Diaphragm, battery and preparation method thereof

By using the core-shell structure of modified resin and fluorine-containing monomers on the lithium battery separator, the problems of insufficient separator adhesion and high energy consumption in the existing technology are solved, and low-cost, low-energy consumption separator preparation is achieved, improving improve the cycle performance of the battery.

CN118763354APending Publication Date: 2024-10-11JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410756448.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing lithium battery separators consume high energy, are expensive, and have insufficient adhesion during the high-temperature hot pressing process, resulting in poor battery cycle performance.

Method used

Modified resin with a core-shell structure is used as the adhesive layer material. The modified resin and adhesive are coated on the surface of the base film to form a core-shell structure of the modified resin. Fluorine-containing monomers are used to improve the adhesive force and Reduce the swelling rate, avoid hot pressing, and only perform cold pressing.

Benefits of technology

It reduces energy consumption and equipment costs during the cell preparation process, improves the adhesion between the separator and the pole piece, maintains electrolyte resistance and electrochemical stability, and extends the cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004889646370000161
    Figure BDA0004889646370000161
  • Figure BDA0004889646370000171
    Figure BDA0004889646370000171
  • Figure BDA0004889646370000181
    Figure BDA0004889646370000181
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a diaphragm, a battery and a preparation method thereof. The diaphragm comprises a base film layer and a binder layer arranged on at least one side surface of the base film layer, the binder layer comprises modified resin and a binder; the modified resin has a core-shell structure, the core of the modified resin comprises a resin matrix, and the shell of the modified resin comprises a grafting monomer; the resin matrix comprises acrylic resin; the grafting monomer comprises a fluorine-containing monomer. The diaphragm disclosed by the invention can reduce the energy consumption of a hot-pressing process and the equipment cost in a battery cell preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a diaphragm and a battery and a method for preparing the same. Background Art

[0002] As an important component of lithium batteries, the diaphragm blocks the passage of electrons and allows the free shuttle of lithium ions, thereby avoiding short circuits caused by contact between the positive and negative electrodes. The commercialized diaphragm base film materials are mainly polyolefin diaphragms based on polyethylene (PE) and polypropylene (PP). The diaphragm base film itself has poor heat resistance, so a heat-resistant layer (heat-resistant materials such as alumina, boehmite, etc.) is usually coated on its surface to improve the heat resistance of the diaphragm.

[0003] However, the lack of bonding between the diaphragm base film and the diaphragm composite with a heat-resistant layer and the electrode cannot improve the hardness of the battery. For this reason, it is necessary to coat an adhesive layer (glue layer) on the base film or the heat-resistant layer to form a glue-coated diaphragm.

[0004] At present, the glue-coated diaphragm market mainly uses PVDF (polyvinylidene fluoride) and PMMA (polymethyl methacrylate) mixed adhesives to spray or roll on the base film, and then hot presses (90-110°C, 6000kg pressure) after the battery cell is wound to soften and deform the PVDF and PMMA particles, thereby improving the bonding force between the pole piece and the diaphragm and reducing the migration distance of lithium ions. This process has become an indispensable procedure in the battery preparation process, especially in rate charging and discharging. However, this process requires high temperatures and extremely expensive hot pressing equipment, resulting in great energy consumption, so the diaphragm cold pressing process has gradually been taken seriously by the industry.

[0005] At the same time, although PVDF has advantages such as low swelling rate, electrolyte resistance and stable electrochemical performance, PVDF has insufficient bonding strength; PMMA has problems such as large swelling rate of electrolyte and poor fatigue resistance (the expansion of the pole piece during charging and discharging causes the swollen PMMA to deform and fall off). Therefore, the use of PVDF / PMMA mixed binder makes the battery unable to cycle for a long time. Summary of the invention

[0006] In view of this, the present invention provides a diaphragm and a battery and a method for preparing the same. The diaphragm can reduce the energy consumption and equipment cost of the hot pressing process caused during the preparation of the battery core.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] In a first aspect, the present invention provides a diaphragm, the diaphragm comprising a base film layer, and an adhesive layer disposed on at least one side surface of the base film layer;

[0009] The adhesive layer includes a modified resin and an adhesive;

[0010] The modified resin has a core-shell structure, the core of the modified resin includes a resin matrix, and the shell of the modified resin includes a grafted monomer;

[0011] The resin matrix includes acrylic resin;

[0012] The grafting monomer includes a fluorine-containing monomer.

[0013] In an embodiment of the present invention, the polymerizable monomer of the acrylic resin includes at least one of butyl acrylate, isooctyl acrylate, ethyl acrylate, methyl methacrylate, styrene, and vinyl acetate.

[0014] In an embodiment of the present invention, the fluorine-containing monomer includes at least one of 2,3,4,5,6-pentafluorostyrene, butyl trifluoromethylacrylate, 4-fluorostyrene, and perfluoroacrylate monomers.

[0015] Preferably, the perfluoroacrylate monomer includes at least one of perfluoroalkylethyl acrylate, perfluorobutylethyl acrylate, perfluorohexylethyl acrylate and perfluorooctylethyl acrylate.

