Polyurethane composition and marine hose

By using a combination of polyether polyol, toluene diisocyanate, urethane prepolymer, specific curing agent and adipic acid in the polyurethane composition, the problem of insufficient performance of the polyurethane composition in the open system in the prior art is solved , achieving excellent room temperature curability, foaming resistance, hardness and water resistance, and is suitable for marine hoses.

CN118765294APending Publication Date: 2024-10-11THE YOKOHAMA RUBBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023893.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult for existing polyurethane compositions to achieve the same or better performance when cured at room temperature in an open system than when using MOCA, including pot life, blistering resistance, hardness, abrasion resistance and water resistance.

Method used

Utilizes an isocyanate-based urethane prepolymer formed from polyether polyol and toluene diisocyanate, combined with trimethylene bis(4-aminobenzoate) or 3,5-diamino-4-chlorobenzoic acid-2 -Methylpropyl curing agent and adipic acid catalyst, control the molar ratio of isocyanate group to amino group and the content of curing agent to form a polyurethane composition with excellent performance.

Benefits of technology

A polyurethane composition has been realized that has excellent curability, foaming resistance, hardness and abrasion resistance under room temperature conditions in an open system, as well as excellent water resistance, and is suitable for the outermost layer of marine hoses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012410600000061
    Figure BDA0005012410600000061
  • Figure BDA0005012410600000062
    Figure BDA0005012410600000062
  • Figure BDA0005012410600000151
    Figure BDA0005012410600000151
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a polyurethane composition which can be used for a long time, has excellent curability in an open system under room temperature conditions, and has excellent blister resistance, hardness after curing, wear resistance, and water resistance; and a marine hose. The present invention is a room-temperature-curable polyurethane composition which contains a urethane prepolymer that is formed from a polyether polyol and a toluene diisocynate and that has an isocyanate group, a urethane prepolymer that contains a trimethylene bis (4-aminobenzoate) and / or a 3, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, 3, 4-trimethyl-1, the present invention relates to a polyurethane resin composition comprising a urethane prepolymer and 3, 5-diamino-4-chlorobenzoic acid-2-methyl propyl ester, a curing agent comprising 3, 5-diamino-4-chlorobenzoic acid-2-methyl propyl ester, and adipic acid as a catalyst, the molar ratio of the isocyanate group of the urethane prepolymer to the amino group of the curing agent being 0.90-2.00, and the molar ratio of trimethylene bis (4-aminobenzoate) and / or 3, 5-diamino-4-chlorobenzoic acid-2-methyl propyl ester being 0.00-0.00. And the content of the 2-methylpropyl 3, 5-diamino-4-chlorobenzoic acid-2-methyl propyl ester accounts for 95-100 mol% of the total amount of the curing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyurethane composition and a hose for ships. Background Art

[0002] Conventionally, crude oil and other petroleum have been transported between onshore oil tanks and offshore tankers using ship hoses.

[0003] For example, polyurethane is used as the outermost layer covering large rubber products such as ship hoses. In addition, 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) has been used as a curing agent used to obtain polyurethane from the viewpoint of excellent balance between curability and physical properties.

[0004] On the other hand, in recent years, from the viewpoint of environmental hygiene, a polyurethane molded product obtained by casting a polyurethane resin composition without using MOCA, heating and curing the composition has been known (for example, Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 4861001 Summary of the invention

[0008] Problems to be solved by the invention

[0009] Among them, the present inventors prepared a polyurethane composition with reference to Patent Document 1, cured it at room temperature in an open system (a state in which it can come into contact with moisture) and evaluated it. As a result, it was found that it is sometimes difficult to obtain performance that is equal to or exceeds that when MOCA is used (obtaining sufficiently long usable time, excellent curing and blistering resistance under room temperature and in an open system, high hardness after curing, and excellent wear resistance and water resistance).

[0010] Therefore, an object of the present invention is to provide a polyurethane composition having excellent usable time, curability at room temperature and in an open system, foaming resistance, hardness after curing, abrasion resistance, and water resistance.

[0011] Another object of the present invention is to provide a hose for a ship.

[0012] Technical means of solving problems

[0013] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that the desired effect can be obtained by using a polyurethane composition comprising a urethane prepolymer formed from a polyether polyol and toluene diisocyanate and having an isocyanate group, a curing agent comprising trimethylene bis(4-aminobenzoate) and / or 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester, and adipic acid as a catalyst, wherein the molar ratio of the isocyanate group of the urethane prepolymer to the amino group of the curing agent and the content of trimethylene bis(4-aminobenzoate) and / or 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester are within specific ranges, thereby completing the present invention.

