Polyethylene powder and method for producing same, and catalyst for olefin polymerization and method for producing same
By controlling the viscosity-average molecular weight and other physical properties of polyethylene powder, a microporous membrane with excellent heat resistance, membrane uniformity and dimensional stability was prepared, solving the problem of insufficient heat resistance of polyethylene powder in microporous membranes for secondary battery separators in the prior art.
Patent Information
- Application Number
- CN202380023600.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-11
AI Technical Summary
When existing polyethylene powder is used to make microporous membranes for secondary battery separators, it lacks sufficient heat resistance, membrane uniformity, and dimensional stability, and cannot meet the requirements for high heat resistance.
By controlling the viscosity-average molecular weight of polyethylene powder between 100,000 and 400,000, and combining differential scanning calorimetry (DSC) and gel permeation chromatography (GPC) to determine the crystal thickness parameters, z-mean shrinkage factor, peak temperature, and absorption coefficient of polyethylene powder within a specific range, a microporous membrane with excellent heat resistance, membrane uniformity, and high heat resistance rate was prepared.
This study significantly improved the heat resistance, membrane uniformity, and dimensional stability of polyethylene powder when it was used to make microporous membranes, thus meeting the requirements for high heat resistance.
Smart Images

Figure BDA0005009570930000061 
Figure BDA0005009570930000091 
Figure BDA0005009570930000211
Abstract
Description
Technical Field
[0001] The present invention relates to polyethylene powder and a method for producing the same, and a catalyst for olefin polymerization and a method for producing the same. Background Art
[0002] Ethylene polymers are used for various purposes such as films, sheets, microporous membranes, fibers, foams, tubes, etc. As the reason for using ethylene polymers, because melt processing is easy, the obtained molded body has high mechanical strength, and chemical resistance, rigidity, etc. are also excellent. Among them, ultra-high molecular weight ethylene polymers have higher mechanical strength due to their large molecular weight, excellent sliding properties and wear resistance, and excellent chemical stability and long-term reliability. Considering this point, ultra-high molecular weight polyethylene powder is used as the raw material of microporous membrane for secondary battery separators, especially represented by lead-acid batteries and lithium-ion batteries.
[0003] As the raw material of secondary battery separator microporous film etc., various ethylene polymers with improved characteristics are proposed.For example, in patent document 1, it is proposed that the specific ratio of the heat of fusion obtained by the intrinsic viscosity in the specified range and under specific measurement conditions using differential scanning calorimeter (DSC) is more than the specific lower limit, so that the ethylene polymer of the molded body (for example, stretched molded body, microporous film) with excellent oxidation resistance and shrinkage resistance can be provided.In addition, for example, in patent document 2, it is proposed that the manufacture method of the supported metallocene catalyst of the polyolefin polymer that can improve the apparent density of the polymer while maintaining the characteristics of the high-activity catalyst and the manufacture method of the polyolefin using the supported metallocene catalyst.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6383479
[0007] Patent Document 2: Japanese Patent Application No. 2017-518423 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In recent years, the requirements for microporous membranes for secondary battery separators have increased rapidly, and polyethylene physical properties are required to be further improved. Specifically, for example, polyethylene that can provide microporous membranes with excellent heat resistance, uniformity of the membrane, dimensional stability and high heat resistance rate is required, but the polyethylene described in Patent Documents 1 and 2 has room for improvement in such physical properties.
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polyethylene powder which is excellent in heat resistance, film uniformity, dimensional stability and high heat resistance rate when formed into a microporous film.
[0011] Means used to solve problems
[0012] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems and have found that by controlling the specified physical properties of polyethylene powder with a specified viscosity-average molecular weight within a specific range, a microporous membrane with excellent heat resistance, film uniformity, dimensional stability and high heat resistance rate can be provided, thereby completing the present invention.
[0013] That is, the present invention is as follows.
[0014] [1] A polyethylene powder, wherein the viscosity average molecular weight of the polyethylene powder is 100,000 or more and 4,000,000 or less,
[0015] The crystal thickness parameter of the polyethylene powder measured using a differential scanning calorimeter (DSC) is 5° C. or more and 9° C. or less.
[0016] [2] The polyethylene powder according to [1], wherein the z-average shrinkage factor g of the polyethylene powder measured by a gel permeation chromatography (GPC) measuring device combined with a differential refractometer and a viscosity detector is z The value of is greater than or equal to 0.600 and less than or equal to 1.
[0017] [3] The polyethylene powder according to [1], wherein in the DSC curve of the second heating process of the polyethylene powder obtained by measurement using a differential scanning calorimeter (DSC) as shown in the following <Measurement Conditions>, the peak temperature (Tm2 top ) is 135°C or higher and 140°C or lower, and the crystal thickness parameter is 6.7°C or higher and 9.0°C or lower.
[0018] <Measurement conditions>
[0019] (1) Stand at 50°C for 1 minute
[0020] (2) Heating from 50°C to 180°C at 10°C / min (first heating process)
[0021] (3) Stand at 180°C for 5 minutes
[0022] (4) Cooling from 180°C to 50°C at 10°C / min
[0023] (5) Stand at 50°C for 5 minutes
[0024] (6) Heating from 50°C to 180°C at 10°C / min (second heating process)
[0025] [4] The polyethylene powder according to any one of [1] to [3], wherein the polyethylene powder can be stretched under the following conditions:
[0026] (Stretching conditions)
[0027] A gel sheet of 100 mm×100 mm×1 mm in thickness containing 30% by mass of polyethylene powder and 70% by mass of liquid paraffin was stretched to 7×7 times at 115°C.
[0028] [5] The polyethylene powder according to any one of [1] to [4], wherein in terahertz measurement, the 400 cm -1 ~450cm -1 The absorption coefficient within the range of is greater than or equal to 1.0 and less than or equal to 4.0.
[0029] [6] The polyethylene powder according to any one of [1] to [5], wherein 1 In the H-NMR measurement, there is no peak in the region shown below,
[0030] (1) 4.8ppm~5.0ppm
[0031] (2)5.6ppm~6.0ppm.
[0032] [7] The polyethylene powder according to any one of [1] to [6], wherein the aluminum content in the polyethylene powder is 0 ppm to 50 ppm.
[0033] [8] The polyethylene powder according to any one of [1] to [7], wherein the silicon content in the polyethylene powder is 0 ppm or more and 30 ppm or less.
[0034] [9] The polyethylene powder according to [1] or [2], wherein in differential scanning calorimetry (DSC) measurement of the polyethylene powder, the temperature of the peak top in the DSC curve in the second heating process is 130° C. or higher and 140° C. or lower.
[0035]
[10] The polyethylene powder according to any one of [1] to [9], wherein the density of the polyethylene powder is 920 kg / m 3 Above and 960kg / m 3 the following.
[0036]
[11] The polyethylene powder according to any one of [1] to
[10] , wherein the polyethylene powder is used for a battery separator.
[0037]
[12] A method for producing an olefin polymerization catalyst, wherein the method for producing an olefin polymerization catalyst comprises the following steps:
[0038] A first supporting reaction step, wherein the inorganic solid particles [A] are reacted with the transition metal compound [B-1] and / or the transition metal compound component [B-2], the activator [C] and / or the organometallic compound component [D]; and
[0039] A second supporting reaction step, wherein the particles obtained in the first supporting reaction step are reacted with a transition metal compound component [B-1] and / or a transition metal compound component [B-2], an activator [C] and / or an organometallic compound component [D],
[0040] The transition metal compound [B-1] is a compound represented by the following (Formula 3), the transition metal compound [B-2] is a compound represented by the following (Formula 4), the activator [C] is a compound represented by the following (Formula 5) or (Formula 6), the organometallic compound component [D] is a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, the inorganic solid particles [A] are porous polymer materials or inorganic solid particles containing at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table,
[0041] The method for producing the olefin polymerization catalyst satisfies the following <Condition 1> and / or <Condition 2>:
[0042] <Condition 1>
[0043] The first loading reaction step includes the following steps:
[0044] a premixing step of reacting the transition metal compound [B-1] and / or the transition metal compound component [B-2] with the activator [C] and / or the organometallic compound component [D]; and
[0045] A step of reacting the inorganic solid particles [A] with the mixture obtained in the pre-mixing step.
[0046] <Condition 2>
[0047] In the first loading reaction step, the molar ratio (([C]+[D]) / [B]) of the molar amount ([C]+[D]) of the activator [C] and the organometallic compound component [D] to the molar amount [B] of the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is greater than 1 and less than 60.
[0048] L 1 j W k M 1 X 1p X 2 q ……(Formula 3)
[0049] (In Formula 3, L 1 each independently represents an n-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group and an octahydrofluorenyl group, wherein the ligand has 1 to 8 substituents as the case may be, and the substituents are each independently selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogenated hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms and a halogenated silyl group and having 20 or less non-hydrogen atoms,
[0050] M 1 represents a transition metal selected from the group of transition metals belonging to Group 4 of the Periodic Table of the Elements having a formal oxidation number of +2, +3 or +4 and having an η5 bond with at least one ligand L,
[0051] W represents a divalent substituent having 50 or less non-hydrogen atoms and bonding to each of L and M with a univalent valency to form a metal ring compound together with L and M,
[0052] X 1 each independently represents an anionic sigma-bonded ligand having 60 or less non-hydrogen atoms selected from the group consisting of a monovalent anionic sigma-bonded ligand, a divalent anionic sigma-bonded ligand divalently bonded to M, and a divalent anionic sigma-bonded ligand monovalently bonded to each of L and M,
[0053] X 2 each independently represents a neutral Lewis base coordinating compound having 40 or less non-hydrogen atoms,
[0054] j is 1 or 2, wherein when j is 2, the two ligands L are bonded to each other through a divalent group having 20 or less non-hydrogen atoms, the divalent group being a group selected from the group consisting of a hydrocarbon diyl group having 1 to 20 carbon atoms, a halogenated hydrocarbon diyl group having 1 to 12 carbon atoms, an alkyleneoxy group having 1 to 12 carbon atoms, an alkyleneamino group having 1 to 12 carbon atoms, a silanediyl group, a halogenated silanediyl group, and a silyleneamino group, k is 0 or 1, p is 0, 1 or 2, wherein in X 1 In the case of a monovalent anionic σ-bonding type ligand or a divalent anionic σ-bonding type ligand bonded to L and M, p is an integer smaller than the formal oxidation number of M by 1 or more, and in the case of X 1In the case of a divalent anionic σ-bonded ligand that bonds only to M, p is an integer that is smaller than the formal oxidation number of M by (j+1) or more, and q is 0, 1, or 2.
[0055]
[0056] (In Formula 4, M 2 represents a transition metal selected from the group consisting of titanium, zirconium and hafnium and having a formal oxidation number of +2, +3 or +4,
[0057] R 5 Each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein in the substituent R 5 When it is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group or a germyl group, two adjacent substituents R 5 bonded to each other to form a divalent group, thereby bonding to the two adjacent substituents R 5 The bonds between the two carbon atoms of the cyclopentadienyl ring to which each is bonded together form a ring,
[0058] X 3 Each independently represents a substituent selected from the group consisting of a halogen ion, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbonoxy group having 1 to 18 carbon atoms, a hydrocarbonamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbonamide group having 1 to 18 carbon atoms, a hydrocarbonphosphine group having 1 to 18 carbon atoms, a hydrocarbonthio group having 1 to 18 carbon atoms, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein two substituents X may be selected from the group consisting of 3 Together they form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms,
[0059] Y 1 Indicates -O-, -S-, -NR 6 -or-PR 6 -, where R 6 represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbonoxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof,
[0060] Z 1 SiR 6 2 , CR 6 2 、SiR 6 2 S i 6 2 , CR 62 CR 6 2 , CR 6 =CR 6 , CR 6 2 S i 6 2
[0061] or GeR 6 2 , where R 6 As defined above,
[0062] n is 1, 2, or 3. )
[0063] (C-1): [L 2 -H] d+ [M 3 r Q s ] d- ……(Formula 5)
[0064] (In Formula 5, [L 2 -H] d+ For proton-donating Bronsted acids, L 2 is a neutral Lewis base. In addition, in Formula 5, [M 3 r Q s ] d- is a compatible non-coordinating anion, M 3 is a metal or metalloid selected from Groups 5 to 15 of the periodic table, Q is independently a hydride ion, a dialkylamino group, a halide ion, an alkoxy group, an allyloxy group, a hydrocarbon group, or a substituted hydrocarbon group having 20 or less carbon atoms, and the number of Q as a halide ion is 1 or less. In addition, r is an integer of 1 to 7, s is an integer of 2 to 14, d is an integer of 1 to 7, and sr=d.)
[0065] (C-2): -(M 4 R 7 t-2 -O) u -……(Formula 6)
[0066] (In Formula 6, M 4 is a metal or metalloid of Group 13 to Group 15 of the Periodic Table, R 7 are each independently a hydrocarbon group having 1 to 12 carbon atoms or a substituted hydrocarbon group having 1 to 12 carbon atoms, and t is a metal M 4 valence, u is an integer greater than 2. )
[0067]
[13] The method for producing an olefin polymerization catalyst according to
[12] , wherein the inorganic solid particles [A] are magnesium chloride particles.
[0068]
[14] An olefin polymerization catalyst, comprising inorganic solid particles [A], a transition metal compound component [B-1] and / or a transition metal compound component [B-2], and an activator [C] and / or an organic metal compound component [D],
[0069] The transition metal compound [B-1] is a compound represented by the following (Formula 3), the transition metal compound [B-2] is a compound represented by the following (Formula 4), the activator [C] is a compound represented by the following (Formula 5) or (Formula 6), the organometallic compound component [D] is a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, the inorganic solid particles [A] are porous polymer materials or inorganic solid particles containing at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table,
[0070] The content (molar) of the central metal M contained in the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is greater than 20 micromoles and less than 1000 micromoles, and the molar ratio (Al / M) of the content (molar) of the central metal M to the content (molar) of Al is greater than 1 and less than 30.
[0071] L 1 j W k M 1 X 1 p X 2 q ……(Formula 3)
[0072] (In Formula 3, L 1 each independently represents an n-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group and an octahydrofluorenyl group, wherein the ligand has 1 to 8 substituents as the case may be, and the substituents are each independently selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogenated hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms and a halogenated silyl group and having 20 or less non-hydrogen atoms,
[0073] M 1represents a transition metal selected from the group of transition metals belonging to Group 4 of the Periodic Table of the Elements having a formal oxidation number of +2, +3 or +4 and having an η5 bond with at least one ligand L,
[0074] W represents a divalent substituent having 50 or less non-hydrogen atoms and bonding to each of L and M with a univalent valency to form a metal ring compound together with L and M,
[0075] X 1 each independently represents an anionic sigma-bonded ligand having 60 or less non-hydrogen atoms selected from the group consisting of a monovalent anionic sigma-bonded ligand, a divalent anionic sigma-bonded ligand divalently bonded to M, and a divalent anionic sigma-bonded ligand monovalently bonded to each of L and M,
[0076] X 2 each independently represents a neutral Lewis base coordinating compound having 40 or less non-hydrogen atoms,
[0077] j is 1 or 2, wherein when j is 2, the two ligands L are bonded to each other through a divalent group having 20 or less non-hydrogen atoms, the divalent group being a group selected from the group consisting of a hydrocarbon diyl having 1 to 20 carbon atoms, a halogenated hydrocarbon diyl having 1 to 12 carbon atoms, an alkyleneoxy group having 1 to 12 carbon atoms, an alkyleneamino group having 1 to 12 carbon atoms, a silane diyl group, a halogenated silane diyl group, and a silyleneamino group, k is 0 or 1, p is 0, 1 or 2, wherein in X 1 In the case of a monovalent anionic σ-bonding type ligand or a divalent anionic σ-bonding type ligand bonded to L and M, p is an integer smaller than the formal oxidation number of M by 1 or more, and in the case of X 1 In the case of a divalent anionic σ-bonded ligand that bonds only to M, p is an integer that is smaller than the formal oxidation number of M by (j+1) or more, and q is 0, 1, or 2.
[0078]
[0079] (In Formula 4, M 2 represents a transition metal selected from the group consisting of titanium, zirconium and hafnium and having a formal oxidation number of +2, +3 or +4,
[0080] R 5 Each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein in the substituent R 5 When it is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group or a germyl group, two adjacent substituents R 5bonded to each other to form a divalent group, thereby bonding to the two adjacent substituents R 5 The bonds between the two carbon atoms of the cyclopentadienyl ring to which each is bonded together form a ring,
[0081] X 3 Each independently represents a substituent selected from the group consisting of a halogen ion, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbonoxy group having 1 to 18 carbon atoms, a hydrocarbonamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbonamide group having 1 to 18 carbon atoms, a hydrocarbonphosphine group having 1 to 18 carbon atoms, a hydrocarbonthio group having 1 to 18 carbon atoms, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein two substituents X may be selected from the group consisting of 3 Together they form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms,
[0082] Y 1 Indicates -O-, -S-, -NR 6 -or-PR 6 -, where R 6 represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbonoxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof,
[0083] Z 1 SiR 6 2 , CR 6 2 、SiR 6 2 S i 6 2 , CR 6 2 CR 6 2 , CR 6 =CR 6 , CR 6 2 S i 6 2
[0084] or GeR 6 2 , where R 6 As defined above,
[0085] n is 1, 2, or 3. )
[0086] (C-1): [L 2 -H] d+ [M 3 r Q s ] d-……(Formula 5)
[0087] (In Formula 5, [L 2 -H] d+ For proton-donating Bronsted acids, L 2 is a neutral Lewis base. In addition, in Formula 5, [M 3 r Q s ] d- is a compatible non-coordinating anion, M 3 is a metal or metalloid selected from Groups 5 to 15 of the periodic table, Q is independently a hydride ion, a dialkylamino group, a halide ion, an alkoxy group, an allyloxy group, a hydrocarbon group, or a substituted hydrocarbon group having 20 or less carbon atoms, and the number of Q as a halide ion is 1 or less. In addition, r is an integer of 1 to 7, s is an integer of 2 to 14, d is an integer of 1 to 7, and sr=d.)
[0088] (C-2): -(M 4 R 7 t-2 -O) u -……(Formula 6)
[0089] (In Formula 6, M 4 is a metal or metalloid of Group 13 to Group 15 of the Periodic Table, R 7 are each independently a hydrocarbon group having 1 to 12 carbon atoms or a substituted hydrocarbon group having 1 to 12 carbon atoms, and t is a metal M 4 valence, u is an integer greater than 2. )
[0090]
[15] The olefin polymerization catalyst according to
[14] , wherein the inorganic solid particles [A] are magnesium chloride particles.
[0091]
[16] A method for producing an olefin polymer, comprising the step of polymerizing olefin using the olefin polymerization catalyst according to
[14] or
[15] .
[0092] Effects of the Invention
[0093] According to the polyethylene powder of the present invention, it is possible to provide a microporous film having excellent heat resistance, film uniformity, dimensional stability, and high heat resistance rate, for example. DETAILED DESCRIPTION
[0094] Hereinafter, a mode for implementing the present invention (hereinafter also referred to as "this embodiment") will be described in detail. It should be noted that the present invention is not limited to this embodiment, and can be implemented with appropriate modifications within the scope of the gist thereof.
[0095] [Polyethylene powder]
[0096] The viscosity average molecular weight of the polyethylene powder of this embodiment is 100,000 or more and 4,000,000 or less.
[0097] The crystal thickness parameter of the polyethylene powder measured using a differential scanning calorimeter (DSC) is 5° C. or more and 9° C. or less.
[0098] The polyethylene powder of the present embodiment has such characteristics and can provide a microporous film having excellent heat resistance, film uniformity, dimensional stability, and high heat resistance rate.
[0099] The z-average shrinkage factor g of the polyethylene powder of the present embodiment measured by a gel permeation chromatography (GPC) measuring apparatus in combination with a differential refractometer and a viscosity detector is z The value (hereinafter also recorded as "average shrinkage factor g z ”) is preferably greater than or equal to 0.600 and less than or equal to 1.
[0100] The polyethylene powder of the present embodiment has such characteristics and can provide a microporous film having more excellent heat resistance, film uniformity, dimensional stability, and high heat resistance rate.
[0101] It should be noted that the crystal thickness parameter is the peak temperature (Tm2 top ) and the temperature of the peak convergence point (Tm2 end ) difference (Tm2 end -Tm2 top ) (hereinafter also referred to as "temperature difference in DSC curve (Tm2 end -Tm2 top )”).