[0016] Preferably, the mass percentage of the grafted monomer in the modified resin is 8% to 10%;

[0017] Preferably, the average particle size of the modified resin is 2 to 3 μm.

[0018] Preferably, in the adhesive layer, the mass percentage of the modified resin is 80% to 90%, and the mass percentage of the adhesive is 10% to 20%.

[0019] In an embodiment of the present invention, the binder includes but is not limited to at least one of acrylic acid-acrylonitrile copolymer (PAA-PAN), polyacrylic acid, polyacrylonitrile (PAN), and polyvinyl alcohol (PVA).

[0020] Preferably, the coating amount of the adhesive layer on the base film layer is 0.25 to 0.35 g / m 2 .

[0021] In an embodiment of the present invention, the base membrane layer includes a base membrane or a base membrane composited with a ceramic layer.

[0022] In an embodiment of the present invention, in the base film composited with the ceramic layer, the ceramic layer is disposed on at least one surface of the base film.

[0023] In a second aspect, the present invention provides a method for preparing the above-mentioned diaphragm, comprising the following steps:

[0024] Step (1), mixing the modified resin, the binder and the solvent, and performing a dispersion treatment to obtain a binder slurry;

[0025] Step (2), applying the adhesive slurry to at least one side of the surface of the base film layer, and drying to obtain a diaphragm.

[0026] In a third aspect, the present invention provides a battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet; the separator in the battery comprises the above-mentioned separator and / or the separator prepared by the above-mentioned preparation method.

[0027] In a fourth aspect, the present invention provides a method for preparing the above-mentioned battery, comprising the following steps:

[0028] Step (1), stacking a positive electrode sheet, a separator and a negative electrode sheet to obtain a battery cell, or stacking a positive electrode sheet, a separator and a negative electrode sheet and then winding them to obtain a battery cell;

[0029] Step (2), subjecting the battery cell to cold pressing or hot pressing.

[0030] Preferably, the cold pressing treatment temperature is 15-25°C, the pressure is 5-10 MPa, and the time is 20-30 seconds;

[0031] Preferably, the temperature of the hot pressing treatment is 80-100° C., the pressure is 3-8 MPa, and the time is 20-30 seconds.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The separator of the present invention introduces a modified resin with a core-shell structure into the binder layer to replace the currently commonly used thermoplastic materials such as PVDF and PMMA as a binder. The modified resin is based on acrylic resin as the core, and a fluorine-containing monomer is grafted on the molecular chain of the resin matrix to form a core-shell structure.

[0034] Among them, the fluorinated monomer is polymerized in the outermost layer. At room temperature, the fluorinated monomer has anti-stickiness, and can wrap the sticky resin matrix inside the core-shell structure to prevent the diaphragm from sticking to each other when rolling up;

[0035] The glass transition temperature of acrylic resin is -15 to 15°C. It has adhesiveness at room temperature. Under the action of external force (such as cold pressing or hot pressing of the diaphragm), the shell layer of the modified resin is crushed, exposing the inner resin matrix, thereby improving the adhesion between the diaphragm and the electrode.

[0036] Therefore, the diaphragm of the present invention does not need to be subjected to hot pressing operation, and only cold pressing operation can be performed to achieve bonding between the diaphragm and the pole piece, thereby reducing energy consumption and equipment costs.

[0037] (2) The CF chemical bond in the fluorinated monomer in the diaphragm of the present invention is extremely short and has a high bond energy (460 kj / mol), which makes it have excellent chemical stability, solvent corrosion resistance, oxidation resistance and electrochemical stability. Its swelling rate in the electrolyte is low, maintaining good electrolyte resistance and electrochemical stability, thereby reducing the impact of the diaphragm on the cycle performance. That is, the present invention not only maintains the advantages of PVDF, but also avoids the weaknesses of PMMA. DETAILED DESCRIPTION

[0038] The present invention discloses a diaphragm and a battery and a method for preparing the same. A person skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to a person skilled in the art and are deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0039] Terminology explanation:

[0040] Glass transition temperature (Tg) refers to the temperature corresponding to the transition from glassy state to highly elastic state. Glass transition is an inherent property of amorphous polymer materials and a macroscopic manifestation of the change in the form of polymer motion. It directly affects the performance and process performance of the material. The glass transition temperature is the lowest temperature at which the molecular chain segments can move. Its level is directly related to the flexibility of the molecular chain. The greater the flexibility of the molecular chain, the lower the glass transition temperature; the greater the rigidity of the molecular chain, the higher the glass transition temperature. The glass transition temperature is one of the characteristic temperatures of polymers. Above the glass transition temperature, the polymer exhibits elasticity, and below the glass transition temperature, it exhibits brittleness.

[0041] Grafting refers to the reaction of combining appropriate branch chains or functional side groups on the macromolecular chain through chemical bonds. The product formed is called a graft copolymer. The grafting formula of the polymer is mainly composed of resin, grafting monomer, initiator and antioxidant.