[0014] The present invention has been accomplished based on the above findings and the like, and specifically, is an invention that solves the above problems by the following configurations.

[0015] [1] A room temperature curable polyurethane composition comprising:

[0016] A urethane prepolymer formed from a polyether polyol and toluene diisocyanate and having an isocyanate group,

[0017] A curing agent comprising trimethylene bis(4-aminobenzoate) and / or 2-methylpropyl 3,5-diamino-4-chlorobenzoate,

[0018] and adipic acid as a catalyst,

[0019] The molar ratio of the isocyanate group of the urethane prepolymer to the amino group of the curing agent is 0.90 to 2.00,

[0020] The content of the trimethylene bis(4-aminobenzoate) and / or the 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester is 95 to 100 mol % of the total amount of the curing agent.

[0021] [2] The polyurethane composition according to [1], wherein the total amount of the curing agent is trimethylene bis(4-aminobenzoate).

[0022] [3] The polyurethane composition according to [1], wherein the total amount of the curing agent is 2-methylpropyl 3,5-diamino-4-chlorobenzoate.

[0023] [4] The polyurethane composition according to any one of [1] to [3], wherein the molar ratio is 1.00 to 1.25.

[0024] [5] The polyurethane composition according to any one of [1] to [4], wherein the molar ratio is 1.02 to 1.08.

[0025] [6] The polyurethane composition according to any one of [1] to [5], wherein the content of the adipic acid is 0.03 to 0.20 parts by mass based on 100 parts by mass of the urethane prepolymer.

[0026] [7] The polyurethane composition according to any one of [1] to [6], wherein the content of the adipic acid is 0.09 to 0.13 parts by mass based on 100 parts by mass of the urethane prepolymer.

[0027] [8] The polyurethane composition according to any one of [1] to [7], which is used for a hose for a ship.

[0028] [9] A hose for a ship, formed using the polyurethane composition according to any one of [1] to [7].

[0029]

[10] The ship hose according to [9], which has an outermost layer formed using the polyurethane composition.

[0030] Effects of the Invention

[0031] The polyurethane composition of the present invention is excellent in usable time, curability at room temperature and in an open system, foaming resistance, hardness after curing, abrasion resistance, and water resistance.

[0032] The polyurethane composition of the present invention can be used to form the marine hose of the present invention. DETAILED DESCRIPTION

[0033] The present invention is described in detail below.

[0034] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values ​​described before and after "to".

[0035] In this specification, unless otherwise specified, the method for producing each component is not particularly limited, and for example, conventionally known methods can be cited.

[0036] In the present specification, unless otherwise specified, each component may be used alone or in combination of two or more substances. When a component includes two or more substances, the content of the component refers to the total content of the two or more substances.

[0037] In this specification, at least one of the usable time, curability at room temperature and in an open system, blister resistance, hardness after curing, abrasion resistance, and water resistance being superior may be referred to as having superior effects of the present invention.

[0038] [Polyurethane composition]

[0039] The polyurethane composition of the present invention (composition of the present invention) is a room temperature curing type polyurethane composition comprising:

[0040] A urethane prepolymer formed from a polyether polyol and toluene diisocyanate and having an isocyanate group,

[0041] A curing agent comprising trimethylene bis(4-aminobenzoate) and / or 2-methylpropyl 3,5-diamino-4-chlorobenzoate,

[0042] and adipic acid as a catalyst,

[0043] The molar ratio of the isocyanate group of the urethane prepolymer to the amino group of the curing agent is 0.90 to 2.00,

[0044] The content of the trimethylene bis(4-aminobenzoate) and / or the 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester is 95 to 100 mol % of the total amount of the curing agent.

[0045] Hereinafter, each component contained in the composition of the present invention will be described in detail.

[0046] [Urethane prepolymer]

[0047] The urethane prepolymer contained in the composition of the present invention is formed from a polyether polyol and toluene diisocyanate.

[0048] [Polyether polyol]

[0049] The polyether polyol used for forming the above-mentioned urethane prepolymer is a compound having a plurality of hydroxyl groups per molecule and a polyether main chain.

[0050] Examples of the polyether polyol include polyoxyethylene glycol (polyethylene glycol), polyoxypropylene glycol (polypropylene glycol: PPG), polyoxypropylene triol, ethylene oxide / propylene oxide copolymers, and polytetramethylene ether glycol (PTMEG).

[0051] From the viewpoint of further improving the effects of the present invention, the polyether polyol preferably contains polytetramethylene ether glycol.

