Anion-doped positive electrode material, preparation method thereof and battery

By introducing anion doping into lithium-ion battery cathode materials and utilizing halogen elements to distribute in transition metal oxides, the problem of poor cycle stability of nickel-rich cathode materials is solved and higher battery cycle performance and endurance are achieved.

CN118763218APending Publication Date: 2024-10-11JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411069634.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing nickel-rich cathode materials for lithium-ion batteries have poor performance in terms of energy density and cycle stability, making it difficult to meet the range requirements of electric vehicles.

Method used

The anion-doped cathode material is doped with halide twice to form a material including transition metal oxide and lithium oxide. The halogen element is distributed in the transition metal oxide, inhibiting the transformation of the layered structure and oxygen release, and enhancing the Structural and thermal stability of materials.

Benefits of technology

The cycle performance and stability of the cathode material are significantly improved, the battery's cruising range is extended, and the capacity retention rate for 100 weeks reaches over 94.2%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763218A_ABST
    Figure CN118763218A_ABST
Patent Text Reader

Abstract

The invention provides an anion-doped positive electrode material, a preparation method thereof and a battery. The anion-doped positive electrode material comprises a transition metal oxide, a lithium oxide and halogen elements distributed in the transition metal oxide and the lithium oxide, the preparation method comprises the following steps: (1) mixing a positive electrode precursor and a first halogen element source, and carrying out first sintering treatment to obtain a modified precursor; (2) mixing a lithium source and the modified precursor obtained in the step (1), and carrying out second sintering treatment to obtain a sintered material; and (3) mixing a second halogen element source and the sintered material obtained in the step (2), and carrying out third sintering treatment to obtain the anion-doped positive electrode material. The negative ions are introduced into the positive electrode material in a two-step sintering manner, so that the electrochemical stability of the nickel-rich positive electrode material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an anion-doped positive electrode material, a preparation method thereof, and a battery. Background Art

[0002] The global number of plug-in hybrid vehicles and pure electric vehicles has increased year by year, but there has always been "range anxiety" about the endurance of electric vehicles. How to extend the range of electric vehicles is one of the main directions of the development of high-performance battery materials.

[0003] Currently, Ni-Co-Mn ternary oxide materials (NCMs) are considered to be the most ideal cathode materials for lithium-ion batteries (LIBs) due to their high energy density, good cycle performance, safety performance and relatively low cost.

[0004] The battery performance of lithium-ion batteries is closely related to the performance of their positive electrode, but the energy density and cycle stability of the traditional nickel-rich NCM positive electrode or NCA positive electrode are relatively poor compared with those of the graphite anode.

[0005] Therefore, it is necessary to develop new nickel-rich cathode materials to improve the cycling stability of lithium-ion batteries. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides an anion-doped positive electrode material and a preparation method and a battery thereof. The positive electrode material is obtained by doping with halides twice, thereby improving the cycle performance, stability and safety of the positive electrode material.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides an anion-doped positive electrode material, wherein the anion-doped positive electrode material comprises a transition metal oxide and a lithium oxide, and a halogen element distributed in the transition metal oxide and the lithium oxide.

[0009] It is worth noting that in the deep charged state, Co 4+ In Ni 4+ Previously reduced, the formed Co 2+Occupies the tetrahedral position. This prolongs the further migration of Ni, prevents the transformation of the layered structure to the rock salt phase, and delays the release of oxygen, thereby improving the structure of the material and the related thermal stability. In order to solve the problems of deterioration of cycle and rate performance, thermal instability, etc. caused by the increase of Ni content and the decrease of Co / Mn content in the NCM system, from the basic goal of improving the overall structural stability and reducing electrode / electrolyte side reactions, element doping is the main strategy to solve these problems. It has been proven by various experiments that the performance of NCM ternary positive electrode materials can be significantly improved by anion and cation doping. Electrochemically inert ions can replace unstable nickel ions, thereby reducing the degree of mixing between Ni and Li, and inhibiting the irreversible phase change during the delithiation process and the phase change occurring during the cycle. Common cation doping elements are generally W, Zr, Ce, Mo, Ta or Nb, etc. These doped elements induce Ni 2+ The formation of and its migration to the Li layer, as well as the presence of spinel or rock salt phase before cycling, help improve the cycle stability. The present invention uses anion doping to stabilize the doping structure by replacing oxygen ions in the NCM positive electrode material to form a stronger chemical bond with the transition metal ions, ultimately improving the cycle stability of the positive electrode material.