[0042] A grafted monomer refers to a molecule that is attached (eg, chemically bonded) to a polymer as a side chain but is not polymerized or copolymerized as part of the polymer backbone.

[0043] The resin matrix refers to the resin component used to form the main body of the modified resin.

[0044] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0045] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0046] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0047] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0048] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0049] In order to reduce the energy consumption and equipment cost of the hot pressing process caused by the preparation of the battery cell, the present invention adopts the following technical solutions:

[0050] In a first aspect, the present invention provides a diaphragm, the diaphragm comprising a base film layer, and an adhesive layer disposed on at least one side surface of the base film layer;

[0051] The adhesive layer includes a modified resin and an adhesive;

[0052] The modified resin has a core-shell structure, the core of the modified resin includes a resin matrix, and the shell of the modified resin includes a grafted monomer;

[0053] The resin matrix includes acrylic resin;

[0054] The grafting monomer includes a fluorine-containing monomer.

[0055] In the embodiment of the present invention, the polymerizable monomer of the acrylic resin includes at least one of butyl acrylate, isooctyl acrylate, ethyl acrylate, methyl methacrylate, styrene, and vinyl acetate. When the polymerizable monomer includes multiple types, the acrylic resin obtained by polymerizing the polymerizable monomers in any proportion can realize the present invention.

[0056] In an embodiment of the present invention, the fluorine-containing monomer includes at least one of 2,3,4,5,6-pentafluorostyrene, butyl trifluoromethylacrylate, 4-fluorostyrene, and perfluoroacrylate monomers.

[0057] Preferably, the perfluoroacrylate monomer includes at least one of perfluoroalkylethyl acrylate, perfluorobutylethyl acrylate, perfluorohexylethyl acrylate and perfluorooctylethyl acrylate.

[0058] Preferably, the mass percentage of the grafted monomer in the modified resin is 8% to 10%. Exemplarily, the mass percentage of the grafted monomer in the modified resin is any one of 8%, 8.5%, 9%, 9.5%, 10%, or any value within the range of any two of the above values. The surface energy of the fluorine-containing monomer is low and has anti-sticking properties. When the mass percentage of the grafted monomer (fluorine-containing monomer) in the modified resin is greater than 10%, when cold pressing or hot pressing is performed during the preparation of the battery cell, the outer shell of the modified resin is not easily crushed, and the sticky resin matrix cannot be exposed, resulting in a decrease in the viscosity of the adhesive layer, thereby affecting the bonding force between the diaphragm and the pole piece; when the mass percentage of the grafted monomer in the modified resin is less than 8%, the modified resin directly exposes more resin matrix, and when the diaphragm is rolled up during the preparation of the diaphragm, the diaphragm will stick together, and the anti-sticking effect cannot be achieved.

[0059] Preferably, the average particle size of the modified resin is 2 to 3 μm. Exemplarily, the average particle size of the modified resin is any value among 2 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, 3 μm, or any value within the range of any two of the above values. When the average particle size of the modified resin is less than 2 μm, when the cold pressing operation is performed during the preparation of the battery cell, the shell of the modified resin is not easily crushed, and the sticky resin matrix cannot be exposed, resulting in a decrease in the viscosity of the adhesive layer, thereby affecting the bonding force between the diaphragm and the pole piece; when the average particle size of the modified resin is greater than 3 μm, the diaphragm will be too thick, which will easily lead to serious misalignment of the pole ear, affecting the quality of the battery cell and the electrical and safety performance of the battery.

[0060] Preferably, in the binder layer, the mass percentage of the modified resin is 80% to 90%, and the mass percentage of the binder is 10% to 20%. Exemplarily, the mass percentage of the modified resin in the binder layer is 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90% or any value in the range of any two of the above values. Exemplarily, the mass percentage of the binder in the binder layer is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or any value in the range of any two of the above values. When the mass percentage of the modified resin exceeds 90%, there is less binder in the binder layer, resulting in the binder layer being unable to adhere to the base film layer.

[0061] In the embodiment of the present invention, the binder includes but is not limited to at least one of acrylic acid-acrylonitrile copolymer (PAA-PAN), polyacrylic acid, polyacrylonitrile (PAN), and polyvinyl alcohol (PVA). The function of the binder is to adhere the modified resin to the base film layer to form a binder layer on the surface of the base film layer. Preferably, acrylic acid-acrylonitrile copolymer (PAA-PAN) is used.

[0062] Preferably, the coating amount of the adhesive layer on the base film layer is 0.25 to 0.35 g / m 2 For example, the coating amount of the adhesive layer on the base film layer is 0.25 g / m 2 , 0.26g / m 2 , 0.27g / m 2 , 0.28g / m 2 , 0.29g / m 2 , 0.3g / m 2 , 0.31g / m 2 , 0.32g / m 2 , 0.33g / m 2 , 0.34g / m 2 , 0.35g / m 2 Any value in or any value in the range consisting of any two of the above values.