[0052] The weight average molecular weight of the polyether polyol is preferably 500 to 20,000 from the viewpoint that the viscosity of the urethane prepolymer obtained by the reaction with isocyanate (isocyanate containing at least toluene diisocyanate) can have appropriate fluidity at room temperature. In the present invention, the weight average molecular weight is a polystyrene conversion value obtained by the GPC method (solvent: tetrahydrofuran (THF)).

[0053] [Toluene diisocyanate]

[0054] The toluene diisocyanate used for forming the urethane prepolymer is not particularly limited. Examples of the toluene diisocyanate include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, and mixtures thereof.

[0055] [Isocyanate group]

[0056] The urethane prepolymer contained in the composition of the present invention has an isocyanate group.

[0057] The isocyanate groups may be derived from toluene diisocyanate.

[0058] The urethane prepolymer may have an isocyanate group at the terminal and / or on the side chain of the urethane prepolymer.

[0059] From the viewpoint of further improving the effects of the present invention, the urethane prepolymer preferably has a plurality of isocyanate groups.

[0060] For the purpose of making the effect of the present invention more excellent, the content of isocyanate groups (NCO%) of the urethane prepolymer is preferably 0.5 to 5% by mass of the total amount of the urethane prepolymer. The content of isocyanate groups (NCO%) may also be a theoretically calculated value. When the urethane prepolymer is a commercially available product, the content of isocyanate groups (NCO%) of the urethane prepolymer may also be a catalog value.

[0061] (Preparation of urethane prepolymer)

[0062] The preparation method of the urethane prepolymer is not particularly limited. For example, the urethane prepolymer can be produced by using a polyol containing at least a polyether polyol (preferably the entire amount of the polyol is polyether polyol) and a polyisocyanate containing at least toluene diisocyanate (preferably the entire amount of the polyisocyanate is toluene diisocyanate), making the isocyanate group of the polyisocyanate excessive relative to the hydroxyl group of the polyol, and mixing them to react.

[0063] [Curing agent]

[0064] The composition of the present invention contains a curing agent, and the curing agent includes trimethylene bis(4-aminobenzoate) and / or 2-methylpropyl 3,5-diamino-4-chlorobenzoate.

[0065] In the present invention, the curing agent refers to a component having a plurality of active hydrogen-containing groups and capable of reacting with the urethane prepolymer. The active hydrogen-containing groups are not particularly limited. For example, amino groups (-NH2) can be cited.

[0066] The reaction of trimethylene bis(4-aminobenzoate) with the urethane prepolymer is slow, so the composition of the present invention can obtain a sufficiently long usable time. The same is true for 2-methylpropyl 3,5-diamino-4-chlorobenzoate.

[0067] [Trimethylene bis(4-aminobenzoate)]

[0068] Trimethylene bis(4-aminobenzoate) is a compound having the following structure and has an amino group (—NH 2 ).

[0069] In this specification, trimethylenebis(4-aminobenzoate) may be referred to as "specific curing agent 1".

[0070] [Chemical formula 1]

[0071]

[0072] [2-Methylpropyl 3,5-diamino-4-chlorobenzoate]

[0073] 3,5-diamino-4-chlorobenzoic acid 2-methylpropyl ester (3,5-diamino-4-chlorobenzoic acid 2-methylpropyl ester) is a compound of the following structure and has an amino group (—NH 2 ).

[0074] In this specification, 2-methylpropyl 3,5-diamino-4-chlorobenzoate may be referred to as "specific curing agent 2".

[0075] [Chemical formula 2]

[0076]

[0077] The curing agent preferably contains the specific curing agent 1 from the viewpoint that the obtained cured product has excellent color development and can suppress discoloration over time.

[0078] [Content of specific curing agent 1, 2]

[0079] In the present invention, the content of trimethylene bis(4-aminobenzoate) and / or 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester is 95 to 100 mol % of the total amount of the curing agent.

[0080] In the present invention, when the curing agent includes the specific curing agent 1 and the specific curing agent 2, the total content of the specific curing agent 1 and the specific curing agent 2 is 95 to 100 mol % of the total amount of the curing agent.

[0081] (Other curing agents)

[0082] When the content of the specific curing agent 1 and / or the specific curing agent 2 is 95 mol % or more and less than 100 mol % of the total amount of the curing agent, the curing agent may further contain a curing agent other than the specific curing agent 1 and the specific curing agent 2 (other curing agents).