[0102] <Measurement conditions>
[0103] (1) Stand at 50°C for 1 minute
[0104] (2) Heating from 50°C to 180°C at 10°C / min (first heating process)
[0105] (3) Stand at 180°C for 5 minutes
[0106] (4) Cooling from 180°C to 50°C at 10°C / min
[0107] (5) Stand at 50°C for 5 minutes
[0108] (6) Heating from 50°C to 180°C at 10°C / min (second heating process)
[0109] In addition, the polyethylene powder of the present embodiment preferably has a peak top temperature (Tm2 top ) is 135°C or higher and 140°C or lower, and the crystal thickness parameter is 6.7°C or higher and 9.0°C or lower.
[0110] <Measurement conditions>
[0111] (1) Stand at 50°C for 1 minute
[0112] (2) Heating from 50°C to 180°C at 10°C / min (first heating process)
[0113] (3) Stand at 180°C for 5 minutes
[0114] (4) Cooling from 180°C to 50°C at 10°C / min
[0115] (5) Stand at 50°C for 5 minutes
[0116] (6) Heating from 50°C to 180°C at 10°C / min (second heating process)
[0117] The polyethylene powder of the present embodiment has such characteristics and can provide a microporous film having more excellent heat resistance, film uniformity, dimensional stability, and high heat resistance rate.
[0118] The mechanism by which the polyethylene powder of this embodiment exhibits the effects described above is not yet clear, but the inventors speculate as follows. The DSC curve of the second temperature increase process obtained by the measurement shown in the above <Measurement Conditions> using a differential scanning calorimeter (DSC) shows the characteristics of crystals generated during the recrystallization process of the polyethylene powder. It is believed that the characteristics of such crystals specifically correspond to the characteristics of crystals generated during the cooling process after melt kneading of the polyethylene powder in the actual process of manufacturing the microporous membrane, and the characteristics of the crystals generated here have an impact on the physical properties of the microporous membrane. In addition, it is believed that the temperature difference (Tm2 end -Tm2 top ) indicates a polyethylene component containing a high melting point within the above range, that is, there is a thick crystalline portion. As a process in which the crystalline portion grows thick, it is speculated that during the cooling process, a low mobility region constrained at a single end like a long chain branch first begins to crystallize, and then further crystallizes with the low mobility region as a core, thereby locally increasing the thickness of the crystalline portion. Moreover, regarding the polyethylene powder of the present embodiment, it is speculated that the generation of such a crystalline portion during the recrystallization process is a reason for being able to provide a microporous film with excellent heat resistance, uniformity of the film, dimensional stability and high heat resistance rate.
[0119] (Viscosity average molecular weight)
[0120] The viscosity average molecular weight of the polyethylene powder of the present embodiment is preferably 200,000 or more and 4,000,000 or less, more preferably 250,000 or more and 3,000,000 or less, and further preferably 300,000 or more and 2,500,000 or less. When the viscosity average molecular weight of the polyethylene powder of the present embodiment is above the above lower limit, there is a tendency to have sufficient mechanical strength when a microporous film is made. In addition, when the viscosity average molecular weight of the polyethylene powder of the present embodiment is below the above upper limit, there is a tendency as follows: excellent molding processability, when a microporous film is made, the generation of uneven thickness and unmelted material (uniformity) is suppressed, and in addition, the stress remaining in the microporous film (low shrinkage) is suppressed, and in addition, it is easy to mix with other polyethylene resins, and segregation is not easy to occur in the microporous film when blended.
[0121] In addition, in this embodiment, the viscosity average molecular weight of the polyethylene powder can be measured by the method described in the examples mentioned later.
[0122] (The temperature difference in the DSC curve (Tm2 end -Tm2 top ))
[0123] The temperature difference (Tm2 end -Tm2 top ) is 5°C or higher and 9°C or lower, preferably 6°C or higher and 8.5°C or lower, and more preferably 6.7°C or higher and 8°C or lower. In addition, the peak top temperature (Tm2 top ) is 135° C. or higher and 140° C. or lower, the temperature difference (Tm2 end -Tm2 top ) is preferably 6.7°C to 9.0°C, more preferably 6.7°C to 8.5°C, and even more preferably 6.7°C to 8°C. When the temperature difference (Tm2 end -Tm2 top ) is above the above lower limit, the heat resistance is improved when the microporous membrane is made by using the high melting point component, and the heat resistance can be improved when the microporous membrane is made by blending with other polyethylene resins. In addition, when the temperature difference (Tm2 end -Tm2 top ) is below the above upper limit value, there is a tendency that when a microporous membrane is made for secondary battery separator, the pores of the microporous membrane are easily closed when the battery generates abnormal heat, and there is a tendency that the microporous membrane can be stretched uniformly during stretching.
[0124] As the temperature difference (Tm2 end -Tm2 top ) is not particularly limited, and examples thereof include: a method of producing a polymer in a manner including a trace amount of long chain branches using a catalyst obtained by a special production method described later. Specifically, examples include: a method of producing in a manner in which the main chain and the side chain are controlled separately and the ratio of the side chain is suppressed to a trace amount. There are no particular limitations on the method of controlling the main chain and the side chain separately, and examples thereof include: using a catalyst comprising two active substances ((A) for macromonomer introduction and (B) for macromonomer synthesis), changing the type of co-catalyst according to each active substance, pre-mixing the co-catalyst and the active substance, and loading them in two or more stages, thereby forming a multilayer structure on the carrier surface. There are no particular restrictions on the method for suppressing the proportion of side chains to a trace amount, and examples thereof include: controlling the ratio of the above-mentioned two active substances ((A) for macromonomer introduction / (B) for macromonomer synthesis) within the range of 1 to 1000, controlling the ratio of the co-catalyst (C) to the active substance (A) for macromonomer introduction ((C) / (A)) within the range of 0.5 to 1.5, and controlling the ratio of the co-catalyst (D) to the active substance (B) for macromonomer synthesis ((D) / (B)) within the range of 1 to 60.
[0125] It should be noted that, in this embodiment, the temperature difference (Tm2 end -Tm2 top ) can be measured by the method described in the examples described later.
[0126] (Average shrinkage factor g z )
[0127] The average shrinkage factor g of the polyethylene powder of this embodiment is z It is preferably 0.600 to 1, more preferably 0.65 to 0.985, and even more preferably 0.7 to 0.97. z When the average shrinkage factor g of the polyethylene powder of this embodiment is greater than or equal to the above lower limit, the stress remaining in the microporous film when the microporous film is made is suppressed (low shrinkage), and the occurrence of entanglement caused by the branch chain is suppressed to a certain extent, thereby promoting crystallization. zWhen it is below the above upper limit value, there is the following tendency: high melting point crystals are easily generated, and the strength when melted is also increased. Therefore, when a microporous membrane is made, the heat resistance is further improved. In addition, the stability during film making is further improved, thereby suppressing film unevenness. By blending with other polyethylene resins, the heat resistance and stretchability of the microporous membrane can be further improved.
[0128] As the average shrinkage factor g z There are no particular restrictions on the method of producing polyethylene powder within the above range, and examples thereof include: a method of producing a polymer in a manner including a trace amount of long chain branches using a catalyst obtained by a special production method described later. Specifically, there are: a production method in which the main chain and the side chain are controlled separately and the ratio of the side chain is suppressed to a trace amount. There are no particular restrictions on the method of controlling the main chain and the side chain separately, and examples thereof include: using a catalyst comprising two active substances ((A) for macromonomer introduction and (B) for macromonomer synthesis), changing the type of co-catalyst according to each active substance, pre-mixing the co-catalyst and the active substance, and loading in two or more stages, thereby forming a multilayer structure on the carrier surface. There are no particular restrictions on the method for suppressing the proportion of side chains to a trace amount, and examples thereof include: controlling the ratio of the above-mentioned two active substances ((A) for macromonomer introduction / (B) for macromonomer synthesis) within the range of 1 to 1000, controlling the ratio of the co-catalyst (C) to the active substance (A) for macromonomer introduction ((C) / (A)) within the range of 0.5 to 1.5, and controlling the ratio of the co-catalyst (D) to the active substance (B) for macromonomer synthesis ((D) / (B)) within the range of 1 to 60.
[0129] It should be noted that, in this embodiment, the average shrinkage factor g of the polyethylene powder is z It can be measured by the method described in Examples below.
[0130] (Evaluation of stretchability)
[0131] The polyethylene powder of the present embodiment is preferably capable of being stretched under the following conditions.
[0132] (Stretching conditions)
[0133] A gel sheet of 100 mm×100 mm×1 mm in thickness containing 30% by mass of polyethylene powder and 70% by mass of liquid paraffin was stretched to 7×7 times at 115°C.
[0134] When the polyethylene powder of the present embodiment can be stretched under the above conditions, the unevenness of the film thickness when the microporous film is formed tends to be suppressed, and the microporous film tends to be able to be produced with high productivity.
[0135] There are no particular restrictions on the method for obtaining polyethylene powder that can be stretched under the above conditions. For example, the method includes: appropriately adjusting the catalyst composition and polymerization conditions to obtain an ultra-high molecular weight component (molecular weight> 10 7 It should be noted that, in the present embodiment, the stretchability under the above conditions can be specifically evaluated by the method described in the examples described later.
[0136] (400cm -1 ~450cm -1 Absorption coefficient in the range of
[0137] The polyethylene powder of this embodiment has a terahertz measurement at 400 cm -1 ~450cm -1 The absorption coefficient in the range of is preferably 1.0 to 4.0, more preferably 1.9 to 3.5, and further preferably 2.1 to 3.5.
[0138] Above 400cm -1 ~450cm -1 The attribution of the absorption peak of terahertz waves in the range of 500cm is still unclear, but terahertz waves are absorbed as vibration energy of polymer chains. -1 ~550cm -1 The absorption peak of the terahertz wave in the range of 400 cm corresponds to the vibration of the amorphous part of polyethylene. -1 ~450cm -1 The absorption peak in the range of corresponds to the vibration derived from the long-chain branched structure present in the amorphous part.
[0139] When the polyethylene powder of this embodiment is measured at 400 cm -1 ~450cm -1 When the absorption coefficient is within the above range, there is a tendency to suppress the stress remaining in the microporous membrane (low shrinkage). In addition, there is a tendency to suppress the unevenness of the film thickness when the microporous membrane is made.
[0140] As obtained in terahertz measurement, 400 cm -1 ~450cm -1 The method of obtaining polyethylene powder with an absorption coefficient within the above range is not particularly limited, and examples thereof include: a method of uniformly introducing the macromolecular monomer by appropriately adjusting the types of active substances and co-catalysts and their combination. It should be noted that in this embodiment, 400 cm -1 ~450cm -1 The absorption coefficient within the range of can be evaluated by the method described in the examples described later.
[0141] ( 1 H-NMR measurement)
[0142] The polyethylene powder of this embodiment is preferably 1 In the H-NMR measurement, there was no peak in the region shown below.
[0143] (1) 4.8ppm~5.0ppm
[0144] (2) 5.6ppm~6.0ppm
[0145] Both (1) and (2) are regions where signals corresponding to terminal double bonds are detected. The absence of a peak in this region indicates that no macromonomer remains in the polyethylene powder.
[0146] For the polyethylene powder of this embodiment, when 1 When there is no peak in the region shown above in the H-NMR measurement, there is a tendency that when a microporous membrane is made, it can be stretched uniformly, thereby suppressing uneven film thickness. In addition, there is a tendency that the stress remaining in the microporous membrane (low shrinkage rate) is further suppressed. In addition, when blended with other polyethylene resins, a uniform microporous membrane can be obtained.
[0147] As obtained in 1 The method of obtaining a polyethylene powder having no peak in the region shown above in H-NMR measurement is not particularly limited, and examples thereof include: a method of loading an active substance capable of introducing a macromolecular monomer on the outermost surface of the catalyst, or appropriately adjusting the catalyst raw material composition and the amount of the comonomer so that no terminal double bond remains. It should be noted that in this embodiment, the polyethylene powder 1 The H-NMR peak can be measured by the method described in Examples below.
[0148] (Aluminum content)
[0149] The aluminum content in the polyethylene powder of the present embodiment is preferably 0 ppm or more and 50 ppm or less, more preferably 0 ppm or more and 30 ppm or less, and further preferably 0 ppm or more and 15 ppm or less. When the aluminum content in the polyethylene powder of the present embodiment is within the above range, it tends to easily generate high melting point crystals, and also tends to become a high-quality microporous membrane when it is made into a microporous membrane. In addition, it can suppress the clogging of the filter during the molding process, thereby improving productivity.
[0150] In addition, in this embodiment, the aluminum content in the polyethylene powder can be measured by the method described in the examples described later.
[0151] (Silicon content)
[0152] The silicon content in the polyethylene powder of the present embodiment is preferably 0 ppm or more and 30 ppm or less, more preferably 0 ppm or more and 10 ppm or less, and further preferably 0 ppm or more and 2 ppm or less. When the silicon content in the polyethylene powder of the present embodiment is within the above range, it tends to easily generate high melting point crystals, and also tends to become a high-quality microporous membrane when it is made into a microporous membrane. In addition, it can suppress the clogging of the filter during the molding process, thereby improving productivity.
[0153] In addition, in this embodiment, the silicon content in the polyethylene powder can be measured by the method described in the examples mentioned later.
[0154] (Temperature of the peak in the DSC curve of the second heating process)
[0155] In the differential scanning calorimeter (DSC) measurement of the polyethylene powder of the present embodiment, the temperature of the peak top in the DSC curve in the second heating process (hereinafter also referred to as “Tm2 top ”) is preferably 130°C to 140°C, more preferably 133°C to 140°C, and even more preferably 135°C to 140°C. In addition, particularly when the crystal thickness parameter is 6.7°C to 9.0°C, the Tm2 of the polyethylene powder of this embodiment is top It is preferably 135°C to 140°C, more preferably 136°C to 140°C, and even more preferably 137°C to 140°C. top When the content is within the above range, the heat resistance of the microporous membrane can be improved, and the temperature can be applied in the heat setting step, so that the residual stress of the microporous membrane can be suppressed and the air permeability of the microporous membrane can be improved.
[0156] As Tm2 top The method for producing polyethylene powder within the above range is not particularly limited, and examples thereof include a method of adjusting the catalyst raw material composition and the amount of comonomer.
[0157] It should be noted that, in this embodiment, Tm2 top It can be measured by the method described in Examples below.
[0158] (density)
[0159] The density of the polyethylene powder of this embodiment is preferably 920 kg / m 3 Above and 960kg / m 3 Below, more preferably 930kg / m 3Above and 955kg / m 3 Below, more preferably 935kg / m 3 Above and 950kg / m 3 When the density of the polyethylene powder of the present embodiment is within the above range, the polyethylene powder tends to have excellent air permeability and heat resistance when formed into a microporous film.
[0160] In addition, in this embodiment, the density of the polyethylene powder can be measured by the method described in the examples mentioned later.
[0161] (Method for producing olefin polymerization catalyst)
[0162] The method for producing an olefin polymerization catalyst according to the present embodiment includes the following steps:
[0163] A first supporting reaction step, wherein the inorganic solid particles [A] are reacted with the transition metal compound [B-1] and / or the transition metal compound component [B-2], the activator [C] and / or the organometallic compound component [D]; and
[0164] A second supporting reaction step, wherein the particles obtained in the first supporting reaction step are reacted with a transition metal compound component [B-1] and / or a transition metal compound component [B-2], an activator [C] and / or an organometallic compound component [D],
[0165] The transition metal compound [B-1] is a compound represented by the following (Formula 3), the transition metal compound [B-2] is a compound represented by the following (Formula 4), the activator [C] is a compound represented by the following (Formula 5) or (Formula 6), the organometallic compound component [D] is a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, the inorganic solid particles [A] are porous polymer materials or inorganic solid particles containing at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table,
[0166] The method for producing an olefin polymerization catalyst satisfies the following <Condition 1> and / or <Condition 2>.
[0167] <Condition 1>
[0168] The first loading reaction step includes the following steps:
[0169] a premixing step of reacting the transition metal compound [B-1] and / or the transition metal compound component [B-2] with the activator [C] and / or the organometallic compound component [D]; and
[0170] A step of reacting the inorganic solid particles [A] with the mixture obtained in the pre-mixing step.
[0171] <Condition 2>
[0172] In the first loading reaction step, the molar ratio (([C]+[D]) / [B]) of the molar amount ([C]+[D]) of the activator [C] and the organometallic compound component [D] to the molar amount [B] of the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is greater than 1 and less than 60.
[0173] L 1 j W k M 1 X 1 p X 2 q ……(Formula 3)
[0174] (In Formula 3, L 1 each independently represents an n-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group and an octahydrofluorenyl group, wherein the ligand has 1 to 8 substituents as the case may be, and the substituents are each independently selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogenated hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms and a halogenated silyl group and having 20 or less non-hydrogen atoms,
[0175] M 1 represents a transition metal selected from the group of transition metals belonging to Group 4 of the Periodic Table of the Elements having a formal oxidation number of +2, +3 or +4 and having an η5 bond with at least one ligand L,
[0176] W represents a divalent substituent having 50 or less non-hydrogen atoms and bonding to each of L and M with a univalent valency to form a metal ring compound together with L and M,
[0177] X 1 each independently represents an anionic sigma-bonded ligand having 60 or less non-hydrogen atoms selected from the group consisting of a monovalent anionic sigma-bonded ligand, a divalent anionic sigma-bonded ligand divalently bonded to M, and a divalent anionic sigma-bonded ligand monovalently bonded to each of L and M,
[0178] X 2each independently represents a neutral Lewis base coordinating compound having 40 or less non-hydrogen atoms,
[0179] j is 1 or 2, wherein when j is 2, the two ligands L are bonded to each other through a divalent group having 20 or less non-hydrogen atoms, the divalent group being a group selected from the group consisting of a hydrocarbon diyl group having 1 to 20 carbon atoms, a halogenated hydrocarbon diyl group having 1 to 12 carbon atoms, an alkyleneoxy group having 1 to 12 carbon atoms, an alkyleneamino group having 1 to 12 carbon atoms, a silanediyl group, a halogenated silanediyl group, and a silyleneamino group, k is 0 or 1, p is 0, 1 or 2, wherein in X 1 In the case of a monovalent anionic σ-bonding type ligand or a divalent anionic σ-bonding type ligand bonded to L and M, p is an integer smaller than the formal oxidation number of M by 1 or more, and in the case of X 1 In the case of a divalent anionic σ-bonded ligand that bonds only to M, p is an integer that is smaller than the formal oxidation number of M by (j+1) or more, and q is 0, 1, or 2.
[0180]
[0181] (In Formula 4, M 2 represents a transition metal selected from the group consisting of titanium, zirconium and hafnium and having a formal oxidation number of +2, +3 or +4,
[0182] R 5 Each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein in the substituent R 5 When it is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group or a germyl group, two adjacent substituents R 5 bonded to each other to form a divalent group, thereby bonding to the two adjacent substituents R 5 The bonds between the two carbon atoms of the cyclopentadienyl ring to which each is bonded together form a ring,
[0183] X 3 Each independently represents a substituent selected from the group consisting of a halogen ion, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbonoxy group having 1 to 18 carbon atoms, a hydrocarbonamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbonamide group having 1 to 18 carbon atoms, a hydrocarbonphosphine group having 1 to 18 carbon atoms, a hydrocarbonthio group having 1 to 18 carbon atoms, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein two substituents X may be selected from the group consisting of 3 Together they form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms,
[0184] Y 1Indicates -O-, -S-, -NR 6 -or-PR 6 -, where R 6 represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbonoxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof,
[0185] Z 1 SiR 6 2 , CR 6 2 、SiR 6 2 S i 6 2 , CR 6 2 CR 6 2 , CR 6 =CR 6 , CR 6 2 S i 6 2
[0186] or GeR 6 2 , where R 6 As defined above,
[0187] n is 1, 2, or 3. )
[0188] (C-1): [L 2 -H] d+ [M 3 r Q s ] d- ……(Formula 5)
[0189] (In Formula 5, [L 2 -H] d+ For proton-donating Bronsted acids, L 2 is a neutral Lewis base. In addition, in Formula 5, [M 3 r Q s ] d- is a compatible non-coordinating anion, M 3 is a metal or metalloid selected from Groups 5 to 15 of the periodic table, Q is independently a hydride ion, a dialkylamino group, a halide ion, an alkoxy group, an allyloxy group, a hydrocarbon group, or a substituted hydrocarbon group having 20 or less carbon atoms, and the number of Q as a halide ion is 1 or less. In addition, r is an integer of 1 to 7, s is an integer of 2 to 14, d is an integer of 1 to 7, and sr=d.)