[0063] In an embodiment of the present invention, the base membrane layer includes a base membrane or a base membrane composited with a ceramic layer.

[0064] In an embodiment of the present invention, in the base film composited with the ceramic layer, the ceramic layer is disposed on at least one surface of the base film.

[0065] In an embodiment of the present invention, the base film is at least one selected from a polyethylene film, a polypropylene film, a polyimide film, a polyvinylidene fluoride film, a polyvinylidene fluoride-hexafluoropropylene film, a polyamide film, and a polyethylene terephthalate film.

[0066] In an embodiment of the present invention, the ceramic layer comprises a ceramic material.

[0067] In an embodiment of the present invention, the ceramic material includes at least one of aluminum oxide, boehmite, calcium carbonate, hydrotalcite, montmorillonite, titanium dioxide, silicon dioxide, zirconium dioxide, magnesium oxide, magnesium hydroxide, magnesium hydroxide, boron nitride, silicon nitride, aluminum nitride, titanium nitride, boron carbide, silicon carbide, and zirconium carbide.

[0068] In a second aspect, the present invention provides a method for preparing the above-mentioned diaphragm, comprising the following steps:

[0069] Step (1), mixing the modified resin, the binder and the solvent, and performing a dispersion treatment to obtain a binder slurry;

[0070] Step (2), applying the adhesive slurry to at least one side of the surface of the base film layer, and drying to obtain a diaphragm.

[0071] In an embodiment of the present invention, the solvent is water.

[0072] In the embodiment of the present invention, the speed of the dispersion treatment is 3000-8000 r / min, and the time is 30-60 min.

[0073] Preferably, the solid content of the binder slurry is 7% to 10%, the viscosity is 10 to 70 mPa·s, and the pH value is 5 to 8. The solid content of the binder slurry can be adjusted by changing the amount of the solvent.

[0074] In an embodiment of the present invention, the coating method includes spray coating and / or roller coating.

[0075] In an embodiment of the present invention, the drying temperature is 50-60°C.

[0076] In a third aspect, the present invention provides a battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet; the separator in the battery comprises the above-mentioned separator and / or the separator prepared by the above-mentioned preparation method.

[0077] In an embodiment of the present invention, the adhesive layer is disposed on at least one side surface of the base film layer, and preferably the adhesive layer is disposed on both side surfaces of the base film layer.

[0078] In an embodiment of the present invention, when the adhesive layer is disposed on one surface of the base film layer, it is preferred that the adhesive layer of the separator is in contact with the positive electrode sheet.

[0079] In an embodiment of the present invention, the battery comprises a lithium ion battery or a sodium ion battery.

[0080] In an embodiment of the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on at least one side of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material, a positive electrode conductor and a positive electrode binder.

[0081] In the embodiment of the present invention, the mass percentage of each component in the positive electrode active material layer is: 80wt% to 99.8wt% of positive electrode active material, 0.1wt% to 10wt% of positive electrode conductor, and 0.1wt% to 10wt% of positive electrode binder.

[0082] In an embodiment of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on at least one side of the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder.

[0083] In the embodiment of the present invention, the mass percentage of each component in the negative electrode active material layer is: 80wt% to 99.8wt% of negative electrode active material, 0.1wt% to 10wt% of negative electrode conductor, and 0.1wt% to 10wt% of negative electrode binder.

[0084] In an embodiment of the present invention, the positive electrode conductive agent or the negative electrode conductive agent includes but is not limited to at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber.

[0085] In an embodiment of the present invention, the positive electrode binder or the negative electrode binder includes but is not limited to at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.

[0086] In an embodiment of the present invention, the positive electrode active material is selected from one or more of transition metal lithium oxides, lithium iron phosphate, and lithium-rich manganese-based materials.

[0087] In another embodiment of the present invention, the positive electrode active material includes at least one of layered transition metal sodium oxide, sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium cobaltate, sodium manganate, sodium nickelate, and Prussian blue.

[0088] In an embodiment of the present invention, the negative electrode active material includes a carbon-based negative electrode material.

[0089] In an embodiment of the present invention, the carbon-based negative electrode material includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, hard carbon, and soft carbon.

[0090] In an embodiment of the present invention, the negative electrode active material may further include a silicon-based negative electrode material.

[0091] In the embodiment of the present invention, the silicon-based negative electrode material is selected from nano-silicon, silicon-oxygen negative electrode material (SiO x(0 < x < 2)) or at least one of silicon-carbon negative electrode materials.

[0092] The present application has no particular limitation on the preparation methods of the positive electrode sheet and the negative electrode sheet. Those skilled in the art can adopt conventional preparation methods as long as the purpose of the present application can be achieved.

[0093] In an embodiment of the present invention, the battery further includes an outer package.

[0094] In an embodiment of the present invention, the battery further includes an electrolyte.

[0095] The present application has no particular limitation on the organic solvents, electrolyte salts, and additives in the electrolyte. Those skilled in the art can select according to actual needs as long as the purpose of the present application can be achieved.