[0083] Other curing agents (excluding specific curing agent 1 and specific curing agent 2) are not particularly limited as long as they are compounds having a plurality of active hydrogen-containing groups (active hydrogen compounds) in one molecule. Examples of the active hydrogen-containing group include hydroxyl groups, amino groups, and imino groups.

[0084] Regarding the curing agent, from the viewpoint of making the effects of the present invention more excellent, the color development of the obtained cured product excellent, and being able to suppress discoloration over time, the curing agent preferably contains trimethylene bis(4-aminobenzoate), and more preferably the entire amount of the curing agent is trimethylene bis(4-aminobenzoate).

[0085] From the viewpoint of achieving more excellent effects of the present invention (particularly abrasion resistance and water resistance), the entire amount of the curing agent is preferably 2-methylpropyl 3,5-diamino-4-chlorobenzoate.

[0086] [Molar ratio of isocyanate group to amino group]

[0087] In the present invention, the molar ratio (NCO / NH2) of the isocyanate group of the urethane prepolymer to the amino group of the curing agent is 0.90 to 2.00.

[0088] As described above, the specific curing agent 1 and the specific curing agent 2 each have an amino group (—NH 2 ).

[0089] From the viewpoint of achieving more excellent effects of the present invention (particularly wear resistance), the molar ratio is preferably 1.00 to 1.25, more preferably 1.02 to 1.08.

[0090] In the present invention, the molar ratio (NCO / NH2) of the isocyanate group of the urethane prepolymer to the amino group of the curing agent can be calculated from the content of the isocyanate group of the urethane prepolymer (NCO%) and the amine value of the curing agent (unit: mgKOH / g) according to the following formula. When the curing agent has an amine value within a numerical range, the average value of the amine value of the curing agent can be used to calculate the molar ratio. When the curing agent is a commercially available product, the product catalog value can be used as the amine value of the curing agent.

[0091] Molar ratio (NCO / NH2) = A / B

[0092] A=Usage amount of urethane prepolymer (g)×NCO%×0.01÷42.1

[0093] B = amount of curing agent used (g) × amine value × 0.001 ÷ 56

[0094] It should be noted that when the curing agent further contains a curing agent (other curing agent) other than the specific curing agent 1 and the specific curing agent 2, the active hydrogen-containing group possessed by the other curing agent can be added to the amino group in the above molar ratio. In the present invention, the molar ratio after addition can be 0.90 to 2.00, and the preferred range is the same as above.

[0095] [Adipic acid]

[0096] The composition of the present invention contains adipic acid as a catalyst.

[0097] Adipic acid can accelerate the reaction between the urethane prepolymer and trimethylene bis(4-aminobenzoate) and / or 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl over time. Therefore, the composition of the present invention can have a sufficiently long usable time and, on the other hand, has excellent curability (particularly curability after 24 hours) at room temperature and in an open system.

[0098] Adipic acid (HOOC-CH2CH2CH2CH2-COOH) is not particularly limited.

[0099] (Adipic acid content)

[0100] From the viewpoint of making the effects of the present invention more excellent, the content of adipic acid is preferably 0.03 to 0.20 parts by mass relative to 100 parts by mass of the above-mentioned urethane prepolymer, and from the viewpoint of making the effects of the present invention (particularly the usable time, curability under room temperature and in an open system, abrasion resistance, and water resistance) more excellent, having excellent workability such as coating due to the low viscosity 5 minutes after the completion of mixing, and being able to suppress the deterioration of physical properties before and after a water resistance test, it is more preferably 0.09 to 0.13 parts by mass relative to 100 parts by mass of the above-mentioned urethane prepolymer.

[0101] (additive)

[0102] The composition of the present invention may contain additives as necessary within a range not impairing the effects of the present invention.

[0103] Examples of additives include fillers, plasticizers, antioxidants, and colorants. The type and content of each additive can be appropriately selected.

[0104] As a preferred embodiment, the composition of the present invention does not contain MOCA.

[0105] As a preferred embodiment, in the composition of the present invention, the content of the metal catalyst (catalyst containing a metal) is 0 to 0.5 parts by mass based on 100 parts by mass of the urethane prepolymer.

[0106] (Method for producing polyurethane composition)

[0107] The method for producing the composition of the present invention is not particularly limited, and examples thereof include a method of mixing the above-mentioned components under a nitrogen atmosphere.

[0108] [Room temperature curing type]

[0109] The polyurethane composition of the present invention is a room temperature curing type. In addition, the polyurethane composition of the present invention can be cured at room temperature and in an open system. That is, the composition of the present invention can be cured by moisture under room temperature conditions to form a polyurethane. The composition of the present invention can be cured under conditions of, for example, 0 to 35° C. and a relative humidity of 20 to 65%.