[0190] (C-2): -(M 4 R 7 t-2 -O) u -……(Formula 6)
[0191] (In Formula 6, M 4 is a metal or metalloid of Group 13 to Group 15 of the Periodic Table, R 7 are each independently a hydrocarbon group having 1 to 12 carbon atoms or a substituted hydrocarbon group having 1 to 12 carbon atoms, and t is a metal M 4 valence, u is an integer greater than 2. )
[0192] The transition metal compound used in the first supporting reaction step is preferably [B-1], and the transition metal compound used in the second supporting reaction step is preferably [B-2]. In addition, the molar ratio (([C]+[D]) / [B]) of the molar amount ([C]+[D]) of the activator [C] and the organometallic compound component [D] in the second supporting reaction step to the molar amount [B] of the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is preferably 0.5 or more and 1.5 or less, and more preferably 0.9 or more and 1.1 or less. In addition, the transition metal compound component ([B-2]) used in the second supporting reaction step is preferably 0.5 or more and 1.5 or less, and more preferably 0.9 or more and 1.1 or less. 2 ]) relative to the transition metal compound component used in the first supporting reaction step ([B 1 The molar ratio of ([B 2 ] / [B 1 ]) is preferably greater than 1 and less than 1000, more preferably greater than 5 and less than 100.
[0193] By including the first loading reaction step and the second loading reaction step, two layers containing a mixture of a transition metal compound and an activator can be formed on the surface of the inorganic solid particles [A]. With this double-layer structure, the macromonomer generated in the first layer is introduced into the transition metal compound in the second layer, so that the control of long chain branches in the production of olefin polymers becomes easy. In addition, by controlling the molar ratio (([C]+[D]) / [B]) and (([B 2 ] / [B 1 ])), the amount of long chain branches in the production of olefin polymers can be suppressed to a trace amount.
[0194] The method for producing an olefin polymerization catalyst according to the present embodiment satisfies the following <Condition 1> and / or <Condition 2>.
[0195] <Condition 1>
[0196] The first loading reaction step includes the following steps:
[0197] a premixing step of reacting the transition metal compound [B-1] and / or the transition metal compound component [B-2] with the activator [C] and / or the organometallic compound component [D]; and
[0198] A step of reacting the inorganic solid particles [A] with the mixture obtained in the pre-mixing step.
[0199] By satisfying <Condition 1>, a layer in which the transition metal compound and the activator are uniformly mixed tends to be formed on the surface of the inorganic solid particles [A]. By forming a uniform mixed layer, the introduction of the macromonomer becomes uniform, and an olefin polymer with less segregation of long-chain branches can be synthesized.
[0200] <Condition 2>
[0201] In the first loading reaction step, the molar ratio (([C]+[D]) / [B]) of the molar amount ([C]+[D]) of the activator [C] and the organometallic compound component [D] to the molar amount [B] of the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is greater than 1 and less than 60, preferably greater than 1 and less than 30.
[0202] By satisfying <Condition 2>, there is a tendency that the amount of macromonomer produced can be suppressed, and therefore the amount of long chain branches can be suppressed to a trace amount in the production of olefin polymers.
[0203] The method for producing an olefin polymerization catalyst according to the present embodiment can synthesize an olefin polymer containing a trace amount of long chain branches by satisfying the above-mentioned process conditions. In addition, in the production of the olefin polymer, the amount and length of the long chain branches can be easily controlled.
[0204] (Inorganic solid particles [A] used in the method for producing an olefin polymerization catalyst)
[0205] The method for producing an olefin polymerization catalyst according to the present embodiment preferably uses magnesium chloride particles as the inorganic solid particles [A].
[0206] When magnesium chloride particles are used as the inorganic solid particles [A] in the method for producing an olefin polymerization catalyst according to the present embodiment, the catalyst particles tend to break easily during polymerization, and an olefin polymer with less metal residue can be produced.
[0207] (Olefin polymerization catalyst)
[0208] The olefin polymerization catalyst of the present embodiment comprises inorganic solid particles [A], a transition metal compound component [B-1] and / or a transition metal compound component [B-2], and an activator [C] and / or an organic metal compound component [D].
[0209] The transition metal compound [B-1] is a compound represented by the above (Formula 3), the transition metal compound [B-2] is a compound represented by the above (Formula 4), the activator [C] is a compound represented by the above (Formula 5) or (Formula 6), the organometallic compound component [D] is a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, the inorganic solid particles [A] are porous polymer materials or inorganic solid particles containing at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table,
[0210] The content (molar) of the central metal M contained in the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is 20 micromoles or more and 1000 micromoles or less, and the molar ratio (Al / M) of the content (moles) of the central metal M to the content (moles) of Al is 1 or more and 30 or less. The content (moles) of the central metal M is preferably 20 micromoles or more and 250 micromoles or less, and the molar ratio (Al / M) is preferably 1 or more and 10 or less.
[0211] When the catalyst for olefin polymerization of the present embodiment contains the above-mentioned components and the content (molar) of the central metal M and the molar ratio (Al / M) of the content (molar) of the central metal M to the content (molar) of Al are within the above-mentioned ranges, it is easy to control the amount and length of the long chain branches of the olefin polymer obtained by polymerization, and the amount of the long chain branches of the olefin polymer can be suppressed to a trace amount.
[0212] In the present embodiment, the content (molar) of the central metal M in the catalyst component and the molar ratio (Al / M) of the content (molar) of the central metal M to the content (molar) of Al can be measured by the method described in the examples described later.
[0213] (Inorganic solid particles [A] contained in olefin polymerization catalyst)
[0214] The inorganic solid particles [A] in the olefin polymerization catalyst of the present embodiment are preferably magnesium chloride particles.
[0215] When the inorganic solid particles [A] in the olefin polymerization catalyst of the present embodiment are magnesium chloride particles, the catalyst particles are easily broken during polymerization, and an olefin polymer with less metal residue tends to be produced.
[0216] It should be noted that the inorganic solid particles [A], transition metal compound [B-1], transition metal compound component [B-2], activator [C] and organometallic compound component [D] in the olefin polymerization catalyst of the present embodiment can appropriately use the contents of the inorganic solid particles [A], transition metal compound [B-1], transition metal compound component [B-2], activator [C] and organometallic compound component [D] described in the [method for producing polyethylene powder] described later. In addition, the conditions in the method for producing the olefin polymerization catalyst of the present embodiment can appropriately use the contents of the conditions described in the [method for producing polyethylene powder] described later.
[0217] The method for producing an olefin polymer according to the present embodiment includes a step of polymerizing olefin using the above-mentioned olefin polymerization catalyst.
[0218] [Method for producing polyethylene powder]
[0219] Hereinafter, an example of the method for producing the polyethylene powder according to the present embodiment will be described.
[0220] (Catalyst component)
[0221] The polyethylene powder of the present embodiment can be produced, for example, by polymerizing ethylene or ethylene and other comonomers using a predetermined catalyst component.
[0222] There is no particular restriction on the catalyst components used in the manufacture of the ethylene polymer constituting the polyethylene powder of this embodiment, and for example, it is preferably composed of inorganic solid particles [A], a transition metal compound component [B-1], a transition metal compound component [B-2], and an activator [C] and / or an organic metal compound component [D].
[0223] In the present embodiment, there are no particular restrictions on the inorganic solid particles [A], and examples thereof include: porous polymer materials (wherein the matrix includes, for example, polyolefins or modified products thereof such as polyethylene, polypropylene, polystyrene, ethylene-propylene copolymers, ethylene-vinyl ester copolymers, styrene-divinylbenzene copolymers, and partially or completely saponified products of ethylene-vinyl ester copolymers; thermoplastic resins such as polyamides, polycarbonates, and polyesters; thermosetting resins such as phenolic resins, epoxy resins, urea-formaldehyde resins, and melamine resins; inorganic solid particles comprising at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table (e.g., silicon dioxide, aluminum oxide, magnesium oxide, magnesium chloride, zirconium oxide, titanium dioxide, boron oxide, calcium oxide, zinc oxide, barium oxide, vanadium pentoxide, chromium oxide, thorium oxide, or mixtures thereof or composite oxides thereof), etc.
[0224] The composite oxide containing silicon dioxide is not particularly limited, and examples thereof include composite oxides of silicon dioxide such as silicon dioxide-magnesium oxide and silicon dioxide-aluminum oxide and oxides of elements selected from elements belonging to Group 2 or Group 13 of the periodic table. In the present embodiment, the inorganic solid particles [A] are preferably selected from silicon dioxide, aluminum oxide, and composite oxides of silicon dioxide and oxides of elements selected from elements belonging to Group 2 or Group 13 of the periodic table.
[0225] There is no particular restriction on the shape of the silica product used as the inorganic solid particles [A], and the shape of the silica can be any shape such as granular, spherical, aggregated, smoky, etc. Preferred examples of commercially available silica products are not particularly limited, and examples thereof include: SD3216.30, SP-9-10046, Davison Syloid TM (Syloid TM) 245, Davison 948 or Davison 952 [all of which are manufactured by Grace Davison (a branch of WR Davison (USA))]; Aerosil 812 [manufactured by Degussa AG (Germany)]; ES70X [manufactured by CrossField (USA)]; P-6, P-10, Q-6 [manufactured by Fuji Silysia (Japan)], etc.
[0226] There is no particular restriction on the properties of magnesium chloride used as the inorganic solid particles [A]. In addition, as a preferred example of the production of magnesium chloride, there can be cited a method of reacting an organic magnesium compound (A-1) soluble in an inert hydrocarbon solvent represented by the following (Formula 1) and a chlorinating agent (A-2) represented by the following (Formula 2).
[0227] (A-1): (M 1 ) γ (Mg) δ (R 1 ) e (R 2 ) f (OR 3 ) g ……(Formula 1)
[0228] (In Formula 1, M 1 is a metal atom belonging to any one selected from the group consisting of Group 12, Group 13 and Group 14 of the Periodic Table, R 1 , R 2 and R 3 Each is a hydrocarbon group having 2 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers satisfying the following relationship.
[0229] 0≤γ, 0<δ, 0≤e, 0≤f, 0≤g, 0<e+f, 0≤g / (γ+δ)≤2, kγ+2δ=e+f+g (where k represents M 1 valence.
[0230] (A-2): H h SiCl i R 4 (4-(h+i)) ……(Formula 2)
[0231] (In Formula 2, R 4 is a hydrocarbon group having 1 or more and 12 or less carbon atoms, and h and i are real numbers satisfying the following relationship: 0<h, 0<i, 0<h+i≤4)
[0232] First, the organomagnesium compound (A-1) will be described.
[0233] The organomagnesium compound (A-1) is represented in the form of an organomagnesium complex soluble in an inert hydrocarbon solvent, including all of a dihydrocarbyl magnesium compound and a complex of the compound with other metal compounds.
[0234] The above relationship of the symbols γ, δ, e, f and g in the above (Formula 1) kγ+2δ=e+f+g represents the stoichiometry of the valence of the metal atom and the substituent.
[0235] In the above (Formula 1), R 1 , R 2 The hydrocarbon group represented is not particularly limited, and for example, each is independently an alkyl group, a cycloalkyl group or an aryl group. More specifically, there is no particular limitation, and examples thereof include methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, and phenyl.
[0236] Among them, R 1 and R 2 Preferably, each is an alkyl group.
[0237] In the case of γ>0, as the metal atom M 1 A metal atom belonging to any one of the groups consisting of Groups 12, 13 and 14 of the periodic table can be used, and more specifically, there is no particular limitation, and examples thereof include zinc, boron, aluminum, etc. Aluminum and zinc are particularly preferred.
[0238] Magnesium relative to metal atoms M 1 The ratio δ / γ is not particularly limited, but is preferably 0.1 or more and 30 or less, and more preferably 0.5 or more and 10 or less.
[0239] When a predetermined organomagnesium compound having γ=0 is used as (A-1), for example, in R 1In the case of 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also brings about a preferred result in the production of the polyethylene powder of the present embodiment.
[0240] In the above (Formula 1), the hydrocarbon group R in the case of γ = 0 1 , R 2 Any one of the following three groups (1), (2) and (3) is preferred.
[0241] Group (1):
[0242] R 1 , R 2 At least one of them is a secondary or tertiary alkyl group having 4 to 6 carbon atoms. 1 , R 2 All of them have 4 to 6 carbon atoms, and at least one of them is a secondary alkyl group or a tertiary alkyl group.
[0243] Group (2):
[0244] R 1 and R 2 are alkyl groups with different carbon number. 1 is an alkyl group having 2 or 3 carbon atoms, and R 2 It is an alkyl group having 4 or more carbon atoms.
[0245] Group (3):
[0246] R 1 , R 2 At least one of them is a hydrocarbon group having 6 or more carbon atoms. 1 , R 2 The total number of carbon atoms contained in the alkyl group is 12 or more.
[0247] The following specifically shows the hydrocarbon group R in the case where γ=0 in the above (Formula 1). 1 , R 2 .
[0248] In group (1), the secondary or tertiary alkyl group having 4 to 6 carbon atoms is not particularly limited, and examples thereof include 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl. 1-methylpropyl is particularly preferred.
[0249] In group (2), the alkyl group having 2 or 3 carbon atoms is not particularly limited, and examples thereof include ethyl group, 1-methylethyl group, propyl group, etc. Ethyl group is particularly preferred.
[0250] The alkyl group having 4 or more carbon atoms is not particularly limited, and examples thereof include butyl, pentyl, hexyl, heptyl, and octyl groups, among which butyl and hexyl groups are particularly preferred.
[0251] In group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, and examples thereof include hexyl, heptyl, octyl, nonyl, decyl, phenyl, 2-naphthyl, etc. Among the hydrocarbon groups, alkyl groups are preferred, and among the alkyl groups, hexyl and octyl groups are more preferred.
[0252] Generally, as the number of carbon atoms contained in the alkyl group increases, it tends to be easily dissolved in an inert hydrocarbon solvent and the viscosity of the solution tends to increase. 1 , R 2 It should be noted that the organomagnesium compound (A-1) is used in the form of an inert hydrocarbon solution, but even if a trace amount of Lewis basic compounds such as ethers, esters, and amines are contained or remain in the solution, it can be used without any influence.
[0253] Next, the alkoxy group (OR 3 ) for explanation.
[0254] As R 3 The hydrocarbon group represented by is preferably an alkyl group or aryl group having 1 to 12 carbon atoms, and more preferably an alkyl group or aryl group having 3 to 10 carbon atoms.
[0255] As R 3 , there are no particular limitations, for example, methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 1,1-dimethylethyl, pentyl, hexyl, 2-methylpentyl, 2-ethylbutyl, 2-ethylpentyl, 2-ethylhexyl, 2-ethyl-4-methylpentyl, 2-propylheptyl, 2-ethyl-5-methyloctyl, octyl, nonyl, decyl, phenyl, naphthyl, etc.
[0256] Particularly more preferred are butyl, 1-methylpropyl, 2-methylpentyl and 2-ethylhexyl.
[0257] The method for synthesizing the organomagnesium compound (A-1) is not particularly limited, and examples thereof include the following method: in an inert hydrocarbon solvent at a temperature of 25° C. to 150° C., a reaction mixture of a compound represented by the formula: 1 MgX 1 Japanese style: R 1 2 Mg(R 1 As mentioned above, X 1 Any one of the organomagnesium compounds in the group consisting of halogen atoms) and belonging to the formula: M 1R 2 k Japanese style: M 1 R 2 (k -1)H(M 1 , R 2 and k as described above), and then react with any one of the organometallic compounds in the group consisting of R 2 (R 2 As described above) or a hydrocarbon alcohol soluble in an inert hydrocarbon solvent having a 2 An organomagnesium compound (A-1) is synthesized by reacting an alkoxymagnesium compound and / or an alkoxyaluminum compound having a hydrocarbon group represented by:
[0258] In the above method, when an organomagnesium compound soluble in an inert hydrocarbon solvent is reacted with an alcohol, the order of the reactions is not particularly limited, and any method of adding alcohol to the organomagnesium compound, adding the organomagnesium compound to alcohol, or adding both simultaneously can be used.
[0259] There is no particular restriction on the reaction ratio of the organic magnesium compound soluble in an inert hydrocarbon solvent and the alcohol. As a result of the reaction, the molar composition ratio of the alkoxy groups in the obtained organic magnesium compound containing alkoxy groups relative to all metal atoms is: g / (γ+δ) is 0≤g / (γ+δ)≤2, preferably 0≤g / (γ+δ)<1.
[0260] Next, the chlorinating agent (A-2) will be described.
[0261] The chlorinating agent (A-2) is a chlorinated silicon compound having at least one Si—H bond represented by (Formula 2).
[0262] (A-2): H h SiCl i R 4 (4 -(h+i))……(Formula 2)
[0263] (In Formula 2, R 4 is a hydrocarbon group having 1 or more and 12 or less carbon atoms, and h and i are real numbers satisfying the following relationship: 0<h, 0<i, 0<h+i≤4)
[0264] In the above (Formula 2), as R 4 The hydrocarbon group represented by is not particularly limited, and examples thereof include aliphatic hydrocarbon groups, alicyclic hydrocarbon groups and aromatic hydrocarbon groups. Specifically, examples thereof include methyl, ethyl, propyl, 1-methylethyl, butyl, pentyl, hexyl, octyl, decyl, cyclohexyl, and phenyl.
[0265] Particularly preferred are alkyl groups having 1 to 10 carbon atoms, and more preferred are alkyl groups having 1 to 3 carbon atoms such as methyl, ethyl, propyl, and 1-methylethyl. In addition, h and i are numbers satisfying the relationship h+i≤4 and greater than 0, and i is preferably 2 to 3.
[0266] The chlorinating agent (A-2) is not particularly limited, and examples thereof include: HSiCl 3 , HSiCl 2 CH 3 , HSiCl 2 C 2 H 5 , HSiCl 2 (C 3 H 7 )、HSiCl 2 (2-C 3 H 7 )、HSiCl 2 (C 4 H 9 )、HSiCl 2 (C 6 H 5 )、HSiCl 2 (4-Cl-C 6 H 4 )、HSiCl 2 (CH=CH 2 )、HSiCl 2 (CH 2 C 6 H 5 )、HSiCl 2 (1-C 10 H 7 )、HSiCl 2 (CH 2 CH=CH 2 ), H 2 SiCl(CH 3 ), H 2 SiCl(C 2 H 5 )、HSiCl(CH 3 ) 2 、HSiCl(C 2 H 5 ) 2 、HSiCl(CH 3 )(2-C 3 H 7 )、HSiCl(CH 3 )(C 6 H 5 )、HSiCl(C 6 H5 ) 2 wait.
[0267] As the chlorinating agent (A-2), a chlorinated silicon compound containing these compounds or a mixture of two or more selected from these compounds is used.
[0268] HSiCl is particularly preferred 3 , HSiCl 2 CH 3 、HSiCl(CH 3 ) 2 , HSiCl 2 (C 3 H 7 ), more preferably HSiCl 3 , HSiCl 2 CH 3 .
[0269] Next, the reaction between the organomagnesium compound (A-1) and the chlorinating agent (A-2) is described.
[0270] During the reaction, the chlorinating agent (A-2) is preferably diluted in advance with an inert hydrocarbon solvent, a chlorinated hydrocarbon such as 1,2-dichloroethane, o-dichlorobenzene, dichloromethane, or an ether solvent such as diethyl ether or tetrahydrofuran, or a mixed solvent thereof. Among them, an inert hydrocarbon solvent is more preferably used from the perspective of catalyst performance.
[0271] The reaction ratio of the organomagnesium compound (A-1) and the chlorinating agent (A-2) is not particularly limited, but the number of moles of silicon atoms contained in the chlorinating agent (A-2) is preferably 0.01 mol or more and 100 mol or less, and more preferably 0.1 mol or more and 10 mol or less, relative to 1 mol of magnesium atoms contained in the organomagnesium compound (A-1).