[0096] Fourthly, the present invention provides a preparation method of the above battery, including the following steps:

[0097] Step (1), laminating the positive electrode sheet, the separator, and the negative electrode sheet to obtain an electrode core, or laminating the positive electrode sheet, the separator, and the negative electrode sheet and then winding them to obtain an electrode core;

[0098] Step (2), performing cold pressing or hot pressing on the electrode core.

[0099] Preferably, the temperature of the cold pressing is 15 - 25°C, the pressure is 5 - 10 MPa, and the time is 20 - 30 s. Exemplarily, the temperature of the cold pressing is any value among 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C or any value within the range value composed of any two of the above values, such as the temperature at room temperature. Exemplarily, the pressure of the cold pressing is any value among 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa or any value within the range value composed of any two of the above values. Exemplarily, the time of the cold pressing is any value among 20 s, 22 s, 24 s, 25 s, 26 s, 28 s, 30 s or any value within the range value composed of any two of the above values.

[0100] Preferably, the temperature of the hot pressing treatment is 80-100°C, the pressure is 3-8MPa, and the time is 20-30s. Exemplarily, the temperature of the hot pressing treatment is any value in 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, 100°C or any value in the range of any two of the above values. Exemplarily, the pressure of the hot pressing treatment is any value in 3MPa, 4MPa, 5MPa, 6MPa, 7MPa, 8MPa or any value in the range of any two of the above values. Exemplarily, the time of the hot pressing treatment is any value in 20s, 22s, 24s, 25s, 26s, 28s, 30s or any value in the range of any two of the above values.

[0101] In the embodiment of the present invention, after the cold pressing treatment or the hot pressing treatment, the process further includes: placing the battery cell in an outer package, injecting electrolyte into the outer package, and obtaining the battery of the present invention.

[0102] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0103] The modified resins used in the following examples are all obtained through commercial channels; they can also be prepared by conventional melt grafting methods.

[0104] The present invention will be further described below in conjunction with embodiments:

[0105] Embodiment 1:

[0106] 1. The raw material composition of the diaphragm in this embodiment:

[0107] (1) Modified resin: 85 parts of 2,3,4,5,6-pentafluorostyrene modified acrylic resin;

[0108] (2) Binder solution: 100 parts of a PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 15 parts of an acrylic acid-acrylonitrile copolymer (PAA-PAN) and 85 parts of water;

[0109] (3) Solvent: 1200 parts of water.

[0110] The grafted monomer (2,3,4,5,6-pentafluorostyrene) in the modified resin accounts for 9% by mass, and the average particle size of the modified resin is 2.5 μm. The polymerized monomers of the acrylic resin in the modified resin include styrene, hydroxyethyl acrylate, butyl acrylate, isooctyl acrylate, acrylic acid and glycidyl methacrylate, and the specific ratio is styrene: hydroxyethyl acrylate: butyl acrylate: isooctyl acrylate: acrylic acid: glycidyl methacrylate = 25:7:125:75:5:20.

[0111] 2. Preparation method of the diaphragm in this embodiment:

[0112] (1) The modified resin, the binder solution and the solvent are mixed, and after high-speed dispersion (8000 r / min, 30 min), a binder slurry with a solid content of 8.1%, a viscosity of 35 mPa·s and a pH of 6.7 is obtained;

[0113] (2) The binder slurry was sprayed on the base film surface and CCS (Ceramic Coated Separator) surface of the diaphragm (purchased from Shanghai Enjie New Materials Technology Co., Ltd., i.e., the base film layer), and dried at 50°C to obtain a diaphragm composited with a binder layer. The single-side coating amount of the binder layer on the base film layer was 0.3 g / m 2 .

[0114] Example 2a:

[0115] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the mass proportion of the grafted monomer in the modified resin is 8%.

[0116] The obtained binder slurry had a solid content of 8.1%, a viscosity of 39 mPa.s, and a pH of 6.5.

[0117] Example 2b:

[0118] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the mass proportion of the grafted monomer in the modified resin is 10%.

[0119] The obtained binder slurry had a solid content of 8.0%, a viscosity of 29 mPa.s, and a pH of 6.9.

[0120] Example 3a:

[0121] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the grafting monomer in the modified resin is replaced by a perfluoroacrylate monomer, i.e., perfluoroalkylethyl acrylate.

[0122] The obtained binder slurry had a solid content of 8.1%, a viscosity of 47 mPa.s, and a pH of 7.0.

[0123] Example 3b:

[0124] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the grafting monomer in the modified resin is replaced by perfluorobutyl ethyl acrylate.

[0125] The obtained binder slurry had a solid content of 7.9%, a viscosity of 36 mPa.s, and a pH of 6.9.

[0126] Example 3c:

[0127] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the grafting monomer in the modified resin is replaced by butyl trifluoromethylacrylate.

[0128] The obtained binder slurry had a solid content of 8.5%, a viscosity of 43 mPa.s, and a pH of 7.1.