[0110] (Purpose, etc.)

[0111] The composition of the present invention can be used, for example, in large rubber products such as ship hoses, and more specifically, can be used, for example, in the outermost layer covering the rubber products.

[0112] The rubber constituting the rubber product is not particularly limited.

[0113] As described above, since the composition of the present invention is a room temperature curing type, it can be applied to large products without using heating or molds, which is useful.

[0114] [Ship hose]

[0115] The ship hose of the present invention is a ship hose formed using the polyurethane composition of the present invention.

[0116] The polyurethane composition used in the marine hose of the present invention is not particularly limited as long as it is the polyurethane composition of the present invention.

[0117] There is no particular limitation on which component the ship hose of the present invention is used for the polyurethane composition.

[0118] From the viewpoint of making the polyurethane composition of the present invention excellent in abrasion resistance, water resistance, etc., the hose for a ship of the present invention preferably has an outermost layer formed using the polyurethane composition.

[0119] The thickness of the outermost layer can be set to, for example, 3 to 20 mm.

[0120] When the ship hose of the present invention has an outermost layer formed using the polyurethane composition, the ship hose body covered by the outermost layer is not particularly limited, and examples thereof include conventionally known materials.

[0121] The surface layer of the ship hose body may be, for example, a rubber layer. The rubber layer may be, for example, a rubber layer containing nitrile rubber as the rubber.

[0122] When the ship hose body has a rubber layer, the ship hose body only needs to be vulcanized.

[0123] (Manufacture of marine hoses)

[0124] The method for producing the ship hose of the present invention includes, for example, applying the polyurethane composition on the surface of a vulcanized rubber ship hose body, and then curing the polyurethane composition under 0 to 35° C. using moisture in the atmosphere to form an outermost layer.

[0125] There is no particular limitation on the method of applying the polyurethane composition to the surface of the main body of the marine hose. For example, various commonly used application methods can be used. Specifically, for example, a method of applying with a brush can be cited.

[0126] Example

[0127] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited to these Examples.

[0128] [Manufacturing of polyurethane composition]

[0129] Each polyurethane composition was prepared by mixing the components in Table 1 below in the compositions (parts by mass) using a stirrer. In the mixing, the urethane prepolymer was heated to 80° C. in advance, and the curing agent was used in a heated and melted state.

[0130] [evaluate]

[0131] The following evaluations were performed using each polyurethane composition produced as described above. The results are shown in Table 1.

[0132] *Usable time (applicable period)

[0133] Evaluation method

[0134] The viscosity of each polyurethane composition produced in the above manner was measured every 60 seconds at 20°C and 50% RH (relative humidity) using a BH viscometer (rotor number: 6, rotation speed 10 rpm), and the time from the start of measurement until the viscosity reached 25,000 mPa·s was defined as the pot life.

[0135] Evaluation benchmark

[0136] If the pot life is 8 to 20 minutes, it is evaluated that the usable time is sufficiently long and this is indicated as "0." The number after "0" is the measurement result of the pot life (minutes).

[0137] If the pot life is more than 3 minutes but less than 8 minutes, it is evaluated that the usable time is slightly short, but there is no problem in practical use, and this is indicated as "Δ". The number after "Δ" is the pot life (minutes).

[0138] In the present invention, if the pot life exceeds 3 minutes, it is evaluated that the usable time is long (the usable time is excellent).

[0139] On the other hand, if the pot life is 3 minutes or less, it is evaluated that the usable time is very short and not practical, and this is indicated by "×". The number after "×" is the pot life (minutes).

[0140] *Viscosity (5 minutes after mixing)

[0141] Each polyurethane composition prepared by mixing in the above manner was placed in an environment of 20°C and 50% RH (relative humidity), and the viscosity (in mPa·s) of the polyurethane composition 5 minutes after the mixing was completed was measured using a BH type viscometer (rotor number: 6, rotation speed 10 rpm). It should be noted that if the above viscosity cannot be measured (for example, the curing of the mixed composition is too fast, resulting in the material being cured at the stage just after mixing), it will be indicated as "cannot be measured".