[0010] Compared with oxygen atoms, halogen atoms have the advantages of inhibiting the formation of cracks in positive electrode materials and accelerating the migration of lithium ions in transition metals, which can better improve the cycle stability of positive electrode materials.

[0011] Preferably, the particle size of the anion-doped positive electrode material is 10-15 μm, for example, it can be 10 μm, 11 μm, 11.2 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm or 15 μm.

[0012] Preferably, the transition metal oxides in the anion-doped positive electrode material include cobalt oxide, nickel oxide and manganese oxide.

[0013] Preferably, the ratio of the total molar amount of transition metal elements to the molar amount of lithium elements in the anion-doped positive electrode material is 1:(1.01-1.05), for example, it can be 1:1.01, 1:1.02, 1:1.03, 1:1.04 or 1:1.05, etc.

[0014] Preferably, the molar ratio of nickel, cobalt and manganese in the anion-doped positive electrode material is (6-9):(0.1-1.2):(0.1-1.2), wherein the proportion of nickel can be, for example, 6, 6.2, 6.3, 6.5, 6.8, 6.9, 7.0, 7.2, 7.5, 7.8, 8.0, 8.2, 8.5, 8.8 or 9, etc.; the proportion of cobalt can be, for example, 0.8, 0.82, 0.85, 0.88, 0.89, 0.9, 0.92, 0.95, 0.98, 1.0, 1.05, 1.08, 1.1, 1.12, 1.15, 1.18 or 1.2, etc.; the proportion of manganese can be, for example, 0.1, 0.2, 0.3, 0.5, 0.8, 0.9, 1.0, 1.1 or 1.2, etc.

[0015] Preferably, the halogen element comprises any one or a combination of at least two of fluorine, chlorine, bromine or iodine, wherein typical but non-limiting combinations are a combination of fluorine and chlorine, a combination of bromine and chlorine, a combination of fluorine and bromine, a combination of fluorine and iodine, and preferably a combination of fluorine and chlorine.

[0016] Preferably, the content of halogen element in the anion-doped positive electrode material is 0.001-20wt%, for example, it can be 0.001wt%, 0.1wt%, 0.2wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 5wt%, 8wt%, 9wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%, etc.

[0017] The present invention further preferably controls the content of halogen elements in the anion-doped positive electrode material within the above range, which can not only better replace the oxygen atoms in the positive electrode material, thereby adjusting the crystal structure and electrochemical properties of the material, but also avoid the situation where excessive doping of anions leads to decreased structural stability of the positive electrode material, decreased conductivity, or limited ion diffusion.

[0018] In a second aspect, the present invention provides a method for preparing the anion-doped positive electrode material according to the first aspect, the preparation method comprising the following steps:

[0019] (1) mixing a positive electrode precursor and a first halogen element source, and performing a first sintering treatment to obtain a modified precursor;

[0020] (2) mixing a lithium source and the modified precursor described in step (1), and performing a second sintering treatment to obtain a sintered material;

[0021] (3) Mixing the second halogen element source and the sintering material of step (2), and performing a third sintering treatment to obtain the anion-doped positive electrode material.

[0022] The preparation method of anion-doped positive electrode materials provided in the second aspect of the present invention has the following characteristics: A. The halogen source can only be mixed with the positive electrode precursor, and cannot be added to the raw materials for preparing the precursor. This is because the addition of the halogen source easily leads to a decrease in the product performance of the precursor during the co-precipitation preparation of the precursor, while when added to the precursor, a stable precursor compound has been formed at this time, and the effect of adding the halogen source on the positive electrode precursor is relatively small; B. The halogen source is added in two steps before and after the lithium source is mixed, so that lithium is intercalated between the halogen elements, thereby reducing the degree of mixing between Ni and Li, inhibiting the irreversible phase change during the delithiation process and the phase change occurring during the cycle process, and ultimately improving the cycle stability of the positive electrode material; C. In the present invention, sintering treatment is performed after the halogen source and the lithium source are added respectively, wherein the role of the first sintering treatment is to promote the migration of transition metal ions by replacing oxygen with halogen elements. The role of the second sintering treatment is to mix the ternary precursor and the lithium salt into a positive electrode material, and the role of the third sintering treatment is that the halogen element promotes Ni 2+ The migration of ions into the Li layer strengthens the structure of the Li layer by preventing the collapse of the Li layer.