[0129] Embodiment 3d:

[0130] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the grafting monomer in the modified resin is replaced by 4-fluorostyrene.

[0131] The obtained binder slurry had a solid content of 8.2%, a viscosity of 41 mPa.s, and a pH of 6.8.

[0132] Embodiment 4a:

[0133] The other conditions of this embodiment are the same as those of embodiment 3a, but the difference from embodiment 3a is that the mass proportion of the grafted monomer in the modified resin is 8%.

[0134] The obtained binder slurry had a solid content of 8.1%, a viscosity of 51 mPa.s, and a pH of 7.1.

[0135] Embodiment 4b:

[0136] The other conditions of this embodiment are the same as those of embodiment 3a, but the difference from embodiment 3a is that the mass proportion of the grafted monomer in the modified resin is 10%.

[0137] The obtained binder slurry had a solid content of 8.1%, a viscosity of 35 mPa.s, and a pH of 7.0.

[0138] Example 5a:

[0139] The other conditions of this embodiment remain unchanged from those of embodiment 1, except that the difference from embodiment 1 is that the polymerization monomers of the acrylic resin in the modified resin are replaced with methyl styrene: hydroxypropyl acrylate: butyl acrylate: isooctyl acrylate: methacrylic acid: glycidyl methacrylate: acrylamide = 50:7.5:125:75:10:7:10.

[0140] The obtained binder slurry had a solid content of 8.5%, a viscosity of 44 mPa.s, and a pH of 7.0.

[0141] Example 5b:

[0142] The other conditions of this embodiment remain unchanged from those of embodiment 1, except that the difference from embodiment 1 is that the polymerization monomers of the acrylic resin in the modified resin are replaced with methyl methacrylate: hydroxyethyl methacrylate: isooctyl acrylate: acrylic acid: vinyl trimethoxysilane: hydroxyethyl acrylamide = 50:7.5:125:10:7:10.

[0143] The obtained binder slurry had a solid content of 7.9%, a viscosity of 39 mPa.s, and a pH of 7.1.

[0144] Example 6a:

[0145] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the raw material ratio of the diaphragm is different.

[0146] (1) Modified resin: 90 parts of 2,3,4,5,6-pentafluorostyrene modified acrylic resin;

[0147] (2) Binder solution: 66.7 parts of PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 10 parts of acrylic acid-acrylonitrile copolymer (PAA-PAN) and 56.7 parts of water;

[0148] (3) Solvent: 1200 parts of water.

[0149] The obtained binder slurry had a solid content of 8.3%, a viscosity of 40 mPa.s, and a pH of 6.8.

[0150] Example 6b:

[0151] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the raw material ratio of the diaphragm is different.

[0152] (1) Modified resin: 80 parts of 2,3,4,5,6-pentafluorostyrene modified acrylic resin;

[0153] (2) Binder solution: 133 parts of PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 20 parts of acrylic acid-acrylonitrile copolymer (PAA-PAN) and 113 parts of water;

[0154] (3) Solvent: 1200 parts of water.

[0155] The obtained binder slurry had a solid content of 8.2%, a viscosity of 66 mPa.s, and a pH of 6.4.

[0156] Example 7a:

[0157] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the average particle size of the modified resin is 2 μm.

[0158] The obtained binder slurry had a solid content of 7.8%, a viscosity of 36 mPa.s, and a pH of 6.8.

[0159] Example 7b:

[0160] The other conditions of this embodiment are the same as those of embodiment 1, but the difference from embodiment 1 is that the average particle size of the modified resin is 3 μm.

[0161] The obtained binder slurry had a solid content of 8.0%, a viscosity of 44 mPa.s, and a pH of 7.1.

[0162] Comparative Example 1:

[0163] The other conditions of this comparative example are the same as those of Example 1, but different from Example 1 in that the modified resin is replaced by a PVDF / PMMA mixed binder, wherein the mass ratio of PVDF to PMMA is 1:1.

[0164] The obtained binder slurry had a solid content of 8.5%, a viscosity of 52.3 mPa.s, and a pH of 7.01.

[0165] Comparative Example 2:

[0166] The other conditions of this comparative example are the same as those of Example 1, except that the modified resin is replaced by unmodified acrylic resin.

[0167] The obtained binder slurry had a solid content of 8.0%, a viscosity of 45.6 mPa.s, and a pH of 6.9.

[0168] Comparative Example 3a:

[0169] The other conditions of this comparative example are the same as those of Example 1, except that the weight percentage of the grafted monomer in the modified resin is 15%.

[0170] The obtained binder slurry had a solid content of 8.2%, a viscosity of 40 mPa.s, and a pH of 7.0.

[0171] Comparative Example 3b:

[0172] The other conditions of this comparative example are the same as those of Example 1, except that the weight percentage of the grafted monomer in the modified resin is 5%.

[0173] The obtained binder slurry had a solid content of 8.1%, a viscosity of 43 mPa.s, and a pH of 6.7.

[0174] Comparative Example 4a:

[0175] The other conditions of this comparative example are the same as those of Example 1, but the difference from Example 1 is that the raw material ratio of the diaphragm is different.