[0272] The reaction method of the organomagnesium compound (A-1) and the chlorinating agent (A-2) is not particularly limited, and any of the following methods can be used: a method in which the organomagnesium compound (A-1) and the chlorinating agent (A-2) are simultaneously introduced into a reactor and reacted simultaneously; a method in which the chlorinating agent (A-2) is introduced into the reactor beforehand, and then the organomagnesium compound (A-1) is introduced into the reactor; or a method in which the organomagnesium compound (A-1) is introduced into the reactor beforehand, and then the chlorinating agent (A-2) is introduced into the reactor. In particular, a method in which the chlorinating agent (A-2) is introduced into the reactor beforehand, and then the organomagnesium compound (A-1) is introduced into the reactor is preferred.
[0273] The reaction temperature of the organomagnesium compound (A-1) and the chlorinating agent (A-2) is not particularly limited, but is preferably 25°C to 150°C, more preferably 30°C to 120°C, and further preferably 40°C to 100°C.
[0274] In the simultaneous addition method of simultaneously introducing the organomagnesium compound (A-1) and the chlorinating agent (A-2) into a reactor and reacting them, it is preferred to adjust the temperature of the reactor to a predetermined temperature in advance and adjust the temperature in the reactor to the predetermined temperature simultaneously with the simultaneous addition.
[0275] In the method of introducing the organomagnesium compound (A-1) into the reactor after previously charging the chlorinating agent (A-2) into the reactor, it is preferred that the temperature of the reactor into which the chlorinating agent (A-2) is charged is adjusted to a predetermined temperature, and the temperature in the reactor is adjusted to a predetermined temperature simultaneously with the introduction of the organomagnesium compound (A-1) into the reactor.
[0276] In the method of placing the organomagnesium compound (A-1) in a reactor in advance and then introducing the chlorinating agent (A-2) into the reactor, it is preferred that the temperature of the reactor into which the organomagnesium compound (A-1) has been placed is adjusted to a predetermined temperature, and the temperature in the reactor is adjusted to a predetermined temperature simultaneously with the introduction of the chlorinating agent (A-2) into the reactor.
[0277] The magnesium chloride obtained by the above reaction is preferably separated by filtration or decantation, and then sufficiently washed with an inert hydrocarbon solvent to remove unreacted products, by-products, and the like.
[0278] Next, the transition metal compound component [B-1] used in the present embodiment will be described.
[0279] Examples of the transition metal compound component [B-1] used in the present embodiment are not particularly limited, and examples thereof include compounds represented by the following (Formula 3).
[0280] L 1 j W k M 1 X 1 p X 2 q ……(Formula 3)
[0281] (In Formula 3, L 1each independently represents an n-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group and an octahydrofluorenyl group, wherein the ligand has 1 to 8 substituents as the case may be, and the substituents are each independently selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogenated hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms and a halogenated silyl group and having 20 or less non-hydrogen atoms,
[0282] M 1 represents a transition metal selected from the group of transition metals belonging to Group 4 of the Periodic Table of the Elements having a formal oxidation number of +2, +3 or +4 and having an η5 bond with at least one ligand L,
[0283] W represents a divalent substituent having 50 or less non-hydrogen atoms and bonding to each of L and M with a univalent valency to form a metal ring compound together with L and M,
[0284] X 1 each independently represents an anionic sigma-bonded ligand having 60 or less non-hydrogen atoms selected from the group consisting of a monovalent anionic sigma-bonded ligand, a divalent anionic sigma-bonded ligand divalently bonded to M, and a divalent anionic sigma-bonded ligand monovalently bonded to each of L and M,
[0285] X 2 each independently represents a neutral Lewis base coordinating compound having 40 or less non-hydrogen atoms,
[0286] j is 1 or 2, wherein when j is 2, the two ligands L are bonded to each other through a divalent group having 20 or less non-hydrogen atoms, the divalent group being a group selected from the group consisting of a hydrocarbon diyl group having 1 to 20 carbon atoms, a halogenated hydrocarbon diyl group having 1 to 12 carbon atoms, an alkyleneoxy group having 1 to 12 carbon atoms, an alkyleneamino group having 1 to 12 carbon atoms, a silanediyl group, a halogenated silanediyl group, and a silyleneamino group, k is 0 or 1, p is 0, 1 or 2, wherein in X 1 In the case of a monovalent anionic σ-bonding type ligand or a divalent anionic σ-bonding type ligand bonded to L and M, p is an integer smaller than the formal oxidation number of M by 1 or more, and in the case of X 1 In the case of a divalent anionic σ-bonding type ligand that bonds only to M, p is an integer that is smaller than the formal oxidation number of M by (j+1) or more, and q is 0, 1 or 2).
[0287] As the ligand X in the compound (Formula 3)1 Examples of the group include, but are not particularly limited to, hydride ions, halogen ions, hydrocarbon groups having 1 to 60 carbon atoms, hydrocarbonoxy groups having 1 to 60 carbon atoms, hydrocarbonamino groups having 1 to 60 carbon atoms, hydrocarbonphosphino groups having 1 to 60 carbon atoms, hydrocarbonthio groups having 1 to 60 carbon atoms, silyl groups, and composite groups thereof.
[0288] As the neutral Lewis base coordination compound X in the compound (Formula 3) 2 Examples of the moiety include, but are not particularly limited to, phosphines, ethers, amines, olefins having 2 to 40 carbon atoms, dienes having 3 to 40 carbon atoms, and divalent groups derived from these compounds.
[0289] The structure of the transition metal compound component [B-1] used in the present embodiment is not particularly limited, but from the viewpoint of reducing the mobility of polyethylene branches, it is preferred to use a compound that can polymerize to give ultrahigh molecular weight polyethylene.
[0290] Specific examples of the transition metal compound component [B-1] used in the present embodiment are not particularly limited, and examples thereof include the following compounds.
[0291] Bis(methylcyclopentadienyl)zirconium dimethyl,
[0292] Bis(n-butylcyclopentadienyl)zirconium dimethyl,
[0293] Bis(indenyl)zirconium dimethyl,
[0294] Bis(1,3-dimethylcyclopentadienyl)zirconium dimethyl,
[0295] (pentamethylcyclopentadienyl)(cyclopentadienyl)zirconium dimethyl,
[0296] Bis(cyclopentadienyl)zirconium dimethyl,
[0297] Bis(pentamethylcyclopentadienyl)zirconium dimethyl,
[0298] Bis(fluorenyl)zirconium dimethyl,
[0299] Bis(methylcyclopentadienyl)dimethyltitanium,
[0300] Bis(n-butylcyclopentadienyl)dimethyltitanium,
[0301] Bis(indenyl)dimethyltitanium,
[0302] Bis(1,3-dimethylcyclopentadienyl)dimethyltitanium,
[0303] (pentamethylcyclopentadienyl)(cyclopentadienyl)dimethyltitanium,
[0304] Bis(cyclopentadienyl)dimethyltitanium,
[0305] Bis(pentamethylcyclopentadienyl)dimethyltitanium,
[0306] Bis(fluorenyl)dimethyltitanium,
[0307] Ethylenebis(indenyl)zirconium dimethyl,
[0308] Ethylenebis(4,5,6,7-tetrahydro-1-indenyl)zirconium dimethyl,
[0309] Ethylenebis(4-methyl-1-indenyl)zirconium dimethyl,
[0310] Ethylenebis(5-methyl-1-indenyl)zirconium dimethyl,
[0311] Ethylenebis(6-methyl-1-indenyl)zirconium dimethyl,
[0312] Ethylenebis(7-methyl-1-indenyl)zirconium dimethyl,
[0313] Ethylenebis(5-methoxy-1-indenyl)zirconium dimethyl,
[0314] Ethylenebis(2,3-dimethyl-1-indenyl)zirconium dimethyl,
[0315] Ethylenebis(4,7-dimethyl-1-indenyl)zirconium dimethyl,
[0316] Ethylenebis(4,7-dimethoxy-1-indenyl)zirconium dimethyl,
[0317] Methylenebis(cyclopentadienyl)zirconium dimethyl,
[0318] Isopropylidene bis(cyclopentadienyl)zirconium dimethyl,
[0319] Isopropylidene (cyclopentadienyl-fluorenyl) zirconium dimethyl,
[0320] Silylenebis(cyclopentadienyl)zirconium dimethyl,
[0321] Dimethylsilylene bis(cyclopentadienyl)zirconium dimethyl,
[0322] [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)-1,2-ethanediyl]dimethyltitanium,
[0323] [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0324] [(N-methylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0325] [(N-phenylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0326] [(N-benzylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0327] [(N-tert-butylamino)(η5-cyclopentadienyl)-1,2-ethanediyl]dimethyltitanium,
[0328] [(N-tert-butylamino)(η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0329] [(N-methylamino)(η5-cyclopentadienyl)-1,2-ethanediyl]dimethyltitanium,
[0330] [(N-methylamino)(η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0331] [(N-tert-butylamino)(η5-indenyl)dimethylsilane]dimethyltitanium,
[0332] [(N-benzylamino)(η5-indenyl)dimethylsilane]dimethyltitanium,
[0333] Nickel dibromide bis(triphenylphosphine),
[0334] Dichlorobis(triphenylphosphine)nickel,
[0335] Nickel dibromide and diacetonitrile,
[0336] Nickel dibromodibenzonitrile,
[0337] Nickel dibromide (1,2-bis(diphenylphosphino)ethane),
[0338] Nickel dibromide (1,3-bis(diphenylphosphino)propane),
[0339] Nickel dibromide (1,1'-bis(diphenylphosphino)ferrocene),
[0340] Dimethylbis(diphenylphosphine)nickel,
[0341] Dimethyl(1,2-bis(diphenylphosphino)ethane)nickel,
[0342] Methyl(1,2-bis(diphenylphosphino)ethane)nickel tetrafluoroborate,
[0343] (2-diphenylphosphino-1-phenylethyleneoxy)phenylpyridine nickel,
[0344] Dichlorobis(triphenylphosphine)palladium,
[0345] Palladium dichlorodibenzonitrile, Palladium dichlorodiacetonitrile,
[0346] Dichloro(1,2-bis(diphenylphosphino)ethane)palladium,
[0347] Bis(triphenylphosphine)palladium bistetrafluoroborate,
[0348] Bis(2,2'-bipyridyl)methyliron tetrafluoroborate ether complex, etc.
[0349] Specific examples of the transition metal compound component [B-1] used in the present embodiment are not particularly limited, and examples thereof include: a compound having a "dimethyl" portion (which is the portion in the middle of the name of each compound, i.e., the portion immediately preceding the portion called "zirconium" or "titanium") in the name of each zirconium compound and titanium compound listed above, which is the same as X in the above (Formula 3) 1 , X 2 The compound is a compound having a name obtained by replacing the name corresponding to the part of (a) with any group listed below.
[0350] "Dichloro"
[0351] "Dibromo"
[0352] "Diiodine"
[0353] "Diethyl",
[0354] "Dibutyl"
[0355] "Diphenyl"
[0356] "Dibenzyl"
[0357] "2-(N,N-dimethylamino)benzyl",
[0358] "2-Butene-1,4-diyl",
[0359] "s-trans-η4-1,4-diphenyl-1,3-butadiene",
[0360] "s-trans-η4-3-methyl-1,3-pentadiene",
[0361] "s-trans-η4-1,4-dibenzyl-1,3-butadiene",
[0362] "s-trans-η4-2,4-hexadiene",
[0363] "s-trans-η4-1,3-pentadiene",
[0364] "s-trans-η4-1,4-dimethylbenzene-1,3-butadiene",
[0365] "s-trans-η4-1,4-bis(trimethylsilyl)-1,3-butadiene",
[0366] "s-cis-η4-1,4-diphenyl-1,3-butadiene",
[0367] "s-cis-η4-3-methyl-1,3-pentadiene",
[0368] "s-cis-η4-1,4-dibenzyl-1,3-butadiene",
[0369] "s-cis-η4-2,4-hexadiene",
[0370] "s-cis-η4-1,3-pentadiene",
[0371] "s-cis-η4-1,4-dimethylbenzene-1,3-butadiene",
[0372] "s-cis-η4-1,4-bis(trimethylsilyl)-1,3-butadiene" and the like.
[0373] As a specific example of such a transition metal compound component [B-1], bis(pentamethylcyclopentadienyl)titanium dichloride is preferred.
[0374] The transition metal compound component [B-1] used in the present embodiment is not particularly limited and can be generally synthesized by a known method.
[0375] Next, the transition metal compound component [B-2] used in the present embodiment will be described.
[0376] The transition metal compound component [B-2] is not particularly limited, but is preferably a compound represented by the following (Formula 4) from the viewpoint of the efficiency of introduction of the macromonomer.
[0377]
[0378] (In Formula 4, M 2 represents a transition metal selected from the group consisting of titanium, zirconium and hafnium and having a formal oxidation number of +2, +3 or +4,
[0379] R 5 Each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein in the substituent R 5 When it is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group or a germyl group, two adjacent substituents R 5 bonded to each other to form a divalent group, thereby bonding to the two adjacent substituents R 5The bonds between the two carbon atoms of the cyclopentadienyl ring to which each is bonded together form a ring,
[0380] X 3 Each independently represents a substituent selected from the group consisting of a halogen ion, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbonoxy group having 1 to 18 carbon atoms, a hydrocarbonamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbonamide group having 1 to 18 carbon atoms, a hydrocarbonphosphine group having 1 to 18 carbon atoms, a hydrocarbonthio group having 1 to 18 carbon atoms, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein two substituents X may be selected from the group consisting of 3 Together they form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms,
[0381] Y 1 Indicates -O-, -S-, -NR 6 -or-PR 6 -, where R 6 represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbonoxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof,
[0382] Z 1 SiR 6 2 , CR 6 2 、SiR 6 2 S i 6 2 , CR 6 2 CR 6 2 , CR 6 =CR 6 , CR 6 2 S i 6 2
[0383] or GeR 6 2 , where R 6 As defined above,
[0384] n is 1, 2, or 3. )
[0385] Specific examples of the transition metal compound component [B-2] used in the present embodiment are not particularly limited, and examples thereof include the following compounds.
[0386] [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)-1,2-ethanediyl]dimethyltitanium,
[0387] [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0388] [(N-methylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0389] [(N-phenylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0390] [(N-benzylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0391] [(N-tert-butylamino)(η5-cyclopentadienyl)-1,2-ethanediyl]dimethyltitanium,
[0392] [(N-tert-butylamino)(η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0393] [(N-methylamino)(η5-cyclopentadienyl)-1,2-ethanediyl]dimethyltitanium,
[0394] [(N-methylamino)(η5-cyclopentadienyl)dimethylsilane]dimethyltitanium,
[0395] [(N-tert-butylamino)(η5-indenyl)dimethylsilane]dimethyltitanium,
[0396] [(N-benzylamino)(η5-indenyl)dimethylsilane]dimethyltitanium, etc.
[0397] Specific examples of the transition metal compound component [B-2] used in the present embodiment are not particularly limited, and examples thereof include: a compound having a "dimethyl" portion (which is the portion in the middle of the name of each compound, i.e., the portion immediately preceding the portion called "titanium") of the name of each titanium compound listed above, which is the same as X in the above (Formula 4) 3 The compound is a compound having a name obtained by replacing the name corresponding to the part of (a) with any group listed below.
[0398] "Dichloro"
[0399] "Dibromo"
[0400] "Diiodine"
[0401] "Diethyl",
[0402] "Dibutyl"
[0403] "Diphenyl"
[0404] "Dibenzyl"
[0405] "2-(N,N-dimethylamino)benzyl",
[0406] "2-Butene-1,4-diyl",
[0407] "s-trans-η4-1,4-diphenyl-1,3-butadiene",
[0408] "s-trans-η4-3-methyl-1,3-pentadiene",
[0409] "s-trans-η4-1,4-dibenzyl-1,3-butadiene",
[0410] "s-trans-η4-2,4-hexadiene",
[0411] "s-trans-η4-1,3-pentadiene",
[0412] "s-trans-η4-1,4-dimethylbenzene-1,3-butadiene",
[0413] "s-trans-η4-1,4-bis(trimethylsilyl)-1,3-butadiene",
[0414] "s-cis-η4-1,4-diphenyl-1,3-butadiene",
[0415] "s-cis-η4-3-methyl-1,3-pentadiene",
[0416] "s-cis-η4-1,4-dibenzyl-1,3-butadiene",
[0417] "s-cis-η4-2,4-hexadiene",
[0418] "s-cis-η4-1,3-pentadiene",
[0419] "s-cis-η4-1,4-dimethylbenzene-1,3-butadiene",
[0420] "s-cis-η4-1,4-bis(trimethylsilyl)-1,3-butadiene" and the like.
[0421] As a specific example of such a transition metal compound component [B-2], [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]titanium complex is preferred.
[0422] The transition metal compound component [B-2] used in the present embodiment is not particularly limited and can be generally synthesized by a known method.
[0423] Next, the activator [C] and the organometallic compound component [D] used in the present embodiment, which can form a complex exhibiting catalytic activity by reacting with the transition metal compound, are described.
[0424] The activator [C] in the present embodiment is not particularly limited, and examples thereof include a compound (C-1) defined by the following (Formula 5).
[0425] (C-1): [L 2 -H] d+ [M 3 r Q s ] d- ……(Formula 5)
[0426] Among them, in formula 5, [L 2 -H] d+ For proton-donating Bronsted acids, L 2 is a neutral Lewis base. In addition, in Formula 5, [M 3 r Q s ] d- is a compatible non-coordinating anion, M 3 is a metal or metalloid selected from Groups 5 to 15 of the periodic table, Q is independently a hydride ion, a dialkylamino group, a halide ion, an alkoxy group, an allyloxy group, a hydrocarbon group, or a substituted hydrocarbon group having 20 or less carbon atoms, and the number of Q being a halide ion is 1 or less. In addition, r is an integer of 1 to 7, s is an integer of 2 to 14, d is an integer of 1 to 7, and sr=d.
[0427] The non-coordinating anion is not particularly limited, and examples thereof include the following compounds.
[0428] Tetraphenylborane anion,
[0429] tri(p-tolyl)(phenyl)boron anion,
[0430] tris(pentafluorophenyl)(phenyl)boron anion,
[0431] Tris(2,4-dimethylphenyl)(hydroxyphenyl)boron anion,
[0432] tris(3,5-dimethylphenyl)(phenyl)boron anion,
[0433] tris(3,5-bis(trifluoromethyl)phenyl)(phenyl)boron anion,
[0434] tris(pentafluorophenyl)(cyclohexyl)borane anion,
[0435] tris(pentafluorophenyl)(naphthyl)boron anion,
[0436] Tetrakis(pentafluorophenyl)borane anion,
[0437] Triphenyl(hydroxyphenyl)borane anion,
[0438] Diphenylbis(hydroxyphenyl)borane anion,
[0439] Triphenyl(2,4-dihydroxyphenyl)borane anion,
[0440] tri(p-tolyl)(hydroxyphenyl)boron anion,
[0441] tris(pentafluorophenyl)(hydroxyphenyl)boron anion,
[0442] Tris(2,4-dimethylphenyl)(hydroxyphenyl)boron anion,
[0443] tris(3,5-dimethylphenyl)(hydroxyphenyl)boron anion,
[0444] tris(3,5-bis(trifluoromethyl)phenyl)(hydroxyphenyl)boron anion,
[0445] tris(pentafluorophenyl)(2-hydroxyethyl)borane anion,
[0446] tris(pentafluorophenyl)(4-hydroxybutyl)borane anion,
[0447] tris(pentafluorophenyl)(4-hydroxycyclohexyl)borane anion,
[0448] tris(pentafluorophenyl)(4-(4'-hydroxyphenyl)phenyl)boron anion,
[0449] tris(pentafluorophenyl)(6-hydroxy-2-naphthyl)boron anion,
[0450] tris(pentafluorophenyl)(4-hydroxyphenyl)borane anion, etc.
[0451] Examples of other preferred non-coordinating anions are not particularly limited, and include, for example, boron anions in which the hydroxyl group of the above-exemplified boron anions is replaced by an NHR group. Here, R is preferably a methyl group, an ethyl group, or a tert-butyl group.