[0023] That is, the present invention can better optimize the structure of the positive electrode material and significantly improve the cycle stability of the anion-doped positive electrode material by adopting the synergistic effect of three-step sintering and adding the halogen element source in two steps before and after the addition of the lithium source.

[0024] Preferably, in step (1), the first halogen element source and the second halogen element source each independently comprise ammonium halide.

[0025] Preferably, the ammonium halide comprises any one of ammonium fluoride, ammonium chloride, ammonium bromide or ammonium iodide or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of ammonium fluoride and ammonium chloride, a combination of ammonium bromide and ammonium chloride, a combination of ammonium fluoride and ammonium bromide, a combination of ammonium iodide and ammonium chloride, and preferably a combination of ammonium fluoride and ammonium chloride.

[0026] The present invention preferably uses ammonium halide, in which ammonium ions can escape in the form of ammonia gas during the sintering process without affecting the performance of the positive electrode material.

[0027] Preferably, the cathode precursor is a cathode precursor prepared by coprecipitation.

[0028] Preferably, the cathode precursor comprises a transition metal hydroxide.

[0029] Preferably, the transition metal hydroxide includes nickel hydroxide, cobalt hydroxide and manganese hydroxide.

[0030] Preferably, the mass percentage of the first halogen element source in the positive electrode precursor is 5-40%, for example, it can be 5%, 6%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38% or 40%, etc.

[0031] The present invention further preferably controls the mass percentage of the first halogen element source in the positive electrode precursor within the above range, which can better improve the cycle stability of the final material.

[0032] Preferably, the mass percentage of the second halogen element source in the sintering material is 5-40%, for example, it can be 5%, 6%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38% or 40%, etc.

[0033] The present invention further preferably controls the mass percentage of the second halogen element source in the positive electrode precursor within the above range, which can better improve the cycle stability of the final material.

[0034] Preferably, the dosage ratio of the first halogen element source to the second halogen element source is 0.8 to 1.2:1, for example, it can be 0.8:1, 0.82:1, 0.85:1, 0.88:1, 0.9:1, 0.92:1, 0.95:1, 0.98:1, 1.0:1, 1.1:1, 1.12:1, 1.15:1, 1.18:1 or 1.2:1, etc. Preferably, the dosage of the two is equivalent, that is, 1:1, so that the distribution of the halogen element is more uniform and the cycle stability of the positive electrode material is higher.

[0035] Preferably, the temperatures of the first sintering treatment and the third sintering treatment are independently 200-600°C, for example, 200°C, 245°C, 289°C, 334°C, 378°C, 423°C, 467°C, 512°C, 556°C or 600°C.

[0036] The present invention preferably controls the sintering temperature within the above range, which can not only avoid the volatilization of the halogen element, but also ensure that the halogen element is doped into the interior and surface of the positive electrode material.

[0037] Preferably, the time for the first sintering treatment and the third sintering treatment is independently 2 to 4 hours, for example, 2 hours, 2.3 hours, 2.5 hours, 2.7 hours, 2.9 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours or 4 hours.

[0038] Preferably, the temperature of the second sintering treatment is 600-1000°C, for example, it can be 600°C, 645°C, 689°C, 734°C, 778°C, 823°C, 867°C, 912°C, 956°C or 1000°C.

[0039] Preferably, the second sintering treatment time is 8 to 20 hours, for example, it can be 8 hours, 10 hours, 11 hours, 12 hours, 14 hours, 15 hours, 16 hours, 18 hours, 19 hours or 20 hours.

[0040] Preferably, the lithium source comprises any one of lithium carbonate, lithium hydroxide or lithium oxide, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of lithium carbonate and lithium hydroxide, a combination of lithium oxide and lithium hydroxide, and a combination of lithium carbonate and lithium oxide.