[0176] (1) Modified resin: 95 parts of 2,3,4,5,6-pentafluorostyrene modified acrylic resin;

[0177] (2) Binder solution: 33.3 parts of PAA-PAN binder with a solid content of 15%; the PAA-PAN binder comprises 5 parts of acrylic acid-acrylonitrile copolymer (PAA-PAN) and 28.3 parts of water;

[0178] (3) Solvent: 1200 parts of water.

[0179] The obtained binder slurry had a solid content of 8.1%, a viscosity of 31 mPa.s, and a pH of 6.7.

[0180] Comparative Example 4b:

[0181] The other conditions of this comparative example are the same as those of Example 1, but the difference from Example 1 is that the raw material ratio of the diaphragm is different.

[0182] (1) Modified resin: 75 parts of 2,3,4,5,6-pentafluorostyrene modified acrylic resin;

[0183] (2) Binder solution: 166.7 parts of PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 25 parts of acrylic acid-acrylonitrile copolymer (PAA-PAN) and 141.7 parts of water;

[0184] (3) Solvent: 1200 parts of water.

[0185] The obtained binder slurry had a solid content of 8.1%, a viscosity of 120 mPa.s, and a pH of 5.2.

[0186] Comparative Example 5a:

[0187] The other conditions of this comparative example are the same as those of Example 1, except that the average particle size of the modified resin is 0.75 μm.

[0188] The obtained binder slurry had a solid content of 8.3%, a viscosity of 42 mPa.s, and a pH of 6.8.

[0189] Comparative Example 5b

[0190] The other conditions of this comparative example are the same as those of Example 1, except that the average particle size of the modified resin is 4.5 μm.

[0191] The obtained binder slurry had a solid content of 8.1%, a viscosity of 31 mPa.s, and a pH of 6.8.

[0192] Adhesion comparison test

[0193] The diaphragms prepared in the above examples and comparative examples were subjected to a comparative test of adhesion. The test method is: the coated diaphragm is passed through a winding machine, the positive and negative electrode sheets and the diaphragm are wound together, and then hot pressed or cold pressed (hot pressed: 90°C, 5MPa, 25s; cold pressed: room temperature (20°C), 8MPa, 25s), and the 180° peeling force of the electrode sheet and the diaphragm is tested with a universal tensile machine. The test results are as follows:

[0194] Table 1 Peel force test results

[0195]

[0196]

[0197] Note: Dry adhesion refers to the bonding strength between the diaphragm and the electrode before being immersed in the electrolyte; wet adhesion refers to the bonding strength between the diaphragm and the electrode after being immersed in the electrolyte.

[0198] From the above results, it can be seen that the diaphragms and pole pieces prepared in Examples 1 to 7 have high adhesion. From the results of Example 2a, Example 1, and Example 2b, it can be seen that as the amount of grafted monomer increases, the adhesion decreases. From the results of Example 6a, Example 1, and Example 6b, it can be seen that as the amount of modified acrylate (modified resin) decreases, the adhesion gradually decreases.

[0199] For the diaphragm of Comparative Example 1, due to the presence of PVDF / PMMA, there is almost no adhesion to the electrode after cold pressing.

[0200] The diaphragm of Comparative Example 2 was added with unmodified acrylic resin. The cold and hot pressing bonding strengths met the standards. However, the diaphragms were bonded to each other during winding, and the coating fell off during the later winding, so mass production was not possible.

[0201] Compared with Example 1, the content of grafted monomer in Comparative Example 3a was too high, the adhesive substance in the core was reduced, and the adhesion after hot pressing and cold pressing was significantly reduced. The content of grafted monomer in Comparative Example 3b was too low, and the modified resin directly exposed more acrylic resin. After winding, it was found that the diaphragm was stuck together, affecting production and use.

[0202] Compared with Example 1, the modified resin content in Comparative Example 4a is too high, the bonding force is low, and the adhesive is too little and cannot adhere well to the base film layer. The modified resin content in Comparative Example 4b is too low, and the bonding material with the electrode is less, resulting in low bonding force to the electrode.

[0203] Compared with Example 1, the modified resin in Comparative Example 5a has a smaller particle size, cannot fully contact the pole piece during cold and hot pressing, and has a lower bonding force. The modified resin in Comparative Example 5b has a larger particle size, and under the same solid ratio, the specific surface area is small, the adhesion strength between the resin and the diaphragm is reduced, and the resin is easy to fall off.

[0204] Diaphragm air permeability test

[0205] The air permeability of the above-mentioned embodiment and comparative example was tested using an air permeability meter. The test results are as follows:

[0206] Table 2 Air permeability test results

[0207]

[0208]

[0209] It can be seen from the above results that the diaphragms prepared in Examples 1 to 7 all have good air permeability.

[0210] In Comparative Example 4b, the content of modified acrylic resin is too high, so the air permeability increment after hot pressing and cold pressing is relatively large.