[0452] In addition, there are no particular restrictions on the proton-donating Bronsted acid, and examples thereof include trialkyl-substituted ammonium cations such as triethylammonium, tripropylammonium, tri-n-butylammonium, trimethylammonium, tributylammonium, and tri-n-octylammonium. In addition, N,N-dimethylanilinium, N,N-diethylanilinium, N,N,2,4,6-pentamethylanilinium, and N,N-dimethylbenzylanimium are also suitable. In addition, dialkylammonium cations such as di(isopropyl)ammonium and dicyclohexylammonium are also suitable, and triphenylammonium is also suitable. Tris(methylphenyl) Tris(dimethylphenyl) isotriaryl cation; or dimethylsulfonium, diethylsulfonium, diphenylsulfonium, etc. are also suitable.
[0453] The activator (C-1) used in this embodiment can be a reaction product with an organoaluminum compound. The organoaluminum compound is not particularly limited, and examples thereof include: trimethylaluminum, triethylaluminum, tributylaluminum, trihexylaluminum, trioctylaluminum, tridecylaluminum, etc.; or reaction products of these alkylaluminums with alcohols such as methanol, ethanol, butanol, pentanol, hexanol, octanol, and decanol, such as dimethyl methoxyaluminum, diethyl ethoxyaluminum, dibutyl butoxyaluminum, etc. In addition, the reaction products with the above-mentioned organoaluminum compounds can be used alone or in combination.
[0454] In the present embodiment, as the activator [C], an organic metal oxide compound (C-2) having a unit represented by the following (Formula 6) can also be used.
[0455] (C-2): -(M 4 R 7 t-2 -O) u -……(Formula 6)
[0456] (Among them, M 4 is a metal or metalloid of Group 13 to Group 15 of the Periodic Table, R 7 are each independently a hydrocarbon group having 1 to 12 carbon atoms or a substituted hydrocarbon group having 1 to 12 carbon atoms, and t is a metal M 4 valence, u is an integer greater than 2. )
[0457] The activator (C-2) is not particularly limited, and examples thereof include an organic aluminum oxy-compound represented by the following (Formula 7).
[0458] [-Al(Me)-O-] v -[-Al(R 8 )-O-] w ……(Formula 7)
[0459] In formula 7, R 8 is a hydrocarbon group having 1 to 12 carbon atoms. 8Specifically, there is no particular limitation, and examples thereof include: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, pentyl, hexyl, octyl, decyl, cyclohexyl, cyclooctyl, etc. Among them, methyl and ethyl are preferred, and methyl is particularly preferred. In the above formula, for example, as examples of organic aluminum oxide compounds composed of an alkyl aluminum unit, there is no particular limitation, and examples thereof include: methylaluminoxane, ethylaluminoxane, n-propylaluminoxane, isopropylaluminoxane, n-butylaluminoxane, isobutylaluminoxane, pentylaluminoxane, hexylaluminoxane, octylaluminoxane, decylaluminoxane, cyclohexylaluminoxane, cyclooctylaluminoxane, etc. Among them, methylaluminoxane and ethylaluminoxane are preferred, and methylaluminoxane is particularly preferred.
[0460] As such, as the organic aluminum oxide compound used in the present embodiment, an organic aluminum oxide compound composed of an alkoxy aluminum unit represented by the above formula can be cited, but it is not necessarily limited to a compound composed of one structural unit, and can also be composed of multiple structural units. Specifically, there is no particular restriction, for example, methylethylaluminoxane, methylpropylaluminoxane, methylbutylaluminoxane, etc. can be cited, and the ratio of various structural units can be arbitrarily selected in the range of 0% to 100%. In addition, it can also be a mixture of multiple organic aluminum oxide compounds composed of one structural unit. Specifically, there is no particular restriction, for example, a mixture of methylaluminoxane and ethylaluminoxane, a mixture of methylaluminoxane and n-propylaluminoxane, a mixture of methylaluminoxane and isobutylaluminoxane, etc. can be cited. In addition, v and w can take any number, and from the perspective of easy manufacturing, the ratio v / w of v to w is preferably 0.1 or more and 10 or less, and more preferably 0.3 or more and 5 or less.
[0461] In addition, the organoaluminum oxy-compound used in the present embodiment may contain unreacted chemical substances from its production method. That is, the organoaluminum oxy-compound is generally prepared by reacting trialkylaluminum with H 2 O, but some of these raw materials may remain as unreacted chemical substances. Specifically, there is no particular limitation, and examples thereof include the following: in the case of synthesizing methylaluminoxane, trimethylaluminum and H 2 O as raw materials, one or both of these raw materials are contained in methylaluminoxane as unreacted chemical substances; etc. In the above-exemplified method for producing an organic aluminum oxy-compound, a ratio of H 2 O more trialkylaluminum, so trialkylaluminum is often contained as a residual chemical substance in the organoaluminum oxy-compound.
[0462] The organometallic compound component [D] in the present embodiment is preferably a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, and an organoaluminum compound and / or an organomagnesium compound are particularly preferred.
[0463] As the organoaluminum compound, it is preferred to use a compound represented by the following (Formula 8) alone or in combination.
[0464] (D-1):AlR 8 l Z 2 (3-1)……(Formula 8)
[0465] (In Formula 8, R 8 is a hydrocarbon group having 1 to 20 carbon atoms, Z 2 is any group belonging to the group consisting of hydrogen, halogen, alkoxy, allyloxy, and siloxy, and l is a number of 2 to 3.)
[0466] In the above (Formula 8), R 8 The hydrocarbon group having 1 or more and 20 or less carbon atoms represented by is not particularly limited, and examples thereof include hydrocarbon groups containing aliphatic hydrocarbons, aromatic hydrocarbons or alicyclic hydrocarbons, and specifically include trialkylaluminums such as trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, tri(2-methylpropyl)aluminum (or triisobutylaluminum), tripentylaluminum, tri(3-methylbutyl)aluminum, trihexylaluminum, trioctylaluminum, and tridecylaluminum; aluminum halide compounds such as diethylaluminum chloride, ethylaluminum dichloride, di(2-methylpropyl)aluminum chloride, ethylaluminum sesquichloride, and diethylaluminum bromide; alkoxyaluminum compounds such as ethoxydiethylaluminum and butoxydi(2-methylpropyl)aluminum; siloxyaluminum compounds such as dimethylhydrogensilyloxydimethylaluminum, ethylmethylhydrogensilyloxydiethylaluminum, and ethyldimethylsilyloxydiethylaluminum, and mixtures thereof as preferred organoaluminum compounds. In particular, trialkylaluminum compounds are more preferred.
[0467] As the organomagnesium compound, it is preferred to use the organomagnesium compound (A-1) represented by the above (Formula 1) alone or in combination.
[0468] Regarding γ, δ, e, f, g, M in the above (Formula 1), 1 , R 1 , R 2 , OR 3 As already described, the organic magnesium compound preferably has high solubility in an inert hydrocarbon solvent, and thus β / α is preferably in the range of 0.5 to 10. In addition, M is further preferably 1 Aluminum compounds.
[0469] As other organic magnesium compounds, organic magnesium compounds (D-2) represented by the following (Formula 9) can be used alone or in combination.
[0470] (D-2): (M 5 ) α (Mg) β (R 9 ) a (R 10 ) b Y 2 c ……(Formula 9)
[0471] (In Formula 9, M 5 is a metal atom belonging to the group consisting of Group 12, Group 13 and Group 14 of the periodic table, R 9 and R 10 is a hydrocarbon group having 2 to 20 carbon atoms, Y 2 Alkoxy, silyloxy, allyloxy, amino, amide, -N=CR 11 ,R 12 、-SR 13 (Among them, R 11 , R 12 and R 13 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 2 α, β, a, b and c are real numbers satisfying the following relationship: 0≤α, 0<β, 0≤a, 0≤b, 0≤c, 0<a+b, 0≤c / (α+β)≤2, mα+2β=a+b+c (where m represents M 5 The atomic valence of
[0472] Next, an example of a method for producing a polyethylene polymerization catalyst from inorganic solid particles [A], transition metal compound component [B-1], transition metal compound component [B-2], and activator [C] and / or organometallic compound component [D] is described.
[0473] In this embodiment, although not particularly limited, the polyethylene polymerization catalyst is produced by reacting, for example, the transition metal compound component [B-1], the transition metal compound component [B-2], the activator [C] and / or the organometallic compound component [D] with the inorganic solid particles [A].
[0474] The reaction is preferably carried out in an inert hydrocarbon solvent. There are no particular restrictions on the inert hydrocarbon solvent, and specific examples include aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane. Among them, it is more preferably carried out in an aliphatic hydrocarbon solvent such as hexane and heptane.
[0475] In this reaction, from the viewpoint of reaction efficiency, the transition metal compound component [B-1] and the transition metal compound component [B-2] are preferably used for the reaction after being dissolved in an inert hydrocarbon solvent. In addition, the concentration during dissolution is not particularly limited, but from the viewpoint of avoiding segregation on the surface of the inorganic solid particles [A], it is preferably 0.01 mol / L or more and 5 mol / L or less, and more preferably 0.05 mol / L or more and 2 mol / L or less.
[0476] In this reaction, only one of the transition metal compound component [B-1] and the transition metal compound component [B-2] may be used, but from the viewpoint of controlling the amount of long chain branches in polyethylene, it is preferred to use both.
[0477] In this reaction, from the viewpoint of easily controlling the amount of long-chain branches of polyethylene, it is preferred to change the type or amount of the activator [C] and the organometallic compound component [D] for each transition metal compound component. In addition, the concentrations of the activator [C] and the organometallic compound component [D] are not particularly limited, but from the viewpoint of reactivity with the transition metal compound component, they are preferably 0.01 mol / L or more and 5 mol / L or less, and more preferably 0.05 mol / L or more and 2 mol / L or less. It should be noted that an inert hydrocarbon solvent is preferably used for diluting the activator [C] and the organometallic compound component [D].
[0478] In this reaction, the method for adding the transition metal compound component [B-1], the transition metal compound component [B-2], the activator [C], and the organometallic compound component [D] is not particularly limited. From the viewpoint of forming a layer of the transition metal compound component and the activator and / or the organometallic compound component, it is preferred to add a mixture obtained by mixing the transition metal compound component with the activator and / or the organometallic compound component in advance to the inorganic solid particles [A]; or to add the transition metal compound component and the activator and / or the organometallic compound component to the inorganic solid particles [A] at the same time. In addition, from the viewpoint of introducing the macromonomer generated from the transition metal compound component [B-1] into the transition metal compound component [B-2], it is preferred to add the transition metal compound component [B-1] activated by the activator [C] and / or the organometallic compound component [D] to the inorganic solid particles [A], and then add the transition metal compound component [B-2] activated by the activator [C] and / or the organometallic compound component [D].
[0479] The reaction temperature of the reaction is not particularly limited, but is preferably -20°C to 100°C, and more preferably 0°C to 80°C, from the viewpoint of reaction efficiency.
[0480] In this reaction, there is no particular restriction on the molar ratio of the transition metal compound component [B-1] to the transition metal compound component [B-2] ([B-2] / [B-1]). From the viewpoint of controlling the amount of long chain branches in polyethylene to a trace amount, it is preferably greater than 1 and less than 1000, and more preferably greater than 5 and less than 100.
[0481] In this reaction, there is no particular restriction on the molar ratio ([C] / [B-1]) of the transition metal compound component [B-1] to the activator [C]. When the activator [C] is (C-1), from the viewpoint of controlling the amount of long-chain branches in polyethylene to a trace amount, the molar ratio is preferably 0.1 to 1, and more preferably 0.1 to 0.5.
[0482] In this reaction, the molar ratio of the transition metal compound component [B-1] to the activator [C] ([C] / [B-1]) is not particularly limited. When the activator [C] is (C-2), from the viewpoint of controlling the amount of long-chain branches in the polyethylene to a trace amount and suppressing the amount of metal residues in the polyethylene, it is preferably 1 to 60, and more preferably 1 to 30.
[0483] In this reaction, there is no particular restriction on the molar ratio ([D] / [B-1]) of the transition metal compound component [B-1] to the organometallic compound component [D]. From the viewpoint of controlling the amount of long chain branches in polyethylene to a trace amount and suppressing the amount of metal residues in polyethylene, it is preferably greater than 1 and less than 60, and more preferably greater than 1 and less than 30.
[0484] In this reaction, there is no particular restriction on the molar ratio ([C] / [B-2]) of the transition metal compound component [B-2] to the activator [C]. When the activator [C] is (C-1), from the viewpoint of controlling the amount of long-chain branches in polyethylene to a trace amount, it is preferably 0.5 to 1.5, and more preferably 0.9 to 1.1.
[0485] In this reaction, the molar ratio of the transition metal compound component [B-2] to the activator [C] ([C] / [B-2]) is not particularly limited. When the activator [C] is (C-2), from the viewpoint of controlling the amount of long-chain branches in the polyethylene to a trace amount and suppressing the amount of metal residues in the polyethylene, it is preferably 2 or more and 200 or less, and more preferably 5 or more and 100 or less.
[0486] In this reaction, there is no particular restriction on the molar ratio ([D] / [B-1]) of the transition metal compound component [B-2] to the organometallic compound component [D]. From the viewpoint of controlling the amount of long chain branches in polyethylene to a trace amount and suppressing the amount of metal residues in polyethylene, it is preferably greater than 1 and less than 60, and more preferably greater than 1 and less than 30.
[0487] Next, the impurity capture agent used in the polymerization of the polyethylene powder according to the present embodiment will be described.
[0488] The impurity scavenger used in the polymerization of the polyethylene powder of the present embodiment is not particularly limited, but the above-mentioned organometallic compound component [D] is preferably used.
[0489] There is no particular limitation on the method of adding the organometallic compound component [D] to the polymerization system under polymerization conditions. The organometallic compound component [D] may be added to the polymerization system separately from the catalyst component or may be added to the polymerization system after reacting with the catalyst component in advance.
[0490] There is no particular restriction on the concentration of the organometallic compound component [D] in the polymerization system. From the viewpoint of completely capturing impurities and the amount of metal residue in the polymer, it is preferably from 0.001 mmol / L to 10 mmol / L, more preferably from 0.01 mmol / L to 5 mmol / L, and even more preferably from 0.05 mmol / L to 2 mmol / L.
[0491] In the present embodiment, the organometallic compound component [D] may be used alone or in combination of two or more.
[0492] (Polymerization method of ethylene polymer)
[0493] The polymerization method of the ethylene polymer constituting the polyethylene powder of the present embodiment is not particularly limited, and examples thereof include a method of polymerizing ethylene or copolymerizing ethylene and a comonomer by suspension polymerization or gas phase polymerization. Among them, suspension polymerization is preferred because it can effectively remove polymerization heat.
[0494] In the suspension polymerization method, an inert hydrocarbon medium can be used as a solvent, and olefin itself can also be used as a solvent.
[0495] There are no particular restrictions on the inert hydrocarbon medium, and examples thereof include: aliphatic hydrocarbons such as propane, butane, isobutane, pentane, isopentane, hexane, heptane, octane, decane, dodecane, kerosene, etc.; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc.; halogenated hydrocarbons such as ethyl chloride, chlorobenzene, dichloromethane, etc., or mixtures thereof, etc.
[0496] In the present embodiment, the polymerization temperature in the polymerization of ethylene is usually preferably 30° C. or higher and 100° C. or lower, more preferably 35° C. or higher and 95° C. or lower, and particularly preferably 40° C. or higher and 90° C. or lower. When the polymerization temperature is 30° C. or higher, industrially efficient production can be achieved. On the other hand, when the polymerization temperature is 100° C. or lower, block scale generated by partial melting of the polymer can be suppressed, and continuous and stable production can be performed without clogging the pipeline.
[0497] The polymerization pressure of the ethylene polymer in the method for producing the polyethylene powder of the present embodiment is preferably normal pressure or higher and 2 MPaG or lower, more preferably 0.2 MPaG or higher and 1.5 MPaG or lower, and even more preferably 0.3 MPaG or higher and 0.9 MPaG or lower.
[0498] When the polymerization pressure is at least normal pressure, industrially efficient production can be achieved. On the other hand, when the polymerization pressure is 2 MPaG or less, stable production tends to be possible without causing bulk fouling due to rapid polymerization in the polymerization reactor.
[0499] Generally, when obtaining an ethylene-based polymer by polymerization, an antistatic agent such as Stadis or STATSAFE manufactured by Innospec (distributor: Maruwa Bussan) can be used to suppress static electricity adhesion of the polymer to the polymerization reactor.
[0500] Regarding antistatic agents such as Stadis and STATSAFE, the antistatic agent diluted in an inert hydrocarbon medium can be added to the polymerization reactor using a pump, etc. The antistatic agent can be added by a method of adding it to a solid catalyst in advance, adding it to the polymerization reactor, etc., and the amount of the antistatic agent added is preferably 1 ppm or more and 500 ppm or less, and more preferably 10 ppm or more and 100 ppm or less, relative to the production of the ethylene-based polymer per unit time.
[0501] As described in the specification of German Patent Application Publication No. 3127133, the molecular weight of ethylene polymer can be controlled by making hydrogen exist in the polymerization system or changing the polymerization temperature. By adding hydrogen as a chain transfer agent in the polymerization system, the molecular weight of ethylene polymer can be controlled within an appropriate range. When adding hydrogen in the polymerization system, the mole fraction of hydrogen is preferably 0 mol % or more and 50 mol % or less, more preferably 0 mol % or more and 30 mol % or less, further preferably 0 mol % or more and 20 mol % or less.
[0502] In addition, when hydrogen is added to the polymerization system, hydrogen can also be contacted with the catalyst in advance and then added to the polymerization system from the catalyst introduction line. Just after the catalyst is introduced into the polymerization system, since the catalyst concentration near the introduction line outlet becomes high, rapid polymerization is performed, and the possibility of generating a local high temperature state becomes high. On the other hand, by contacting hydrogen and the catalyst before introducing them into the polymerization system, the initial activity of the catalyst can be suppressed, and the generation of block fouling caused by rapid polymerization, the deactivation of the catalyst at high temperature, etc. can be suppressed.
[0503] In addition, in the present embodiment, in addition to the above-mentioned components, other known components useful in the production of polyethylene may be contained.
[0504] The polymerization reaction can be carried out in any of a batch method, a semi-continuous method and a continuous method, but is preferably carried out in a continuous method.
[0505] By continuously supplying ethylene gas, solvent, catalyst, etc. into the polymerization system and continuously discharging them together with the produced ethylene polymer, it is possible to suppress local high temperature state due to rapid reaction of ethylene and make the polymerization system more stable.
[0506] When ethylene reacts in a uniform state in the polymerization system, the generation of branches, double bonds, etc. in the polymer chain is suppressed, or the generation of low molecular weight components and ultra-high molecular weight bodies due to the decomposition and cross-linking of the ethylene polymer is suppressed, and the crystalline components of the ethylene polymer are easily generated. Thus, it is easy to obtain a sufficient amount of crystalline components required for achieving the strength required for the microporous membrane, etc.
[0507] The polymerization reaction of the ethylene-based polymer may be a single-step polymerization method using one polymerization reactor, or a multi-step polymerization method in which polymerization is carried out sequentially and continuously in two or more polymerization reactors connected in series.
[0508] A suspension of an ethylene-based polymer containing the polyethylene powder constituting the present embodiment is quantitatively extracted from the polymerization reactor and transferred to a flash tank, and unreacted ethylene, hydrogen, and comonomer (limited to the case where copolymerization is carried out in the reactor) are separated.
[0509] The solvent separation method in the polymerization step of the polyethylene powder of the present embodiment can be any of decantation, centrifugation, filtration, etc., and centrifugation is more preferred because it has a good separation efficiency between the ethylene polymer and the solvent.
[0510] The method for deactivating the catalyst used in the polymerization step of the ethylene polymer constituting the polyethylene powder of the present embodiment is not particularly limited, but the deactivation of the catalyst is preferably carried out after the ethylene polymer is separated from the solvent.
[0511] By introducing a chemical agent for deactivating the catalyst after separating the polyethylene powder from the solvent, it is possible to suppress precipitation of low molecular weight components, catalyst components, etc. contained in the solvent into the ethylene-based polymer.
[0512] The chemical agent for deactivating the catalyst is not particularly limited, and examples thereof include oxygen, water, alcohols, glycols, phenols, carbon monoxide, carbon dioxide, ethers, carbonyl compounds, and alkynes.
[0513] In the method for producing polyethylene powder of the present embodiment, it is preferred to separate the ethylene polymer from the solvent and then perform a drying step. In the drying step, a rotary kiln method, a paddle method, a fluidized bed dryer, etc. are preferably used. In addition, the drying temperature is preferably 50° C. to 150° C., and more preferably 70° C. to 110° C.