[0041] Preferably, the preparation method comprises the following steps:

[0042] (1) mixing a positive electrode precursor and ammonium halide, wherein the mass percentage of the ammonium halide in the positive electrode precursor is 5 to 30%, and performing a first sintering treatment at 200 to 600° C. for 2 to 4 hours to obtain a modified precursor;

[0043] (2) mixing a lithium source and the modified precursor described in step (1), and performing a second sintering treatment at 600 to 1000° C. for 8 to 20 hours to obtain a sintered material;

[0044] (3) Mixing ammonium halide and the sintering material of step (2), wherein the mass percentage of ammonium halide in the sintering material is 5-30%, and performing a third sintering treatment at 200-600° C. for 2-4 hours to obtain the anion-doped positive electrode material.

[0045] The present invention has no special limitation on the mixing in the above process, and any device and method for mixing known to those skilled in the art may be used, and may also be adjusted according to the actual process.

[0046] In a second aspect, the present invention provides a battery, comprising the anion-doped positive electrode material described in the first aspect.

[0047] Preferably, the battery is a solid-state sulfide battery.

[0048] Compared with the prior art, the present invention has at least the following beneficial effects:

[0049] (1) The anion-doped positive electrode material provided by the present invention introduces anions into the positive electrode material to form stronger chemical bonds with transition metal ions, thereby improving the cycle performance and stability safety of the battery material;

[0050] (2) The preparation method of the anion-doped positive electrode material provided by the present invention introduces halogen ions by adopting a two-step sintering method before and after the addition of the lithium source, which not only does not affect the formation of the positive electrode material precursor, but also can significantly improve the cycle stability of the positive electrode material. Under preferred conditions, after it is prepared into a CR2032 button battery, the 0.1C first discharge capacity is above 193.9mAh / g, the 1C first discharge capacity is above 172.3mAh / g, and the capacity retention rate for 100 weeks is above 94.2%. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is a SEM image of the anion-doped positive electrode material prepared in Example 1 of the present invention.

[0052] Figure 2 This is an enlarged SEM image of the anion-doped positive electrode material prepared in Example 1 of the present invention.

[0053] Figure 3 It is a SEM picture of the anion-doped positive electrode material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0054] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0055] It should be understood that, in the description of the present invention, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0056] In order to facilitate the experiment, the precursors of the following anion-doped positive electrode materials were prepared by the following means: 130L of pure water, sodium hydroxide solution and ammonia water were added to the reactor and stirred and mixed, and 1.5m 3 / h of nitrogen to control the pH, total alkali and ammonia content of the reactor bottom liquid at 11.6-11.8, 15-25g / L and 6-9g / L. Set the initial speed of the reactor to 280rpm, and control the temperature of the reactor at 56℃. Add ternary solution, sodium hydroxide solution and ammonia water to the reactor at a flow rate of 8L / h, 2.7L / h and 1.5L / h respectively. After 8h of startup, introduce 0.5m 3 / h of air. During the reaction stabilization period (24 hours after startup), the pH is controlled at 10.9-11.3, the total alkali and ammonia are controlled at 16-18g / L and 6-7g / L respectively, and the reaction is stopped when D50 grows to the target particle size.

[0057] However, it does not mean that the precursor in the present invention can only be prepared by the above method. Other feasible preparation methods of precursors known to those skilled in the art can be used in the present invention and will not be described in detail here.

[0058] Example 1

[0059] This embodiment provides an anion-doped positive electrode material, and the preparation method of the anion-doped positive electrode material comprises the following steps:

[0060] (1) Mix 20g of dried positive electrode precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2 and 4g NH4F were uniformly coated on a quartz plate, placed in a tubular sintering furnace and subjected to a first sintering treatment at 400°C for 2h to obtain a modified precursor;

[0061] (2) mixing lithium carbonate and the modified precursor described in step (1) according to Li / M=1.02:1 (M represents a transition metal), and performing a second sintering treatment at 800° C. for 12 h to obtain a sintered material;

[0062] (3) Mix 4 g NH4F and the sintering material of step (2), mix them evenly, place them on a quartz plate, put them in a sintering furnace, and perform a third sintering treatment at 600° C. for 2 h to obtain the anion-doped positive electrode material (such as Figures 1-2 shown).