[0142] The viscosity of the polyurethane composition 5 minutes after the mixing is not particularly limited, but is preferably 5,000 to 25,000 mPa·s as a viscosity that allows for coating. When the viscosity of the polyurethane composition 5 minutes after the mixing is 5,000 mPa·s or more, even if the mixed polyurethane composition is coated on a cylindrical rubber product such as a ship hose, the polyurethane composition is unlikely to drip from the rubber product, making it easy to ensure the thickness of the polyurethane composition, which is preferred from this point of view. When the viscosity of the polyurethane composition 5 minutes after the mixing is 25,000 mPa·s or less, it is preferred from the viewpoint of easy coating.

[0143] From the above viewpoints, the viscosity of the polyurethane composition 5 minutes after the completion of mixing is more preferably 7,000 to 10,000 mPa·s, and even more preferably 7,000 to 15,000 mPa·s.

[0144] *Curing (hardness after 24 hours at room temperature in an open system)

[0145] Evaluation method

[0146] Each polyurethane composition prepared in the above manner was cast into a 10 mm thick mold (5 cm long, 5 cm wide), and then cured for 24 hours in an environment of 20° C. and 50% RH (relative humidity) with the upper part of the mold open.

[0147] After the curing, the hardness of the obtained cured product (cured product after 24 hours) was measured in accordance with JIS K6253-3:2012.

[0148] Evaluation benchmark

[0149] If the hardness measured in the above manner at room temperature (20° C.) and after 24 hours in an open system is 50 or more, the curability is evaluated to be excellent. The greater the hardness is than 50, the more excellent the curability is.

[0150] On the other hand, when the hardness is less than 50, the curability is evaluated to be poor.

[0151] * Foam resistance

[0152] Evaluation method

[0153] A 5 mm thick mold (15 cm long and 20 cm wide) was placed on a rubber sheet formed of nitrile rubber, and each polyurethane composition manufactured in the above manner was cast in the mold, and then cured for 7 days in an environment of 20°C and 50% RH (relative humidity) with the upper part of the mold open.

[0154] After curing, the obtained cured product (laminate of rubber layer and polyurethane layer) was cut into strips of 15 cm in length and 25 mm in width, and the interface between the polyurethane layer and the rubber layer in the cut section in the longitudinal direction of the strip was visually observed.

[0155] Evaluation benchmark

[0156] If there were no bubbles in the interface or if there were bubbles but the number of bubbles was less than 10, and there were no cracks in the interface, the blistering resistance was evaluated to be excellent and represented as "0".

[0157] When the interface is in the above-described state, it is considered that the adhesion between the polyurethane layer and the rubber layer is excellent.

[0158] On the other hand, when there were 10 or more bubbles at the interface, or cracks at the interface, the blister resistance was evaluated to be poor.

[0159] When the interface is in the above-described state, it is considered that the adhesion between the polyurethane layer and the rubber layer is poor.

[0160] *JIS-A hardness (hardness after 7 days)

[0161] Evaluation method

[0162] Each polyurethane composition produced in the above manner was cast into a 2 mm thick mold and then cured for 7 days in an environment of 20° C. and 50% RH (relative humidity) with the upper part of the mold open.

[0163] After the curing, the hardness of the obtained sheet-like cured product (cured product after 7 days) was measured in accordance with JIS K6253-3:2012.

[0164] In this specification, if the polyurethane composition is cured under the above conditions (cured for 7 days at 20° C. and 50% RH with the upper portion of the mold open), the obtained cured product is regarded as a completely cured product.

[0165] Evaluation benchmark

[0166] When the hardness of the cured product obtained as described above after 7 days is 83 to 93, it is evaluated that the hardness after complete curing is excellent.

[0167] On the other hand, when the hardness is less than 83 or exceeds 93, it is evaluated that the hardness after complete curing is low.

[0168] It should be noted that if a solidified product was not obtained after the 7-day curing, it was indicated as “unable to produce a sheet.” In addition, if a solidified product was not obtained after the 7-day curing, the JIS-A hardness, the wear resistance and the water resistance described later were not evaluated.

[0169] * Wear resistance: DIN wear volume (mm 3 )

[0170] Evaluation method

[0171] Three sheets of the cured products (cured products after 7 days) obtained for measuring the JIS-A hardness were stacked and subjected to a DIN wear test using the B method (a test method in which the drum is rotated) in accordance with JIS K 6264-2:2005 to measure the wear volume (mm). 3 ).

[0172] Evaluation benchmark

[0173] If the above wear volume is 100mm 3 The smaller the wear volume is, the better the wear resistance is. 3 , the better the wear resistance.

[0174] On the other hand, if the above wear volume exceeds 100mm 3 , the wear resistance is evaluated as poor.