[0514] In addition, it is also effective to introduce an inert gas such as nitrogen into the dryer to promote drying. In this case, it is also more effective to add steam or the like as a chemical agent to deactivate the catalyst.
[0515] After the ethylene-based polymer constituting the polyethylene powder of the present embodiment is dried, it may be sieved to remove coarse powder.
[0516] The polyethylene powder of the present embodiment may be a mixture of a plurality of polyethylene powders containing an ethylene-based polymer obtained by the above-mentioned production method.
[0517] Furthermore, the present invention may be used in combination with known additives such as a slip agent, a neutralizer, an antioxidant, a light stabilizer, an antistatic agent, and a pigment, as required.
[0518] The lubricant or neutralizer is not particularly limited, and examples thereof include aliphatic hydrocarbons, higher fatty acids, higher fatty acid metal salts, alcohol fatty acid esters, waxes, higher fatty acid amides, silicone oils, rosin, etc. Specifically, stearates such as calcium stearate, magnesium stearate, and zinc stearate are suitable additives.
[0519] The antioxidant is not particularly limited, but for example, phenolic compounds or phenolic phosphorus-containing compounds are preferred. Specifically, phenolic antioxidants such as 2,6-di-tert-butyl-4-methylphenol (butylhydroxytoluene), octadecyl 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate, and tetrakis(methylene-(3,5-di-tert-butyl-4-hydroxyhydrocinnamate))methane; phenolic phosphorus-containing antioxidants such as 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphophetidine; and phosphorus-containing antioxidants such as 4,4'-biphenylene diphosphite tetrakis(2,4-di-tert-butylphenyl) ester, tris(2,4-di-tert-butylphenyl) phosphite, and cyclic neopentanetetraylbis(2,4-di-tert-butylphenyl phosphite).
[0520] The light stabilizer is not particularly limited, and examples thereof include benzotriazole-based light stabilizers such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole and 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole; and hindered amine-based light stabilizers such as bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino)hexamethylene}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}].
[0521] The antistatic agent is not particularly limited, and examples thereof include aluminosilicate, kaolin, clay, natural silica, synthetic silica, silicates, talc, diatomaceous earth, and fatty acid glycerides.
[0522] [use]
[0523] The polyethylene powder of the present embodiment can be used as a raw material for various molded bodies such as microporous films, fibers, particularly high-strength fibers, sintered bodies, press-molded bodies, and plunger extrusion-molded bodies.
[0524] The polyethylene powder of this embodiment is particularly suitable as a raw material for a microporous film for battery separators.
[0525] [Molding body]
[0526] The molded product of the present embodiment is a molded product of the polyethylene powder of the present embodiment described above.
[0527] The molded body is not particularly limited, and examples thereof include microporous membranes, particularly microporous membranes for battery separators, fibers, particularly high-strength fibers, sintered bodies, press-molded bodies, and plunger extrusion-molded bodies.
[0528] The method for producing the molded body is not particularly limited, and examples thereof include a molding method that involves the steps of extruding a resin using a wet extrusion method, stretching, extracting, and drying.
[0529] The battery separator is not particularly limited, and examples thereof include separators for lithium ion secondary batteries and separators for lead acid batteries.
[0530] Example
[0531] Hereinafter, the present embodiment will be described in more detail by way of specific examples and comparative examples, but the present invention is not limited to the following examples and comparative examples.
[0532] First, the method for evaluating the physical properties of polyethylene powder will be described.
[0533] [Physical properties of polyethylene powder]
[0534] (Viscosity average molecular weight (Mv))
[0535] The viscosity average molecular weight of the polyethylene powder is measured by the method shown below in accordance with ISO 1628-3 (2010).
[0536] First, weigh 4.0 mg to 4.5 mg of polyethylene powder in a dissolving tube. The weighed mass is recorded as "m (unit: mg)" in the following formula. Next, use a vacuum pump to degas the air inside the dissolving tube and replace it with nitrogen, then add 20 mL of decalin (decalin after adding 1 g / L of 2,6-di-tert-butyl-4-methylphenol, degassing with a vacuum pump and replacing it with nitrogen, hereinafter referred to as decalin), stir at 150°C for 90 minutes to dissolve the polyethylene powder, and thus prepare a decalin solution.
[0537] Then, the decalin solution was placed in a Cannon-Fenske viscometer (manufactured by Shibata Scientific Instruments Co., Ltd. / viscometer No. 100) in a constant temperature liquid tank at 135° C., and the falling time between the marking lines (t s ).
[0538] In addition, the falling time (t b ), and the specific viscosity (η) is calculated according to the following (Formula A) sp ).
[0539] η sp =(t s / t b )-1(Formula A)
[0540] By specific viscosity (η sp) and concentration (C) (unit: g / dL) are used to calculate the intrinsic viscosity IV ([η]) using the following (Formula B) and (Formula C).
[0541] Concentration C = m / (20×γ) / 10 (unit: g / dL) (Formula B)
[0542] γ = (density of decalin at 20°C) / (density of decalin at 135°C)
[0543] =0.888 / 0.802=1.107
[0544] Intrinsic viscosity IV = (η sp / C) / (1+0.27×η sp )(Formula C)
[0545] The intrinsic viscosity IV is substituted into the following (Formula D) to determine the viscosity average molecular weight (Mv).
[0546] Viscosity average molecular weight (Mv) = (5.34 × 10 4 )×[η] 1.49 (Formula D)
[0547] (Difference between the temperature of the peak top and the temperature of the peak convergence point in the DSC curve of the second heating process (crystal thickness parameter))
[0548] It was determined by the method shown below using a differential scanning calorimeter (manufactured by PerkinElmer Inc. / product name: DSC8000).
[0549] First, an aluminum pan containing 8.5 mg of polyethylene powder was placed in a heating furnace in a DSC device and heated according to the <measurement conditions> shown below. However, all heating operations were performed under a nitrogen atmosphere.
[0550] <Measurement conditions>
[0551] (1) Stand at 50°C for 1 minute
[0552] (2) Heating from 50°C to 180°C at 10°C / min (first heating)
[0553] (3) Stand at 180°C for 5 minutes
[0554] (4) Cooling from 180°C to 50°C at 10°C / min
[0555] (5) Stand at 50°C for 5 minutes
[0556] (6) Heating from 50°C to 180°C at 10°C / min (second heating)
[0557] Then, the temperature (Tm2) at which the peak of the endothermic peak obtained in the second temperature increase process appears is determined. top ) and the peak convergence point (Tm2 end ).
[0558] Finally, the values of each temperature are substituted into the (Formula E) shown below to calculate the difference between the temperature of the peak top and the temperature of the peak convergence point in the DSC curve of the second heating process (crystal thickness parameter).
[0559] (Temperature difference) = Tm2 end -Tm2 top (Formula E)
[0560] It should be noted that regarding Tm2 end , calculate according to the steps shown below.
[0561] <Tm2 end Calculation steps>
[0562] (1) Differentiate the amount of heat absorbed during the second heating process by temperature.
[0563] (2) For the absolute value of the differential value obtained in (1), the absolute value of the differential value obtained in (1) is calculated from Tm2 top The temperature when the number of starts and the temperature when it first reaches below 0.01 is taken as Tm2 end .
[0564] (z-average shrinkage factor g z )
[0565] The calculation was performed by the method shown below using a gel permeation chromatography (GPC) measuring apparatus (manufactured by Agilent / product name: PL-GPC220) equipped with a differential refractometer (RI) and a viscosity detector (Viscometer).
[0566] First, a predetermined amount of polyethylene powder was added to 1,2,4-trichlorobenzene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with 125 mg / L of antioxidant 4,4'-thiobis(2-tert-butyl-5-methylphenol) added). At this time, the concentration was prepared as shown in the following <Sample Concentration>.
[0567] <Sample concentration>
[0568] When Mv is less than 300,000: 10 mg / 10 mL
[0569] When Mv is greater than or equal to 300,000 and less than 1,000,000: 3 mg / 10 mL
[0570] When Mv is greater than or equal to 1 million and less than 2 million: 2 mg / 10 mL
[0571] When Mv is greater than or equal to 2 million and less than 3 million: 1.5 mg / 10 mL
[0572] When Mv is 3 million or more: 1.5 mg / 15 mL
[0573] The prepared sample solution was heated and shaken according to the <Dissolution Conditions> shown below. The dissolved sample solution was placed in an automatic sampler heated to 160° C. without cooling.
[0574] <Dissolution conditions>
[0575] (1) Heat to 150°C and let stand for 1 hour
[0576] (2) Heating to 150°C while shaking for 2 hours
[0577] (3) Heat to 150°C and let stand for 30 minutes
[0578] Next, measurement was performed under the <GPC measurement conditions> shown below.
[0579] <GPC measurement conditions>
[0580] Differential Refractometer (RI): Built-in
[0581] Viscometer: PL-BV400
[0582] Detector connection method: parallel connection
[0583] Column: PLgel 20 μm MIXED-A 300×7.5 mm (manufactured by Agilent)
[0584] Column connection method: connect two of the above columns in series
[0585] Mobile phase: 1,2,4-trichlorobenzene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., with antioxidant 4,4'-thiobis(2-tert-butyl-5-methylphenol) added at a concentration of 125 mg / L)
[0586] Column temperature: 160°C
[0587] Detector temperature: 160°C
[0588] Sample solution temperature: 160°C
[0589] Injection temperature: 160°C
[0590] Injection volume: 0.5mL
[0591] Flow rate: 1.0mL / min
[0592] In addition, the column calibration was performed by the universal calibration method using the <Sample for Calibration Curve Preparation> shown below.
[0593] <Samples for Calibration Curve Creation>
[0594] Made by Agilent, EasiVial TM PS-H Polystyrene (High MW)
[0595] Agilent, PL Polymer Standard (Model: PL2013-6001)
[0596] Manufactured by Agilent, PL Polymer Standard (Model: PL2014-9001)
[0597] Next, the data obtained by measuring under the above conditions were analyzed using CIRRUSGPC / SEC Software (version 3.4) manufactured by Agilent, and a Mark-Houwink Plot (a double logarithmic plot obtained by plotting the molecular weight MW on the horizontal axis and the intrinsic viscosity IV on the vertical axis) was prepared. In this figure, for the region on the low molecular weight side lower than the peak top molecular weight and the region where the double logarithmic plot changes linearly, the following (Formula F) was used for fitting, and a linear reference line represented by (Formula G) was prepared.
[0598] log 10 IV=alog 10 MW+log 10 C (Formula F)
[0599] log 10 IV=a linear log 10 MW+log 10 C linear (Formula G)
[0600] (In formula F and formula G, a and C are variables used in fitting, a linear and C linear are constants obtained through fitting)
[0601] Next, using the following (Formula H) and (Formula I), the intrinsic viscosity IV of the sample with the same molecular weight is used. sample and the intrinsic viscosity IV of the linear baseline linear The values of g' and g' are calculated z .
[0602] g'=IV sample / IV linear (Formula H)
[0603] g' z =Σ(Conc i ×MW i ×g' i ) / Σ(Conc i ×MW i ) (Formula I)
[0604] (In Formula I, Conc i is the solution concentration of the i-th fraction, MW i is the molecular weight of the i-th fraction, g' i is the g' of the i-th fraction)
[0605] Finally, the z-average shrinkage factor g is calculated using the following (Formula J): z .
[0606] z-average shrinkage factor g z =g' z (1 / 0.75) (Formula J)
[0607] (Evaluation of stretchability)
[0608] Evaluation was performed by the method shown below using a Labo Plastomill mixer (main body model: 30C150, mixer model: R-60) and a simultaneous biaxial stretching machine manufactured by Toyo Seiki Co., Ltd.
[0609] First, in a resin container, 12 g of polyethylene powder, 0.4 g of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (product name: Adecastab AO-60G) manufactured by ADEKA Corporation as an antioxidant, and 28 g of liquid paraffin (product name: P-350P) manufactured by MORESCO Co., Ltd. were thoroughly mixed to obtain a mixture.
[0610] Next, the mixture was placed in a LaboPlastomill mixer (main body model: 30C150, mixer model: R-60) manufactured by Toyo Seiki Co., Ltd., set at a temperature of 200° C., and kneaded for 10 minutes at a rotation speed of 5 rpm, and then further kneaded for 10 minutes at a rotation speed of 50 rpm, thereby obtaining a polyethylene gel. The gel was formed into a sheet based on the <Gel Sheet Preparation Conditions> shown below.
[0611] <Gel sheet production conditions>
[0612] (1) The polyethylene gel is filled into a mold of 200 mm x 200 mm x 1 mm thick.
[0613] (2) Using a press machine with a set temperature of 180°C, the mold was heated to 1 kg / cm 2 Preheat for 3 minutes at 10 kg / cm 2 Press down for 2 minutes.
[0614] (3) Using a room temperature cooling press, at 10 kg / cm 2 The mold was cooled for 10 minutes.
[0615] (4) The resulting film was cut into a size of 100 mm x 100 mm x 1 mm thick to obtain a gel sheet.
[0616] The gel sheet thus obtained was stretched to 7×7 times at 115° C. using a simultaneous biaxial stretching machine to obtain a stretched film. At this time, stretchability was evaluated according to the following (Stretchability Evaluation Criteria).
[0617] (Evaluation criteria for stretchability)
[0618] ○(Pass): No membrane rupture
[0619] ×(Unqualified): There is membrane rupture
[0620] (400cm -1 ~450cm -1 Absorption coefficient in the range of
[0621] The wavelength at 400 cm was measured using a Fourier transform far-infrared spectrometer (manufactured by JASCO Corporation, model: VIR-F4000) by the following method (terahertz measurement). -1 ~450cm -1 The absorption coefficient is within the range of .
[0622] First, polyethylene powder was formed into a sheet using a heated automatic press (manufactured by Shinto Metal Industries, Ltd., model: SFA-37H) and a cooled manual press (manufactured by Oji Machinery Co., Ltd., model: J-37) under the <pressing conditions> shown below.
[0623] <Pressure conditions>
[0624] (1) 8 g of polyethylene powder was filled into a mold of 50 mm×50 mm×2 mm in thickness.
[0625] (2) Using a heated automatic press set at 210°C, the mold was pressed at 5 kg / cm 2 Preheat for 5 minutes at 15 kg / cm 2Press down for 25 minutes.
[0626] (3) Using a room temperature cooled manual press, press at 10 kg / cm 2 The mold was cooled for 10 minutes to obtain a sheet.
[0627] Next, the obtained sheet was punched into a disk with a diameter of 20 mm to obtain a measurement sample. The measurement sample was measured under the following <Terahertz measurement conditions> using a Fourier transform far-infrared spectrometer (manufactured by JASCO Corporation, model: VIR-F4000).
[0628] <Terahertz measurement conditions>
[0629] Wavelength range: 50cm -1 ~600cm -1
[0630] Measurement environment: In the atmosphere, room temperature (25°C)
[0631] Light source: Ceramic
[0632] Beam diameter: about 8mm to about 9mm
[0633] Bracket aperture: 10mm
[0634] In addition, based on the incident light intensity I obtained under the above measurement conditions 0 and the transmitted light intensity I, the absorption coefficient at each wave number is calculated according to the following (Formula K), and the 400cm -1 ~450cm -1 The absorption coefficient is within the range of .
[0635] α=-log 10 (I 0 / I) / 0.4343x……(Formula K)
[0636] α: Absorption coefficient [cm -1 ]
[0637] I 0 : The intensity of the electromagnetic wave before incident
[0638] I: The intensity of the electromagnetic wave after incident (transmitted light intensity)
[0639] x: sample thickness [cm]
[0640] ( 1 H-NMR measurement)
[0641] It was determined by the method shown below using a nuclear magnetic resonance apparatus (manufactured by Bruker Corporation / product name: AvanceNEO600).
[0642] First, measurement was performed under the following <NMR measurement conditions>.
[0643] <NMR measurement conditions>
[0644] Observation core: 1 H
[0645] Observation frequency: 600MHz
[0646] Pulse program: zg30
[0647] Pulse waiting time: 1 second
[0648] Cumulative times: 1024 times
[0649] Measuring temperature: 130℃
[0650] Chemical shift standard: 7.219ppm (o-DCBz)
[0651] Sample concentration: 1% by weight
[0652] Sample tube: 5mmφ
[0653] Next, the obtained data were checked for the presence or absence of signals (peaks) in two regions: (1) 4.8 ppm to 5.0 ppm and (2) 5.6 ppm to 6.0 ppm.
[0654] (aluminum content and silicon content)
[0655] The element content of the polyethylene powder was determined by high frequency plasma mass spectrometry according to JIS K0133. The sample was prepared by pressurized acid hydrolysis using nitric acid using a microwave decomposition device (model ETHOSTC, manufactured by Milestone General Co., Ltd.). For the prepared sample, the aluminum content and silicon content in the polyethylene powder were quantified by the internal standard method using ICP-MS (inductively coupled plasma mass spectrometer, model X series X7, manufactured by Thermo Fisher Scientific).
[0656] (Temperature of the peak in the DSC curve of the second heating process)
[0657] In the DSC measurement when the above-mentioned (difference between the temperature of the peak top in the DSC curve in the second heating process and the temperature of the peak convergence point) is obtained, the temperature of the peak top in the DSC curve in the second heating process (Tm2 top ).
[0658] (density)
[0659] The density of the polyethylene powder was determined by the following methods (1) to (7).
[0660] (1) Polyethylene powder is filled into a mold of 100 mm×100 mm×2 mm thick.
[0661] (2) Using a press set at 190°C, at 10 kg / cm 2 Preheat the mold for 3 minutes, perform 3 degassing operations, and 2 Press down for 2 minutes.
[0662] (3) The mold is cooled to room temperature by cooling and pressing to obtain a pressed tablet.
[0663] (4) Slices of 20 mm×20 mm×2 mm in thickness were cut out from the obtained pressed sheet.
[0664] (5) The cut sections were placed in a test tube and heated at 120° C. for 1 hour in a nitrogen atmosphere.
[0665] (6) After heating, the slices were cooled at 20° C. for 1 hour to obtain a molded body sample for density measurement.
[0666] (7) The density of the molded product sample was measured according to JIS K7112:1999 (D method), and the obtained value was taken as the density of the polyethylene powder (kg / m 3 ).
[0667] (Content (mol) of central metal M contained in transition metal compound component [B-1] and / or transition metal compound component [B-2] in the catalyst component and molar ratio (Al / M) of the content (mol) of central metal M to the content (mol) of Al)
[0668] The element contents in the catalyst components were measured using a microwave plasma atomic emission spectrometer (manufactured by Agilent, model: 4210MP-AES / G8007A).
[0669] First, an acid hydrolysis solution of the catalyst component was prepared based on the <decomposition conditions> shown below.
[0670] <Decomposition conditions>
[0671] (1) Under a nitrogen atmosphere, 100 mg to 500 mg of the catalyst component is weighed into a pressure-resistant container.
[0672] (2) Add 10 mL of sulfuric acid (1+1) to the pressure-resistant container of (1), and stir for more than 1 hour.
[0673] (3) The aqueous solution obtained in (2) was adjusted to 100 mL.
[0674] (4) 2 mL to 20 mL of the aqueous solution obtained in (3) was taken and further fixed to 100 mL. The amount of the aliquot was appropriately adjusted according to the amount of luminescence in the measurement described below.
[0675] Next, for the obtained acid hydrolysis solution, based on the <MP-AES measurement conditions> shown below, a microwave plasma atomic emission spectrometer (manufactured by Agilent, model: 4210MP-AES / G8007A) is used to quantify the content (molar) of the central metal M and the content (molar) of Al contained in the transition metal compound component [B-1] and / or the transition metal compound component [B-2] in the catalyst component by the external standard method, and their molar ratio (Al / M) is calculated.
[0676] <MP-AES measurement conditions>
[0677] Standard solution for device calibration: ICP-OES & MP-AES Wavecal: Al, As, Ba, Cd, Co, Cr, Cu, Mn, Mo, Ni, Pb, Se, Sr, Zn (5 mg / L); K (50 mg / L) dissolved in 5% HNO 3 middle
[0678] Background correction: Automatic
[0679] Reading time: 3 seconds
[0680] Observation location: 0
[0681] Atomizer flow rate: M (0.5L / min~1.0L / min), Al (0.95L / min)
[0682] Repeated number of measurements: 3
[0683] Pump speed: 15 rpm
[0684] Introduction time: 15 seconds
[0685] Stabilization time: 15 seconds
[0686] Number of pixels: 3
[0687] Standard solution for calibration curve preparation: Standard solution for atomic absorption analysis corresponding to each element (manufactured by Kanto Chemical Co., Ltd.)