[0063] Example 2

[0064] This embodiment provides an anion-doped positive electrode material, and the preparation method of the anion-doped positive electrode material comprises the following steps:

[0065] (1) Mix 20g of dried positive electrode precursor Ni 0.7 Co 0.2 Mn 0.1 (OH)2 and 1g NH4Cl were uniformly coated on a quartz plate, placed in a tubular sintering furnace and subjected to a first sintering treatment at 600°C for 2h to obtain a modified precursor;

[0066] (2) mixing lithium hydroxide and the modified precursor described in step (1) according to Li / M=1.05:1 (M represents a transition metal), and performing a second sintering treatment at 1000° C. for 8 h to obtain a sintered material;

[0067] (3) Mix 1.2 g NH4Cl and the sintering material of step (2), mix them evenly and place them on a quartz plate evenly coated with the mixture, put them in a sintering furnace, and perform a third sintering treatment at 200° C. for 4 h to obtain the anion-doped positive electrode material with a particle size D50 of 12 μm.

[0068] Example 3

[0069] This embodiment provides an anion-doped positive electrode material, and the preparation method of the anion-doped positive electrode material comprises the following steps:

[0070] (1) Mix 20g of dried positive electrode precursor Ni 0.9 Co 0.01 Mn 0.09 (OH)2 and 8g NH4Cl were uniformly coated on a quartz plate, placed in a tubular sintering furnace and subjected to a first sintering treatment at 200°C for 4h to obtain a modified precursor;

[0071] (2) mixing lithium oxide and the modified precursor described in step (1) according to Li / M=1.01:1 (M represents a transition metal), and performing a second sintering treatment at 600° C. for 20 hours to obtain a sintered material;

[0072] (3) Mix 8 g of NH4Cl and the sintering material described in step (2), mix them evenly and place them on a quartz plate evenly coated with the mixture, put them in a sintering furnace, and perform a third sintering treatment at 600°C for 2 h to obtain the anion-doped positive electrode material with a particle size D50 of 15 μm.

[0073] Example 4

[0074] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that of Embodiment 1 except that NH4F is replaced by NH4Cl in step (1) and step (3), and will not be described again.

[0075] Example 5

[0076] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that of Embodiment 1 except that NH4F in step (1) and step (3) is replaced by NH4Br, and the details are not repeated here.

[0077] Example 6

[0078] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that of Embodiment 1 except that NH4F in step (1) and step (3) is replaced by NH4I positive electrode material, and the details are not repeated here.

[0079] Example 7

[0080] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that in Embodiment 1 except that the amount of NH4F in step (1) and step (3) is 0.5 g, and the rest is not repeated here.

[0081] Example 8

[0082] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that of Embodiment 1 except that 10 g of NH4F is used as the positive electrode material in step (1) and step (3), and will not be described in detail here.

[0083] Example 9

[0084] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that of Embodiment 1 except that NH4F in the positive electrode material in step (1) is replaced by NH4Cl, and the details are not repeated here.

[0085] Example 10

[0086] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that of Embodiment 1 except that NH4F is replaced by NH4Cl positive electrode material in step (3), and will not be described again.

[0087] Embodiment 11

[0088] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that in Embodiment 1, except that 4gNH4F in step (1) and step (3) is replaced by 2gNH4Cl+2gNH4F positive electrode material, and is not described again.

[0089] Example 12

[0090] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that in Embodiment 1 except that the temperature of the first sintering treatment in the preparation method is 700° C., and will not be described in detail here.

[0091] Example 13

[0092] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that in Embodiment 1 except that the temperature of the first sintering treatment in the preparation method is 100° C., and will not be described in detail here.

[0093] Embodiment 14

[0094] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that in Embodiment 1 except that the temperature of the third sintering treatment in the preparation method is 700° C., and will not be described in detail here.

[0095] Embodiment 15

[0096] This embodiment provides an anion-doped positive electrode material. The anion-doped positive electrode material is the same as that in Embodiment 1 except that the temperature of the third sintering treatment in the preparation method is 100° C., and will not be described again.

[0097] Comparative Example 1

[0098] This comparative example provides a positive electrode material. The positive electrode material is the same as that of Example 1 except that NH4F is not added in steps (1) and (3). The description is omitted here. Figure 3 shown.