[0175] *Water resistance: 100% modulus after 60℃ warm water × 4W (MPa)

[0176] Evaluation method

[0177] A water resistance test was conducted by immersing the same sheet-shaped cured product (cured product after 7 days) obtained for measuring the JIS-A hardness in warm water at 60° C. for 4 weeks.

[0178] After the water resistance test, the cured product was pulled out of the warm water, and a dumbbell No. 3 test piece was punched out from the cured product. A tensile test was performed at a tensile speed of 200 mm / min in accordance with JIS K6251:2017, and the 100% modulus (MPa) after the water resistance test was measured.

[0179] Evaluation benchmark

[0180] If the 100% modulus after the water resistance test is 4.0 MPa or more, the water resistance (warm water resistance) is evaluated to be excellent. The larger the 100% modulus is than 4.0 MPa, the more excellent the water resistance (warm water resistance) is.

[0181] On the other hand, when the 100% modulus is less than 4.0 MPa, the water resistance is evaluated to be poor.

[0182] 100% modulus before water resistance test (MPa)

[0183] A dumbbell-shaped No. 3 test piece was punched out from the same sheet-like cured product (cured product after 7 days) as the cured product obtained for measuring the JIS-A hardness (not subjected to water resistance test), and a tensile test was performed at a tensile speed of 200 mm / min in accordance with JIS K6251:2017 to measure the 100% modulus (MPa) before the water resistance test.

[0184] ·100% modulus maintenance rate before and after water resistance test

[0185] The 100% modulus after the water resistance test and the 100% modulus before the water resistance test measured in the above manner were substituted into the following formula to calculate the maintenance rate of the 100% modulus before and after the water resistance test.

[0186] 100% modulus maintenance rate before and after water resistance test (%)

[0187] =A÷B×100

[0188] A: 100% modulus after water resistance test

[0189] B: 100% modulus before and after water resistance test

[0190] The larger the maintenance rate is, the more deterioration in physical properties of the ship hose during use can be suppressed, which is preferable from this viewpoint.

[0191] *Color rendering

[0192] Evaluation method

[0193] The color (transparency) of the sheet-like cured product (cured product after 7 days) obtained for the measurement of the JIS-A hardness was visually confirmed.

[0194] Evaluation benchmark

[0195] In the present invention, if the above-mentioned solidified material is transparent, it is evaluated as the color development of the solidified material is excellent. In the case where the above-mentioned solidified material is transparent, the above-mentioned solidified material can also be colored. Regarding the situation where the above-mentioned solidified material is transparent, the following situations can be listed: the solidified material is, for example, colorless and transparent, yellow transparent, orange transparent, or red transparent. Since the color development of the solidified material is excellent, the appearance of the solidified material is also excellent, so it is preferred.

[0196] On the other hand, if the cured product is not transparent, the color development of the cured product is evaluated to be poor. Examples of the case where the cured product is not transparent include a case where the cured product is turbid or a case where the color of the cured product is darker than red (eg brown).

[0197] [Table 1]

[0198]

[0199] [Table 2]

[0200]

[0201] The details of each component shown in Table 1 are as follows.

[0202] (Urethane prepolymer)

[0203] Urethane prepolymer: trade name HYPRENE L-100, produced by Mitsui Chemicals Co., Ltd. Urethane prepolymer having an isocyanate group formed from polytetramethylene ether glycol and toluene diisocyanate (TDI). The isocyanate group content (NCO%) of the urethane prepolymer is 4.2% by mass.

[0204] (Curing agent)

[0205] The details of each curing agent used in the examples are shown below. It should be noted that the amine value of each curing agent is the value of the amine value used in the calculation of the molar ratio (NCO / NH2) of the isocyanate group of the urethane prepolymer to the amino group of the curing agent.

[0206] ·Trimethylene bis(4-aminobenzoate): Trade name CUA-4, produced by KUMIAI CHEMICAL INDUSTRY CO., LTD. Molecular weight 314.3. Amine value 346-368 mgKOH / g (357 mgKOH / g). Specific curing agent 1

[0207] (Comparison) 4,4-diamino-3,3-diethyl-5,5-dimethyldiphenylmethane: Trade name CurehardMED-J, produced by KUMIAI CHEMICAL INDUSTRY CO., LTD. Amine value 386-408 mgKOH / g (397 mgKOH / g)

[0208] ·(Comparison) 3,3'-dichloro-4,4'-diaminodiphenylmethane: MOCA. Trade name IHARA CUAMINE MT, produced by KUMIAI CHEMICAL INDUSTRY CO., LTD. Amine value 415-426 mgKOH / g (420.5 mgKOH / g)