[0211] Swelling rate test

[0212] The adhesive layer film in the diaphragm prepared in the embodiment and the comparative example is placed in an electrolyte solvent (the electrolyte solvent consists of ethylene carbonate (EC), diethyl carbonate (DEC), propyl propionate (PP), and propylene carbonate (PC), and the mass ratio of EC:DEC:PP:PC is 2:2:3:3), immersed at 45°C for 24 hours, the floating liquid on the surface of the film is wiped off, the weight of the film after immersion is weighed, and the weight gain rate is calculated to obtain the swelling rate.

[0213] Table 3 Swelling rate test results

[0214]

[0215]

[0216] Note: In Comparative Example 1, PVDF and PMMA adhesives were tested separately. The PVDF item tested the swelling rate of PVDF powder, and the PMMA item tested the swelling rate of the adhesive film made by drying PMMA liquid adhesive.

[0217] From the above results, it can be seen that the fluorine-containing monomer-modified acrylates in Examples 1 to 7 all have a good swelling rate, which means that they can be better dissolved and mixed with the substrate during coating, and have stronger adhesive ability and better bonding.

[0218] In Comparative Example 1, PMMA has a high swelling rate, which will affect the conductivity between the active material and the current collector, causing battery capacity decay.

[0219] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A diaphragm, It is characterized in that The diaphragm includes a base film layer, and an adhesive layer disposed on at least one side surface of the base film layer; The adhesive layer includes a modified resin and an adhesive; The modified resin has a core-shell structure, the core of the modified resin includes a resin matrix, and the shell of the modified resin includes a grafted monomer; The resin matrix includes acrylic resin; The grafting monomer includes a fluorine-containing monomer.

2. The diaphragm according to claim 1, It is characterized in that The polymerizable monomer of the acrylic resin includes at least one of butyl acrylate, isooctyl acrylate, ethyl acrylate, methyl methacrylate, styrene and vinyl acetate; The fluorine-containing monomer includes at least one of 2,3,4,5,6-pentafluorostyrene, butyl trifluoromethylacrylate, 4-fluorostyrene, and perfluoroacrylate monomers; Preferably, the perfluoroacrylate monomer includes at least one of perfluoroalkylethyl acrylate, perfluorobutylethyl acrylate, perfluorohexylethyl acrylate and perfluorooctylethyl acrylate.

3. The diaphragm according to claim 1, It is characterized in that The mass percentage of the grafted monomer in the modified resin is 8% to 10%; Preferably, the average particle size of the modified resin is 2 to 3 μm.

4. The diaphragm according to claim 1, It is characterized in that In the adhesive layer, the mass percentage of the modified resin is 80% to 90%, and the mass percentage of the adhesive is 10% to 20%.

5. The diaphragm according to claim 1, It is characterized in that The binder includes at least one of acrylic acid-acrylonitrile copolymer, polyacrylic acid, polyacrylonitrile and polyvinyl alcohol.

6. The diaphragm according to claim 1, It is characterized in that The coating amount of the adhesive layer on the base film layer is 0.25 to 0.35 g / m 2 .

7. The diaphragm according to any one of claims 1 to 6, It is characterized in that The base film layer includes a base film or a base film composited with a ceramic layer; In the base film composited with a ceramic layer, the ceramic layer is disposed on at least one surface of the base film.

8. A method for preparing the diaphragm according to any one of claims 1 to 7, It is characterized in that The steps include: The modified resin, the binder and the solvent are mixed and dispersed to obtain a binder slurry; The binder slurry is applied to at least one surface of the base film layer and dried to obtain a diaphragm.

9. A battery, It is characterized in that The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet, and the separator comprises the separator according to any one of claims 1 to 7 and / or the separator prepared by the preparation method according to claim 8.

10. A method for preparing the battery according to claim 9, It is characterized in that The steps include: The positive electrode sheet, the separator and the negative electrode sheet are stacked to obtain a battery cell, or the positive electrode sheet, the separator and the negative electrode sheet are stacked and then wound to obtain a battery cell; The battery cell is subjected to cold pressing or hot pressing; Preferably, the temperature of the cold pressing treatment is 15-25°C, the pressure is 5-10MPa, and the time is 20-30s; Preferably, the temperature of the hot pressing treatment is 80-100° C., the pressure is 3-8 MPa, and the time is 20-30 seconds.

Citation Information

Patent Citations

  • Binder composition for non-aqueous secondary cell function layer, slurry composition for non-aqueous secondary cell function layer, function layer for non-aqueous secondary cell, separator provided with function layer for non-aqueous secondary cell, non-aqueous secondary cell, and method for producing same

    CN110383530A

  • Composition for nonaqueous secondary battery functional layers, battery member for nonaqueous secondary batteries, method for producing laminate for nonaqueous secondary batteries, and nonaqueous secondary battery

    CN111492505A

  • Composition for nonaqueous secondary battery functional layers, battery member for nonaqueous secondary batteries, method for producing laminate for nonaqueous secondary batteries, and nonaqueous secondary battery