[0099] Comparative Example 2

[0100] This comparative example provides a positive electrode material. The positive electrode material is the same as that of Example 1 except that no NH4F is added in step (1) and 8g NH4F is added in step (3). The details are not described here.

[0101] Comparative Example 3

[0102] This comparative example provides a positive electrode material. The positive electrode material is the same as that of Example 1 except that no NH4F is added in step (3) and 8g NH4F is added in step (1), and thus will not be described in detail.

[0103] Comparative Example 4

[0104] This comparative example provides a positive electrode material. The positive electrode material is the same as that of Example 1 except that the first sintering treatment is not performed in step (1), and the details are not described again.

[0105] Comparative Example 5

[0106] This comparative example provides a positive electrode material. The positive electrode material is the same as that of Example 1 except that the third sintering treatment is not performed in step (3), and details thereof will not be repeated here.

[0107] The results of this test are all the results of the test with the power off. The specific steps are as follows: weigh the positive electrode material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 and dissolve them in N-methylpyrrolidone (NMP) and mix them evenly; then, use a coater to apply the slurry on aluminum foil and dry it in a vacuum drying oven at 80°C for 8 hours. Finally, punch the aluminum foil into 1.13cm 2The positive electrode sheet was obtained by forming a circular shape. The obtained electrode sheet was used as the positive electrode, the lithium metal sheet was used as the counter electrode, and a porous polypropylene membrane (Celgard2400, USA) was used as a separator to separate the positive electrode and the counter electrode. The CR2032 button battery was assembled in an argon glove box. The cycle performance test was carried out at 2.5V to 4.55V at a rate of 0.1C and 1C using a battery test system (Blue Electric CT2001A, Wuhan, China). The test results are shown in Table 1.

[0108] The test results of the above embodiments and comparative examples are shown in Table 1.

[0109] Table 1

[0110]

[0111]

[0112] From Table 1, we can see the following points:

[0113] (1) It can be seen from Examples 1 to 6 and Examples 9 to 11 that the anion-doped positive electrode material provided by the present invention has excellent long-term cycle stability. After being prepared into a CR2032 button battery, the 0.1C first discharge capacity is above 193.9 mAh / g, the 1C first discharge capacity is above 172.3 mAh / g, and the capacity retention rate for 100 weeks is above 94.2%;

[0114] (3) Combining Example 1 and Examples 7 to 8, it can be seen that in Example 1, the amount of NH4F in step (1) and step (3) is 4 g, compared with 0.5 g of NH4F in step (1) and step (3) in Example 7, and 10 g of NH4F in step (1) and step (3) in Example 8. In Example 1, the 0.1C first discharge capacity is 197.5 mAh / g, the 1C first discharge capacity is 175.3 mAh / g, and the capacity retention rate for 100 weeks is 96.7%, while in Examples 7 to 8, the amount of NH4F in step (1) and step (3) is 0.5 g, and the amount of NH4F in step (1) and step (3) is 10 g. 8, the capacity retention rates after 100 weeks are only 93.2% and 93.1%, respectively, which indicates that a high halogen doping element will cause a large number of halogen atoms to occupy the lattice position of the oxide, hindering the migration of metal ions, and a low halogen doping element will cause only a small amount of halogen atoms to replace the oxygen in the oxide, slowing down the migration of transition metal ions and causing the collapse of the Li layer, both of which will affect the cycle performance of the battery. The present invention can be more conducive to improving the cycle performance of the battery by preferably controlling the amount of ammonium halide added within a reasonable range;

[0115] (3) It can be seen from Examples 12 to 15 that the present invention preferably controls the temperature of the first sintering treatment and the third sintering treatment within a specific range, which can better promote the doping of ammonium halide and improve the cycle performance of the battery;

[0116] (4) In Comparative Example 1, ammonium fluoride was not doped, and the capacity retention rate after 100 weeks was only 89.2%. In Comparative Examples 2 and 3, ammonium fluoride was added only in one step, and the capacity retention rates after 100 weeks were only 90.9% and 91.8%, respectively. In Comparative Examples 3 to 4, the first sintering treatment and the third sintering treatment were performed respectively. The first sintering treatment was not performed, resulting in the halogen element being unable to replace oxygen to promote the migration of transition metal ions, affecting the cycle performance; the third sintering treatment was not performed, and the halogen element was unable to promote Ni 2+ The migration of ions to the Li layer and the prevention of the collapse of the Li layer affect the cycle performance; the capacity retention rates after 100 weeks in comparative examples 3 to 4 are only 88.7% and 87.9%, respectively, which shows that the present invention can significantly improve the cycle performance of the battery by adding ammonium halide for doping and adopting a three-step sintering step.

