickly take it out of the muffle furnace after the insulation is completed, and water quench it.

[0067] Step 8, the tensile test specimen after rolling and solid solution obtained in step 7 is subjected to a tensile test, and the mechanical properties are as follows: Figure 3 shown.

[0068] Example 3

[0069] Steps 1-4 are as described in Example 2.

[0070] Step 5, take the cube obtained in step 4 and keep it at 750°C for 10 minutes.

[0071] Step 6: hot-roll the heated cubes in step 5 at 750°C. Keep at 750°C for 1 minute, roll 0.1mm, and the rolling process time is 15-25 seconds. The front and back sides are rolled alternately and evenly, and the total deformation is 80%. Finally, the alloy sheet with a thickness of 1.2mm is rolled.

[0072] Step 7, take the alloy sheet obtained in step 6, and use an electric spark cutting machine to cut out a bone-shaped tensile specimen. The rolled alloy is subjected to TEM analysis, such as Figure 5 As shown in the figure, according to Fourier transform analysis, the microstructure after hot rolling at 750℃ is α+β dual-phase microstructure.

[0073] Step 8, place the tensile specimen in step 7 in a muffle furnace at 800°C, keep it warm for 5 minutes, and quickly cool it with water.

[0074] In step 9, the tensile test specimens in steps 7 and 8 are subjected to tensile tests, and the mechanical properties are as follows: Figure 4 shown.

[0075] Example 4

[0076] The alloy subjected to solution treatment in Example 2, hot rolling and hot rolling high temperature short time tempering in Example 3 was subjected to XRD detection. The results are as follows: Figure 6 shown.

Claims

1. A method for designing a metastable β titanium alloy with high strength and plasticity matching, comprising the following steps: Step 1, determining the Ti-Mo-Al-V-Cr titanium alloy system; Step 2, according to Phase stability diagram, located at a selected point in the TWIP deformation zone, using and The calculation formula can reversely infer the alloy composition; Step 3, according to the Mo equivalent calculation method, adjusting the proportion of the alloy so that its Mo equivalent conforms to the metastable β titanium alloy; Step 4: Under the criteria of step 2 and step 3, determine that the alloy of the present invention is Ti-11Mo-5Al-4V-3.5Cr.

2. The method according to claim 1, characterized in that In step 1, Mo and V are β isomorphous elements, and Cr is a eutectoid element that can significantly strengthen the β matrix and refine the grain size. Al is an α stabilizing element, which is conducive to the precipitation of α nanophase. The α nanoprecipitate has high hardness and has a strengthening effect on the alloy. is 2.7728, According to the Mo equivalent calculation method, the Mo equivalent of the titanium alloy of the present invention is 14.

28.

3. A preparation method and conventional processing method of a metastable β titanium alloy with high strength and plasticity matching, wherein the titanium alloy is a Ti-11Mo-5Al-4V-3.5Cr alloy, comprising the following steps: Step 1, preparing high-purity raw materials according to the designed composition, and using an arc melting method to obtain an alloy ingot; Step 2, placing the ingot from step 1 in a muffle furnace, heating it to 1000° C. and keeping it at that temperature for 3 hours, and then quickly water quenching it; Step 3, using an electric spark cutting machine to cut the ingot from step 2 into cubes that are easy to roll, keeping the surface flat; Step 4, rolling the ingot obtained in step 3 at room temperature, with a total rolling deformation of 80%; Step 5, taking the alloy sheet obtained in step 4, and cutting out a bone-shaped tensile specimen using an electric spark cutting machine; Step 6, placing the tensile specimen obtained in step 5 in a muffle furnace for solution treatment, and taking it out for rapid water quenching.

4. The method according to claim 3, characterized in that In step 1, the Mo element accounts for 11% (wt%), the Al element accounts for 5% (wt%), the V element accounts for 4% (wt%), the Cr element accounts for 3.5% (wt%), and the remaining component is Ti. In step 4, multiple rolling passes are performed, each rolling pass has a reduction of 0.1 mm, and the front and back sides are alternately rolled evenly.

5. A processing method for optimizing the strength and plasticity of a metastable β titanium alloy comprises the following steps: Step 1. Perform the same operation as steps 1 to 3 in claim 3 to obtain a cube that is easy to roll; Step 2. Place the cube in step 1 at a temperature close to the phase transition temperature and keep it warm for 10 to 30 minutes; Step 3. The heated cubic block in step 2 is hot rolled at a temperature close to the phase transition temperature, with a pressing amount of 0.1 mm each time and a total deformation amount of 80%; Step 4. Take the alloy sheet obtained in step 3 and cut out a bone-shaped tensile specimen using an electric spark cutting machine; Step 5. Place the tensile specimen in a muffle furnace for high temperature and short time tempering.

6. The method according to claim 5, characterized in that In step 3, the temperature is kept at the near phase transition temperature for 1 minute, and the thickness is rolled by 0.1 mm. The rolling process time is 15 to 25 seconds, and the front and back sides are rolled alternately and evenly. In step 5, the tensile specimen is placed in a muffle furnace for high temperature tempering.

7. Mechanical experiments on the tensile specimens in claims 3 and 5 can show that a high-strength and plastically matched titanium alloy is obtained.

Citation Information

Patent Citations

  • High-strength and high-plasticity beta titanium alloy with TRIP / TWIP effect and preparation method thereof

    CN107723510A

  • Ti6Al7Nb titanium alloy sheet and preparation method thereof

    CN111346920A

  • Ti-V-Mo-Zr-Cr-Al series high-strength metastable beta titanium alloy and manufacturing method thereof

    CN112662912A

  • High-toughness low-modulus titanium / beta-titanium alloy multilayer composite material and preparation method thereof

    CN113385671A

  • Tissue property regulation and control method for high strength and toughness matching of near-beta titanium alloy

    CN116536602A