[0688] Calibration curve concentration: 8 points: 0.5mg / L, 1mg / L, 2mg / L, 5mg / L, 10mg / L, 20mg / L, 50mg / L, 100mg / L
[0689] [Production of microporous membrane and evaluation of its properties]
[0690] (Method for producing microporous membrane)
[0691] First, in a resin container, 12 g of the polyethylene powder of each example and comparative example, 0.4 g of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (product name: Adecastab AO-60G) manufactured by ADEKA Corporation as an antioxidant, and 28 g of liquid paraffin (product name: P-350P) manufactured by MORESCO Co., Ltd. were thoroughly mixed to obtain a mixture.
[0692] Next, the mixture was placed in a LaboPlastomill mixer (main body model: 30C150, mixer model: R-60) manufactured by Toyo Seiki Co., Ltd., set at a temperature of 200° C., and kneaded for 10 minutes at a rotation speed of 5 rpm, and then further kneaded for 10 minutes at a rotation speed of 50 rpm, thereby obtaining a polyethylene gel. The gel was formed into a sheet based on the <Gel Sheet Preparation Conditions> shown below.
[0693] <Gel sheet production conditions>
[0694] (1) The polyethylene gel is filled into a mold of 200 mm x 200 mm x 1 mm thick.
[0695] (2) Using a press machine with a set temperature of 180°C, the mold was heated to 1 kg / cm 2 Preheat for 3 minutes at 10 kg / cm 2 Press down for 2 minutes.
[0696] (3) Using a room temperature cooling press, at 10 kg / cm 2 The mold was cooled for 10 minutes to obtain a gel sheet.
[0697] The gel sheet thus obtained was stretched to 7×7 times at 115° C. (when the viscosity average molecular weight of polyethylene is greater than or equal to 100,000 and less than 2.5 million) or 120° C. (when the viscosity average molecular weight of polyethylene is greater than or equal to 2.5 million and less than 4 million) using a synchronous biaxial stretching machine to obtain a stretched film. Then, the stretched film was immersed in n-hexane for 20 minutes twice to extract and remove the liquid paraffin, and then air-dried. Then, it was heat-set at 125° C. for 3 minutes to obtain a microporous membrane.
[0698] The stretching temperature and the heat setting temperature were appropriately adjusted for each microporous membrane within a specified temperature range.
[0699] (Evaluation of Heat Resistance of Microporous Film)
[0700] As an evaluation index of heat resistance, the heat shrinkage rate of the microporous film at high temperature was evaluated.
[0701] Specifically, eight films of 100 mm×50 mm were punched out from a 250 mm×250 mm microporous membrane obtained by the above-mentioned [Microporous membrane production method] and allowed to stand in an oven set at 140° C. for 60 minutes.
[0702] After being heated and allowed to stand, the film was cooled at room temperature for 15 minutes, and then the size of the microporous film was measured and the heat shrinkage (%) was calculated by the following formula.
[0703] Then, the average value of the measured values at a total of 8 points was calculated, and the heat resistance was evaluated according to the following evaluation criteria.
[0704] (Thermal shrinkage ratio) = ((Thermal shrinkage ratio in the long side direction) + (Thermal shrinkage ratio in the short side direction)) / 2
[0705] (Thermal shrinkage in the long side direction) = (1-D 长边140 / D 长边23 )×100
[0706] (Thermal shrinkage in the short side direction) = (1-D 短边140 / D 短边23 )×100
[0707] D 长边140 :Dimensions in the long side direction at 140°C [mm]
[0708] D 长边23 :Dimensions in the long side direction at 23°C [mm]
[0709] D 短边140 :Short side dimension at 140℃[mm]
[0710] D 短边23 :Short side dimension at 23℃[mm]
[0711] (Evaluation Criteria)
[0712] ◎(Good): Less than 40%
[0713] ○(Normal): 40% or more and less than 50%
[0714] × (poor): more than 50%
[0715] (Evaluation of Uniformity of Microporous Film)
[0716] As an evaluation index of uniformity, the uniformity of the thickness of the microporous membrane was evaluated.
[0717] The microporous membrane obtained by the above-mentioned [Method for producing microporous membrane] was punched out from 250 mm × 250 mm into 8 sheets of 100 mm × 50 mm, and the film thickness of each sheet was measured at 23° C. using a micro thickness gauge (model: KBM) manufactured by Toyo Seiki Seisaku-sho Co., Ltd. The film thickness was measured at 3 locations on one punched film.
[0718] Then, the standard deviation of the measured values at a total of 24 points was calculated, and the uniformity was evaluated according to the following evaluation criteria.
[0719] (Evaluation Criteria)
[0720] ◎(Good): Less than 0.5μm
[0721] ○(Normal): 0.5μm or more and less than 1μm
[0722] ×(bad): 1μm or more
[0723] (Evaluation of Dimensional Stability of Microporous Membranes)
[0724] As an evaluation index of dimensional stability, the heat shrinkage of the microporous membrane was evaluated.
[0725] Specifically, eight films of 100 mm×50 mm were punched out from a 250 mm×250 mm microporous membrane obtained by the above-mentioned [Microporous membrane production method] and allowed to stand in an oven set at 120° C. for 60 minutes.
[0726] After being heated and allowed to stand, the film was cooled at room temperature for 15 minutes, and then the size of the microporous film was measured and the heat shrinkage (%) was calculated by the following formula.
[0727] Then, the average value of the measured values at a total of 8 points was calculated, and the dimensional stability was evaluated according to the following evaluation criteria.
[0728] (Thermal shrinkage ratio) = ((Thermal shrinkage ratio in the long side direction) + (Thermal shrinkage ratio in the short side direction)) / 2
[0729] (Thermal shrinkage in the long side direction) = (1-D 长边120 / D 长边23 )×100
[0730] (Thermal shrinkage in the short side direction) = (1-D 短边120 / D 短边23 )×100
[0731] D 长边120 :Dimensions in the long side direction at 120°C [mm]
[0732] D 长边23 :Dimensions in the long side direction at 23°C [mm]
[0733] D 短边120 :Short side dimension at 120℃[mm]
[0734] D 短边23 :Short side dimension at 23℃[mm]
[0735] (Evaluation Criteria)
[0736] ◎(Good): Less than 10%
[0737] ○(Normal): 10% or more and less than 20%
[0738] × (difference): more than 20%
[0739] (Evaluation of the heat resistance improvement rate of microporous membrane)
[0740] The microporous membrane obtained by using 12g of high-density polyethylene "SH800" (trademark, manufactured by Asahi Kasei Corporation) with a viscosity average molecular weight (Mv) of 300,000 instead of 12g of polyethylene powder of each embodiment and comparative example in the above (method for manufacturing microporous membrane), and the microporous membrane obtained by using 8.4g of high-density polyethylene "SH800" (trademark, manufactured by Asahi Kasei Corporation) with a viscosity average molecular weight (Mv) of 300,000 instead of 12g of polyethylene powder of each embodiment and comparative example in the above (method for manufacturing microporous membrane) were evaluated by the method described in the above (evaluation of heat resistance of microporous membrane). Then, the high heat resistance rate was evaluated according to the following evaluation criteria.
[0741] (High heat resistance rate) = (1-S 添加后 / S 添加前 )×100
[0742] S 添加后 : Thermal shrinkage of the microporous membranes to which the polyethylene powders of the examples and comparative examples were added [%]
[0743] S 添加前 :Heat shrinkage of microporous film using only high-density polyethylene "SH800" [%]
[0744] (Evaluation Criteria)
[0745] ◎(Good): 20% or more
[0746] ○(Normal): 10% or more and less than 20%
[0747] ×(Bad): Less than 10%
[0748] [Preparation of catalyst component]
[0749] (Preparation of Inorganic Solid Particles [A]: (a-1) to (a-3))
[0750] Inorganic solid particles (a-1) to (a-3) were prepared according to the following (1) to (2).
[0751] (Preparation of Inorganic Solid Particles (a-1))
[0752] <(1) Synthesis of organomagnesium compound (A-1)>
[0753] 1 mol / L Mg was added to an 8 L stainless steel autoclave that was fully purged with nitrogen. 6 (C 4 H 9 ) 12 Al(C 2 H 5 ) 3 2000mL of hexane solution (equivalent to 2000 mmol in terms of magnesium and aluminum) was added to the autoclave, and 146mL of 5.47 mol / L n-butanol hexane solution was added dropwise from the feed line connected to the autoclave for 3 hours while stirring at 50°C. After the reaction was completed, 300mL of hexane was used to clean the line. Then, stirring was continued at 50°C for 2 hours. After the reaction was completed, the reaction product cooled to room temperature was used as raw material (A-1). Raw material (A-1) is an organic magnesium compound with a magnesium concentration of 0.704 mol / L.
[0754] <(2) Synthesis of Inorganic Solid Particles (a-1)>
[0755] 1000 mL of a 1 mol / L hexane solution of trichlorosilane was added to an 8L stainless steel autoclave fully purged with nitrogen, and 1340 mL of a hexane solution of an organic magnesium compound of the raw material (A-1) (equivalent to 943 mmoles of magnesium) was added dropwise at 65° C. for 3 hours, and the reaction was continued while stirring at 65° C. for 1 hour. After the reaction was completed, the supernatant was removed and washed 4 times with 1800 mL of hexane to obtain inorganic solid particles (a-1) (magnesium chloride particles). The particles were analyzed, and the magnesium contained in 1 g of the solid was 7.5 mmoles.
[0756] (Preparation of Inorganic Solid Particles (a-2))
[0757] 130 g of heat-treated silica (Fuji Silysia Co., Ltd. / product name: Q-6) and 2500 mL of hexane were added to an 8 L stainless steel autoclave fully purged with nitrogen to obtain a slurry. While the obtained slurry was maintained at 20° C. under stirring, 260 mL of 1 mol / L methylaluminoxane (toluene solution, manufactured by Tosoh Fine Chemicals Co., Ltd.) was added, and the reaction was continued while stirring for 2 hours. After the reaction was completed, the supernatant was removed and washed 4 times with 1800 mL of hexane to obtain inorganic solid particles (a-2).
[0758] (Preparation of Inorganic Solid Particles (a-3))
[0759] 10g of silica (Grace Davision / product name: Sylopol 952) and 100mL of toluene after heat treatment were added to a 300mL glass container fully substituted with nitrogen to obtain a slurry. While the obtained slurry was maintained at 80°C under stirring, 90mL of 1 mol / L of methylaluminoxane (toluene solution, manufactured by Tosoh Fine Chemicals Co., Ltd.) was added and then stirred for 1 hour. After stirring, the container temperature was cooled to room temperature, 40mL of 1 mol / L of methylaluminoxane (toluene solution, manufactured by Tosoh Fine Chemicals Co., Ltd.) was added, and then the reaction was continued while stirring for 1 hour. After the reaction was completed, the supernatant was removed and washed 4 times with 100mL of toluene to obtain inorganic solid particles (a-3).
[0760] (Preparation of transition metal compound component [B-2]: (b-1))
[0761] In a 3L glass container fully purged with nitrogen, 200 mmol of [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]titanium-1,3-pentadiene was dissolved in 1000 mL of Isopar E [manufactured by Exxon Chemical Co.], and 40 mL of 1 mol / L ethylbutylmagnesium (hexane solution) was added. Hexane was further added to adjust the titanium complex concentration to 0.08 mol / L, thereby obtaining a transition metal compound component (b-1).
[0762] (Preparation of Activating Agent [C]: (c-1))
[0763] In a 500 mL glass container fully purged with nitrogen, 17.8 g of tris(pentafluorophenyl)(4-hydroxyphenyl) boronate bis(hydrogenated tallow alkyl)methylammonium was added to 156 ml of toluene and dissolved, thereby obtaining a 100 mM toluene solution of the boride. While the toluene solution of the boride was maintained at 25° C., 15.6 mL of 1 mol / L ethoxydiethylaluminum (hexane solution) was added, and hexane was further added to adjust the boride concentration in the toluene solution to 0.08 mol / L. Then, the mixture was stirred at 25° C. for 1 hour, thereby preparing an activator (c-1).
[0764] (Synthesis of organometallic compound component [D]: (d-1))
[0765] 2000 mL of 1 mol / L Mg was placed in an 8 L stainless steel autoclave that was fully purged with nitrogen. 6 (C 4 H 9 ) 12 Al(C 2 H 5 ) 3 The mixture was stirred at 80°C for 2 hours while pressure feeding 240 mL of a hexane solution of 8.33 mol / L methyl hydrogen polysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.). After the reaction was completed, the reaction product was cooled to room temperature and used as an organometallic compound component (d-1). The organometallic compound component (d-1) had a total concentration of 0.786 mol / L of magnesium and aluminum.
[0766] (Example 1)
[0767] (Preparation of Catalyst Component (A))
[0768] In a 50 mL glass container fully purged with nitrogen, 0.0011 mmol of bis(pentamethylcyclopentadienyl)titanium dichloride (Cp * 2 TiCl 2 ) was dissolved in 3 mL of toluene, 1.42 mol / L of modified methylaluminoxane (MMAO, hexane solution, manufactured by Tosoh Fine Chemicals Co., Ltd.) was added, and the mixture was reacted at 25°C for 1 hour to obtain an active material (A1).
[0769] Next, while 10mL of hexane slurry containing 0.44g of the above-mentioned inorganic solid particles (a-1) was maintained at 25°C, the solution of the above-mentioned active material (A1) was added in full amount and reacted for 1 hour. After the reaction was completed, the supernatant was removed and washed 4 times with hexane to remove the unreacted raw material components. It should be noted that, through this reaction, a layer of the above-mentioned active material (A1) was formed on the surface of the above-mentioned inorganic solid particles (a-1). Then, 1.4mL of the above-mentioned transition metal compound component (b-1) and 1.4mL of the activator (c-1) were added simultaneously and reacted for 2 hours. After the reaction was completed, the supernatant was removed and washed 4 times with hexane to remove the unreacted raw material components, thereby obtaining the catalyst component (A). It should be noted that, as described above, by loading the above-mentioned transition metal compound component (b-1) and the activator (c-1) (multi-stage loading) after the loading of the above-mentioned active material (A1), a double-layer structure was formed on the surface of the above-mentioned inorganic solid particles (a-1).
[0770] (Examples 2 to 9, Comparative Examples 2, 5, and 6)
[0771] (Preparation of Catalyst Components (B) to (H), (J), (M), (N), and (E'))
[0772] Catalyst components (B) to (H), (J), (M), (N), and (E') were prepared in the same manner as in the preparation of the catalyst component (A), except that the catalyst synthesis conditions were changed as shown in Tables 1 and 2.
[0773] (Example 10)
[0774] (Preparation of Catalyst Component (O))
[0775] Catalyst component (O) was prepared in the same manner as in the preparation of catalyst component (A), except that the catalyst synthesis conditions were changed as shown in Table 1 and the reaction temperature in the premixing step for obtaining the active material (A1) was adjusted to 90°C.
[0776] (Comparative Example 1)
[0777] (Preparation of Catalyst Component (I))
[0778] In a 50 mL glass container fully purged with nitrogen, 10 mL of toluene slurry containing 1 g of the inorganic solid particles (a-3) was maintained at 40° C., and 0.1 mmol of bis(n-butylcyclopentadienyl)zirconium dichloride (nBuCp 2 ZrCl 2) and react for 1 hour. Then, 0.1 mmol of [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]dichlorotitanium (b-2) pre-dissolved in toluene was added and reacted for 1 hour. Finally, 0.2 mmol of tetrakis(pentafluorophenyl)boron N,N'-dimethylanilinium (c-2) pre-dissolved in toluene was added and reacted for 1 hour. After the reaction was completed, the supernatant was removed and washed 4 times with toluene to remove the unreacted raw material components. Then, toluene was removed by vacuum drying to prepare catalyst component (I).
[0779] (Comparative Example 3)
[0780] (Preparation of Catalyst Component (K))
[0781] While stirring at 10° C., 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of an organic metal compound component (d-1) were added simultaneously to 1970 mL of a hexane slurry containing 110 g of the inorganic solid particles (a-1) over 3 hours. After the addition, the reaction was continued at 10° C. for 1 hour. After the reaction was completed, the supernatant was removed and washed 4 times with hexane to remove unreacted raw material components, thereby preparing a catalyst component (K).
[0782] (Comparative Example 4)
[0783] (Preparation of Catalyst Component (L))
[0784] 1600 mL of hexane was added to an 8L stainless steel autoclave fully purged with nitrogen. While stirring at 40°C, 800 mL of a 1 mol / L hexane solution of titanium tetrachloride and 1017 mL of an organometallic compound component (d-1) were added simultaneously over 2 hours. After the addition, the temperature was slowly raised and the reaction was continued at 40°C for 1 hour. After the reaction was completed, 1600 mL of the supernatant was removed and washed 4 times with 1600 mL of hexane to prepare a catalyst component (L).
[0785]
[0786]
[0787] It should be noted that in Tables 1 and 2, a-1 to a-3 represent the inorganic solid particles (a-1) to (a-3) prepared above, b-1 represents the transition metal compound component (b-1) prepared above, b-2 represents [(N-tert-butylamino)(tetramethyl-η5-cyclopentadienyl)dimethylsilane]titanium dichloride, c-1 represents the activator (c-1) prepared above, c-2 represents N,N'-dimethylanilinium tetrakis(pentafluorophenyl)boride, d-1 represents the organic metal compound component (d-1) synthesized above, Cp * 2 TiCl 2 represents bis(pentamethylcyclopentadienyl)titanium dichloride, Cp 2 TiCl 2 stands for bis(cyclopentadienyl)titanium dichloride, nBuCp 2 ZrCl 2 represents bis(n-butylcyclopentadienyl)zirconium dichloride, Cp * 2 ZrCl 2 stands for bis(pentamethylcyclopentadienyl)zirconium dichloride, TiCl 4 Represents titanium tetrachloride, Ti(OBu) 4 Tetrabutoxytitanium (IV) (monomer), EtAlCL 2 stands for ethylaluminum dichloride, Et 2 AlCl represents diethylaluminum chloride, MMAO represents modified methylaluminoxane, and MAO represents methylaluminoxane.
[0788] [Manufacturing of polyethylene powder and microporous membrane]
[0789] (Example 11)
[0790] <Polymerization of polyethylene powder (A)>
[0791] Polymerization of polyethylene powder was carried out by the method described below using a 1.5 L stainless steel autoclave polymerization reactor which was fully purged with nitrogen.
[0792] First, 800mL of hexane as a solvent was put into a polymerization reactor heated to 60°C, and 0.4 mmol of an organic metal compound component (d-1) as an impurity capture agent was added. Then, ethylene was added so that the internal pressure reached 0.65MPa, and 1.25 micromoles of the above-mentioned catalyst component (A) was added in terms of Ti. In addition, 0.5mL of hydrogen was added for every 1L of ethylene consumption. While maintaining the internal pressure at 0.65MPa and the internal temperature at 60°C, polymerization was carried out for 30 minutes while stirring at a stirring speed of 1200rpm. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated using methanol. Then, the reaction mixture was filtered, washed, and air-dried to obtain polyethylene powder (A). The polymerization activity in the polymerization reactor was 3500g per 1g of catalyst.
[0793] Table 5 shows the results of the various evaluations performed on the polyethylene powder (A) and the microporous membrane of the polyethylene powder (A) produced by the above-mentioned [Method for producing microporous membrane].
[0794] (Examples 12 to 20 and Comparative Examples 7, 8, 11, 12)
[0795] Polyethylene powder and microporous membrane thereof were produced in the same manner as in Example 11, except that the polymerization conditions were changed as shown in Tables 3 and 4, and the above-mentioned various evaluations were performed. The results are shown in Tables 5 and 6. It should be noted that in Example 15 and Comparative Example 12, 0.05 mol% of 1-butene as a comonomer was copolymerized.