[0117] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An anion-doped positive electrode material, characterized in that: The anion-doped positive electrode material includes transition metal oxide and lithium oxide, and halogen elements distributed in the transition metal oxide and lithium oxide.

2. The anion-doped positive electrode material according to claim 1, characterized in that: The particle size of the anion-doped positive electrode material is 10 to 15 μm; Preferably, the transition metal oxide in the anion-doped positive electrode material includes cobalt oxide, nickel oxide and manganese oxide; Preferably, the ratio of the total molar amount of transition metal elements to the molar amount of lithium elements in the anion-doped positive electrode material is 1:(1.01-1.05); Preferably, the molar ratio of nickel, cobalt and manganese in the anion-doped positive electrode material is (6-9):(0.8-1.2):(0.1-1.2).

3. The anion-doped positive electrode material according to claim 1 or 2, characterized in that: The halogen element includes any one of fluorine, chlorine, bromine or iodine or a combination of at least two, preferably a combination of fluorine and chlorine; Preferably, the content of halogen elements in the anion-doped positive electrode material is 0.001-20 wt %.

4. A method for preparing an anion-doped positive electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) mixing a positive electrode precursor and a first halogen element source, and performing a first sintering treatment to obtain a modified precursor; (2) mixing a lithium source and the modified precursor described in step (1), and performing a second sintering treatment to obtain a sintered material; (3) Mixing the second halogen element source and the sintering material of step (2), and performing a third sintering treatment to obtain the anion-doped positive electrode material.

5. The preparation method according to claim 4, characterized in that: In step (1), the first halogen element source and the second halogen element source each independently comprise ammonium halide; Preferably, the ammonium halide includes any one of ammonium fluoride, ammonium chloride, ammonium bromide or ammonium iodide, or a combination of at least two of them. Preferably, the cathode precursor is a cathode precursor prepared by coprecipitation; Preferably, the cathode precursor comprises a transition metal hydroxide; Preferably, the transition metal hydroxide includes nickel hydroxide, cobalt hydroxide and manganese hydroxide.

6. The preparation method according to claim 4 or 5, characterized in that: The mass percentage of the first halogen element source in the positive electrode precursor is 5 to 40%; Preferably, the mass percentage of the second halogen element source in the sintering material is 5-40%.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The temperatures of the first sintering treatment and the third sintering treatment are independently 200 to 600° C.; Preferably, the time of the first sintering treatment and the third sintering treatment is independently 2 to 4 hours.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The temperature of the second sintering treatment is 600-1000° C.; Preferably, the second sintering treatment takes 8 to 20 hours.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: (1) mixing a positive electrode precursor and ammonium halide, wherein the mass percentage of the ammonium halide in the positive electrode precursor is 5 to 40%, and performing a first sintering treatment at 200 to 600° C. for 2 to 4 hours to obtain a modified precursor; (2) mixing a lithium source and the modified precursor described in step (1), and performing a second sintering treatment at 600 to 1000° C. for 8 to 20 hours to obtain a sintered material; (3) Mixing ammonium halide and the sintering material of step (2), wherein the mass percentage of ammonium halide in the sintering material is 5-40%, and performing a third sintering treatment at 200-600° C. for 2-4 hours to obtain the anion-doped positive electrode material.

10. A battery, characterized in that: The battery comprises the anion-doped positive electrode material according to any one of claims 1 to 3.

Citation Information

Cited By

  • Anion-doped cobaltosic oxide as well as preparation method and application thereof

    CN119370901A

  • Surface-modified high-nickel positive electrode material as well as preparation method and application thereof

    CN119612616A

  • Halogen bulk phase doped cobalt oxide oxygen evolution catalyst and preparation method and application thereof

    CN122189742A