[0796] (Comparative Example 9)
[0797] Hexane, ethylene, hydrogen, and catalyst are continuously supplied to a 300L container-type polymerization reactor without baffles and with full-area stirring blades. The polymerization ethylene partial pressure is adjusted to 0.5MPa. The polymerization temperature is maintained at 75°C by jacket cooling. Hexane is supplied from the bottom of the polymerization reactor at 40L / hour, and the average residence time is 3 hours. Before the catalyst is supplied to the polymerization reactor, 2 mmoles of 1M ethylaluminum dichloride are added and mixed with respect to 1g of the catalyst component (K), and then the supernatant is decanted and replaced with hexane. After this pretreatment is performed 3 times, it is used as a catalyst. With respect to 1g of the pretreated catalyst component (K), 20 mmoles of triisobutylaluminum as an impurity capture agent are mixed in a buffer tank before the polymerization supply. The mixed catalyst component (K) is added to the polymerization reactor at a rate of 0.2g / hour. Ethylene and hydrogen are introduced into the gas phase, and hydrogen is continuously supplied by a pump in a manner that the hydrogen concentration relative to the ethylene in the gas phase is 5 mol%. In addition, the stirring speed was set to 230 rpm.
[0798] The liquid was continuously extracted into a flash tank at a pressure of 0.05 MPa and a temperature of 70° C. so that the liquid level in the polymerization reactor was kept constant, and unreacted ethylene and hydrogen were separated.
[0799] Next, the polymerized slurry is continuously transferred to a centrifugal separator so that the liquid level in the polymerization reactor is kept constant, and the polyethylene powder and other components such as the solvent are separated.
[0800] The separated polyethylene powder was dried while blowing nitrogen at 78°C. It should be noted that in the drying process, the catalyst and the co-catalyst were deactivated by spraying steam on the polymerized powder. 1000 ppm of calcium stearate (manufactured by Dainichi Chemical Co., Ltd., C60) was added to the obtained polyethylene powder and mixed evenly using a Henschel mixer. The polyethylene powder that did not pass through the sieve was removed from the obtained polyethylene powder using a sieve with a mesh size of 425 μm, thereby obtaining a polyethylene powder (K). The polymerization activity in the polymerization reactor was 20,000 g per 1 g of catalyst.
[0801] Table 6 shows the results of the various evaluations performed on the polyethylene powder (K) and the microporous membrane of the polyethylene powder (K) produced by the above-mentioned [Method for producing microporous membrane].
[0802] (Comparative Example 10)
[0803] Hexane, ethylene, hydrogen and catalyst are continuously supplied to a container-type 300L polymerization reactor with a stirring device. The polymerization pressure is 0.35MPa. The polymerization temperature is maintained at 75°C by jacket cooling. Hexane is supplied from the bottom of the polymerization vessel at 40L / hour, and the average residence time is 3 hours. Catalyst component (L) is used as the catalyst, and triisobutylaluminum is used as an impurity capture agent. Triisobutylaluminum is added to the polymerization vessel at a rate of 10 mmol / hour. Catalyst component (L) is supplied at a rate of 0.2g / hour. Hydrogen is continuously supplied by a pump in a gas phase concentration of 2000ppm. The stirring speed is set to 230rpm. A 100 mmol / L hexane solution of n-butanol is supplied in a manner that the amount of n-butanol is 1ppm / hour relative to the polymerization speed (manufacturing speed) of 10kg / hour, thereby obtaining a polymerization slurry. The obtained polymerization slurry was conveyed to a centrifuge to separate the polyethylene powder from the solvent and the like other than the polyethylene powder, and then the polyethylene powder and 60° C. methanol were stirred and contacted for 1 hour. The polymerization slurry containing the polyethylene powder and methanol was conveyed to a centrifuge to separate the polyethylene powder from the solvent and the like other than the polyethylene powder. The separated polyethylene powder was dried while blowing nitrogen at 70° C. The polyethylene powder that did not pass through the sieve was removed from the polyethylene powder thus obtained using a sieve with a mesh size of 425 μm, thereby obtaining polyethylene powder (L). The polymerization activity in the polymerization reactor was 30,000 g per 1 g of the catalyst.
[0804] Table 6 shows the results of the various evaluations performed on the polyethylene powder (L) and the microporous membrane of the polyethylene powder (L) produced by the above-mentioned [Method for producing microporous membrane].
[0805]
[0806]
[0807] It should be noted that in Tables 3 and 4, d-1 represents the above-synthesized organometallic compound component (d-1), Et 3 Al represents triethylaluminum, iBu 3 Al represents triisobutylaluminum.
[0808]
[0809]
[0810] This application is based on Japanese patent application (Japanese Patent Application No. 2022-059266) filed on March 31, 2022, and its contents are incorporated herein by reference.
[0811] Industrial Applicability
[0812] The polyethylene powder of the present invention is excellent in heat resistance, film uniformity, dimensional stability and high heat resistance rate when it is made into a microporous film, and has industrial applicability.
Claims
1. A polyethylene powder, wherein: The viscosity average molecular weight of the polyethylene powder is 100,000 or more and 4,000,000 or less, The crystal thickness parameter of the polyethylene powder measured using a differential scanning calorimeter (DSC) is 5° C. or more and 9° C. or less.
2. The polyethylene powder according to claim 1, wherein The z-average shrinkage factor g of the polyethylene powder measured by a gel permeation chromatography (GPC) measuring device combined with a differential refractometer and a viscosity detector is z The value of is greater than or equal to 0.600 and less than or equal to 1.
3. The polyethylene powder according to claim 1, wherein In the DSC curve of the second heating process of the polyethylene powder obtained by the measurement shown in the following <Measurement Conditions> using a differential scanning calorimeter (DSC), the peak temperature (Tm2 top ) is 135° C. or higher and 140° C. or lower, and the crystal thickness parameter is 6.7° C. or higher and 9.0° C. or lower, <Measurement conditions> (1) Stand at 50°C for 1 minute (2) Heating from 50°C to 180°C at 10°C / min (first heating process) (3) Stand at 180°C for 5 minutes (4) Cooling from 180°C to 50°C at 10°C / min (5) Stand at 50°C for 5 minutes (6) The temperature was raised from 50°C to 180°C at a rate of 10°C / min (second heating process).
4. The polyethylene powder according to claim 2 or 3, wherein The polyethylene powder can be stretched under the following conditions: (Stretching conditions) A gel sheet of 100 mm×100 mm×1 mm in thickness containing 30% by mass of polyethylene powder and 70% by mass of liquid paraffin was stretched to 7×7 times at 115°C.
5. The polyethylene powder according to claim 2 or 3, wherein In the terahertz measurement, the 400 cm -1 ~450cm -1 The absorption coefficient within the range of is greater than or equal to 1.0 and less than or equal to 4.
0.
6. The polyethylene powder according to claim 2 or 3, wherein: In the polyethylene powder 1 In the H-NMR measurement, there is no peak in the region shown below, (1) 4.8ppm~5.0ppm (2)5.6ppm~6.0ppm.
7. The polyethylene powder according to claim 2 or 3, wherein: The aluminum content in the polyethylene powder is 0 ppm or more and 50 ppm or less.
8. The polyethylene powder according to claim 2 or 3, wherein: The silicon content in the polyethylene powder is 0 ppm or more and 30 ppm or less.
9. The polyethylene powder according to claim 2, wherein: In differential scanning calorimetry (DSC) of the polyethylene powder, the temperature of the peak top in the DSC curve in the second temperature increase process is 130° C. or higher and 140° C. or lower.
10. The polyethylene powder according to claim 2 or 3, wherein: The density of the polyethylene powder is 920 kg / m 3 Above and 960kg / m 3 the following.
11. The polyethylene powder according to claim 2 or 3, wherein: The polyethylene powder is used for battery separators.
12. A method for producing a catalyst for olefin polymerization, wherein: The method for producing the olefin polymerization catalyst comprises the following steps: A first supporting reaction step, wherein the inorganic solid particles [A] are reacted with the transition metal compound [B-1] and / or the transition metal compound component [B-2], the activator [C] and / or the organometallic compound component [D]; and A second supporting reaction step, wherein the particles obtained in the first supporting reaction step are reacted with a transition metal compound component [B-1] and / or a transition metal compound component [B-2], an activator [C] and / or an organometallic compound component [D], The transition metal compound [B-1] is a compound represented by the following (Formula 3), the transition metal compound [B-2] is a compound represented by the following (Formula 4), the activator [C] is a compound represented by the following (Formula 5) or (Formula 6), the organometallic compound component [D] is a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, the inorganic solid particles [A] are porous polymer materials or inorganic solid particles containing at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table, The method for producing an olefin polymerization catalyst satisfies the following <Condition 1> and / or <Condition 2>, <Condition 1> The first loading reaction step includes the following steps: a premixing step of reacting the transition metal compound [B-1] and / or the transition metal compound component [B-2] with the activator [C] and / or the organometallic compound component [D]; and a step of reacting the inorganic solid particles [A] with the mixture obtained in the premixing step, <Condition 2> In the first supporting reaction step, the molar ratio (([C]+[D]) / [B]) of the molar amount ([C]+[D]) of the activator [C] and the organometallic compound component [D] to the molar amount [B] of the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is 1 or more and 60 or less, L 1 j W k M 1 X 1 p X 2 q ……(Formula 3) (In Formula 3, L 1 each independently represents an n-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group and an octahydrofluorenyl group, wherein the ligand has 1 to 8 substituents as the case may be, and the substituents are each independently selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogenated hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms and a halogenated silyl group and having 20 or less non-hydrogen atoms, M 1 represents a transition metal selected from the group of transition metals belonging to Group 4 of the Periodic Table of the Elements having a formal oxidation number of +2, +3 or +4 and having an η5 bond with at least one ligand L, W represents a divalent substituent having 50 or less non-hydrogen atoms and bonding to each of L and M with a univalent valency to form a metal ring compound together with L and M, X 1 each independently represents an anionic sigma-bonded ligand having 60 or less non-hydrogen atoms selected from the group consisting of a monovalent anionic sigma-bonded ligand, a divalent anionic sigma-bonded ligand divalently bonded to M, and a divalent anionic sigma-bonded ligand monovalently bonded to each of L and M, X 2 each independently represents a neutral Lewis base coordinating compound having 40 or less non-hydrogen atoms, j is 1 or 2, wherein when j is 2, the two ligands L are bonded to each other through a divalent group having 20 or less non-hydrogen atoms, the divalent group being a group selected from the group consisting of a hydrocarbon diyl group having 1 to 20 carbon atoms, a halogenated hydrocarbon diyl group having 1 to 12 carbon atoms, an alkyleneoxy group having 1 to 12 carbon atoms, an alkyleneamino group having 1 to 12 carbon atoms, a silanediyl group, a halogenated silanediyl group, and a silyleneamino group, k is 0 or 1, p is 0, 1 or 2, wherein in X 1 In the case of a monovalent anionic σ-bonding type ligand or a divalent anionic σ-bonding type ligand bonded to L and M, p is an integer smaller than the formal oxidation number of M by 1 or more, and in the case of X 1 In the case of a divalent anionic σ-bonded ligand that is bonded only to M, p is an integer that is (j+1) or more smaller than the formal oxidation number of M, and q is 0, 1 or 2); (In Formula 4, M 2 represents a transition metal selected from the group consisting of titanium, zirconium and hafnium and having a formal oxidation number of +2, +3 or +4, R 5 Each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein in the substituent R 5 When it is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group or a germyl group, two adjacent substituents R 5 bonded to each other to form a divalent group, thereby bonding to the two adjacent substituents R 5 The bonds between the two carbon atoms of the cyclopentadienyl ring to which each is bonded together form a ring, X 3 Each independently represents a substituent selected from the group consisting of a halogen ion, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbonoxy group having 1 to 18 carbon atoms, a hydrocarbonamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbonamide group having 1 to 18 carbon atoms, a hydrocarbonphosphine group having 1 to 18 carbon atoms, a hydrocarbonthio group having 1 to 18 carbon atoms, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein two substituents X may be selected from the group consisting of 3 Together they form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms, Y 1 Indicates -O-, -S-, -NR 6 -or-PR 6 -, where R 6 represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbonoxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof, Z 1 represents SiR 6 2. CR 6 2. SiR 6 2SiR 6 2. CR 6 2CR 6 2. CR 6 =CR 6 . CR 6 2SiR 6 2 or GeR 6 2, where R 6 As defined above, n is 1, 2 or 3); (C-1): [L 2 -H] d+ [M 3 r Q s ] d- ……(Formula 5) (In Formula 5, [L 2 -H] d+ For proton-donating Bronsted acids, L 2 is a neutral Lewis base; in addition, in Formula 5, [M 3 r Q s ] d- is a compatible non-coordinating anion, M 3 is a metal or metalloid selected from Groups 5 to 15 of the periodic table, Q is independently a hydride ion, a dialkylamino group, a halide ion, an alkoxy group, an allyloxy group, a hydrocarbon group, or a substituted hydrocarbon group having 20 or less carbon atoms, and the number of Q being a halide ion is 1 or less; r is an integer of 1 to 7, s is an integer of 2 to 14, and d is an integer of 1 to 7, sr=d); (C-2): -(M 4 R 7 t-2 -O) u -……(Formula 6) (In Formula 6, M 4 is a metal or metalloid of Group 13 to Group 15 of the Periodic Table, R 7 are each independently a hydrocarbon group having 1 to 12 carbon atoms or a substituted hydrocarbon group having 1 to 12 carbon atoms, and t is a metal M 4 valence, u is an integer greater than 2).
13. The method for producing an olefin polymerization catalyst according to claim 12, wherein: The inorganic solid particles [A] are magnesium chloride particles.
14. A catalyst for olefin polymerization, wherein: The olefin polymerization catalyst comprises inorganic solid particles [A], a transition metal compound component [B-1] and / or a transition metal compound component [B-2], and an activator [C] and / or an organic metal compound component [D]. The transition metal compound [B-1] is a compound represented by the following (Formula 3), the transition metal compound [B-2] is a compound represented by the following (Formula 4), the activator [C] is a compound represented by the following (Formula 5) or (Formula 6), the organometallic compound component [D] is a compound containing at least one metal selected from the group consisting of Group 1, Group 2, Group 12 and Group 13 of the periodic table, the inorganic solid particles [A] are porous polymer materials or inorganic solid particles containing at least one element selected from the group consisting of Groups 2 to 4, Groups 13 and 14 of the periodic table, The content (mol) of the central metal M contained in the transition metal compound component [B-1] and / or the transition metal compound component [B-2] is 20 micromol or more and 1000 micromol or less, and the molar ratio (Al / M) of the content (mol) of the central metal M to the content (mol) of Al is 1 or more and 30 or less, L 1 j W k M 1 X 1 p X 2 q ……(Formula 3) (In Formula 3, L 1 each independently represents an n-bonding cyclic anionic ligand selected from the group consisting of a cyclopentadienyl group, an indenyl group, a tetrahydroindenyl group, a fluorenyl group, a tetrahydrofluorenyl group and an octahydrofluorenyl group, wherein the ligand has 1 to 8 substituents as the case may be, and the substituents are each independently selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a halogenated hydrocarbon group having 1 to 12 carbon atoms, an aminohydrocarbon group having 1 to 12 carbon atoms, a hydrocarbyloxy group having 1 to 12 carbon atoms, a dihydrocarbylamino group having 1 to 12 carbon atoms, a hydrocarbylphosphino group having 1 to 12 carbon atoms, a silyl group, an aminosilyl group, a hydrocarbyloxysilyl group having 1 to 12 carbon atoms and a halogenated silyl group and having 20 or less non-hydrogen atoms, M 1 represents a transition metal selected from the group of transition metals belonging to Group 4 of the Periodic Table of the Elements having a formal oxidation number of +2, +3 or +4 and having an η5 bond with at least one ligand L, W represents a divalent substituent having 50 or less non-hydrogen atoms and bonding to each of L and M with a univalent valency to form a metal ring compound together with L and M, X 1 each independently represents an anionic sigma-bonded ligand having 60 or less non-hydrogen atoms selected from the group consisting of a monovalent anionic sigma-bonded ligand, a divalent anionic sigma-bonded ligand divalently bonded to M, and a divalent anionic sigma-bonded ligand monovalently bonded to each of L and M, X 2 each independently represents a neutral Lewis base coordinating compound having 40 or less non-hydrogen atoms, j is 1 or 2, wherein when j is 2, the two ligands L are bonded to each other through a divalent group having 20 or less non-hydrogen atoms, the divalent group being a group selected from the group consisting of a hydrocarbon diyl group having 1 to 20 carbon atoms, a halogenated hydrocarbon diyl group having 1 to 12 carbon atoms, an alkyleneoxy group having 1 to 12 carbon atoms, an alkyleneamino group having 1 to 12 carbon atoms, a silanediyl group, a halogenated silanediyl group, and a silyleneamino group, k is 0 or 1, p is 0, 1 or 2, wherein in X 1 In the case of a monovalent anionic σ-bonding type ligand or a divalent anionic σ-bonding type ligand bonded to L and M, p is an integer smaller than the formal oxidation number of M by 1 or more, and in the case of X 1 In the case of a divalent anionic σ-bonded ligand that is bonded only to M, p is an integer that is (j+1) or more smaller than the formal oxidation number of M, and q is 0, 1 or 2); (In Formula 4, M 2 represents a transition metal selected from the group consisting of titanium, zirconium and hafnium and having a formal oxidation number of +2, +3 or +4, R 5 Each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 8 carbon atoms, a silyl group, a germyl group, a cyano group, a halogen atom, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein in the substituent R 5 When it is a hydrocarbon group having 1 to 8 carbon atoms, a silyl group or a germyl group, two adjacent substituents R 5 bonded to each other to form a divalent group, thereby bonding to the two adjacent substituents R 5 The bonds between the two carbon atoms of the cyclopentadienyl ring to which each is bonded together form a ring, X 3 Each independently represents a substituent selected from the group consisting of a halogen ion, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbonoxy group having 1 to 18 carbon atoms, a hydrocarbonamino group having 1 to 18 carbon atoms, a silyl group, a hydrocarbonamide group having 1 to 18 carbon atoms, a hydrocarbonphosphine group having 1 to 18 carbon atoms, a hydrocarbonthio group having 1 to 18 carbon atoms, and a composite group thereof, and having 1 to 20 non-hydrogen atoms, wherein two substituents X may be selected from the group consisting of 3 Together they form a neutral conjugated diene or divalent group having 4 to 30 carbon atoms, Y 1 Indicates -O-, -S-, -NR 6 -or-PR 6 -, where R 6 represents a hydrogen atom, a hydrocarbon group having 1 to 12 carbon atoms, a hydrocarbonoxy group having 1 to 8 carbon atoms, a silyl group, a halogenated alkyl group having 1 to 8 carbon atoms, a halogenated aryl group having 6 to 20 carbon atoms, or a composite group thereof, Z 1 represents SiR 6 2. CR 6 2. SiR 6 2SiR 6 2. CR 6 2CR 6 2. CR 6 =CR 6 . CR 6 2SiR 6 2 or GeR 6 2, where R 6 As defined above, n is 1, 2 or 3); (C-1): [L 2 -H] d+ [M 3 r Q s ] d- ……(Formula 5) (In Formula 5, [L 2 -H] d+ For proton-donating Bronsted acids, L 2 is a neutral Lewis base; in addition, in Formula 5, [M 3 r Q s ] d- is a compatible non-coordinating anion, M 3 is a metal or metalloid selected from Groups 5 to 15 of the periodic table, Q is independently a hydride ion, a dialkylamino group, a halide ion, an alkoxy group, an allyloxy group, a hydrocarbon group, or a substituted hydrocarbon group having 20 or less carbon atoms, and the number of Q being a halide ion is 1 or less; r is an integer of 1 to 7, s is an integer of 2 to 14, and d is an integer of 1 to 7, sr=d); (C-2): -(M 4 R 7 t-2 -O) u -……(Formula 6) (In Formula 6, M 4 is a metal or metalloid of Group 13 to Group 15 of the Periodic Table, R 7 are each independently a hydrocarbon group having 1 to 12 carbon atoms or a substituted hydrocarbon group having 1 to 12 carbon atoms, and t is a metal M 4 valence, u is an integer greater than 2).
15. The catalyst for olefin polymerization according to claim 14, wherein The inorganic solid particles [A] are magnesium chloride particles.
16. A method for producing an olefin polymer, wherein: The method for producing an olefin polymer comprises the step of polymerizing olefin using the olefin polymerization catalyst according to claim 14 or 15.