[0209] · 2-Methylpropyl 3,5-diamino-4-chlorobenzoate: trade name ADDOLINK1604, produced by Lanxess Co., Ltd., molecular weight 242.7. Amine value 452 to 479 mgKOH / g (465.5 mgKOH / g). Specific curing agent 2

[0210] (Comparison) Dimethylthiotoluenediamine: trade name HARTCURE 30, produced by KUMIAI CHEMICAL INDUSTRY CO., LTD. Amine value 531 mgKOH / g (531 mgKOH / g)

[0211] (adipic acid)

[0212] Adipic acid: produced by Asahi Kasei Corporation

[0213] In Table 1, with Comparative Example 1 containing MOCA but not containing specific curing agent 1 and specific curing agent 2 as a reference, Comparative Example 2 in which the content of specific curing agent 1 and / or specific curing agent 2 does not meet the prescribed range has a short usable time, low hardness after complete curing (after 7 days), and poor abrasion resistance and water resistance. It should be noted that Comparative Example 1 containing MOCA but not containing specific curing agent 1 and specific curing agent 2 is not preferred from the viewpoint of environmental hygiene.

[0214] Comparative Example 3, which did not contain the specific curing agent 1 and the specific curing agent 2 but contained 4,4-diamino-3,3-diethyl-5,5-dimethyldiphenylmethane, had a short usable time and could not produce a sheet.

[0215] Comparative Example 4 in which the content of the specific curing agent 1 and / or the specific curing agent 2 did not satisfy the prescribed range had a short usable time, low hardness after complete curing (after 7 days), and poor water resistance.

[0216] Comparative Example 5, which did not contain the specific curing agent 1 and the specific curing agent 2 but contained dimethylthiotoluenediamine, had a short usable time and could not produce a sheet.

[0217] Comparative Example 6, in which the molar ratio (NCO / NH2) of the isocyanate group of the urethane prepolymer to the amino group of the curing agent is less than 0.90, has low hardness after complete curing (after 7 days), and poor curability, abrasion resistance and water resistance under room temperature and in an open system.

[0218] Comparative Example 7 in which the molar ratio (NCO / NH2) exceeded 2.00 had poor blister resistance.

[0219] Comparative Example 8 containing no adipic acid had low hardness after complete curing (after 7 days), and was inferior in curability and water resistance at room temperature and in an open system.

[0220] Comparative Example 9 containing no adipic acid had poor curability at room temperature and in an open system.

[0221] In contrast, the polyurethane composition of the present invention can obtain a sufficiently long usable time, has excellent curability and foaming resistance at room temperature and in an open system, and has excellent hardness, abrasion resistance, and water resistance (warm water resistance) after curing (after 7 days).

[0222] The usable time, curability in an open system at room temperature, foaming resistance, hardness after curing (after 7 days), abrasion resistance, and water resistance (warm water resistance) of the polyurethane composition of the present invention are equal to or better than those of Comparative Example 1. Among them, from the comparison between Example 1 and Comparative Example 1, it can be seen that the polyurethane composition of the present invention has a longer usable time and excellent abrasion resistance compared with Comparative Example 1 containing MOCA.

[0223] The color development of the cured products obtained in Examples 1 to 7, 10, and 11 was excellent. On the other hand, the color development of the cured product obtained in Example 8 was poor. This is considered to be due to the use of specific curing agent 2 in Example 8. In Example 9, specific curing agents 1 and 2 were used together, and it is considered that the color development was poor as in Example 8 due to the use of specific curing agent 2.

[0224] The comparison results of Examples 10, 1 to 3, and 11 show that the viscosity of Examples 10 and 1 to 3 is lower than that of Example 11, and the viscosity of the polyurethane composition is lower. The viscosity of Example 11 is higher, and the viscosity increases faster, after 5 minutes of mixing.

[0225] Therefore, in the present invention, from the viewpoint of facilitating the application of the polyurethane composition (for example, application to a large rubber product such as a ship hose), it is considered that the content of adipic acid is preferably 0.15 parts by mass or less, and more preferably 0.13 parts by mass or less, relative to 100 parts by mass of the urethane prepolymer.

[0226] Regarding the above-mentioned "preferably less than 0.13 parts by mass", in terms of the usable time of Examples 2 and 3, Example 2 is 1 minute longer than Example 3. Furthermore, in terms of the viscosity 5 minutes after the mixing is completed, the comparison results of Examples 2 and 3 show that the viscosity of Example 2 is much lower than that of Example 3.

[0227] In addition, regarding the curability and wear resistance at room temperature in an open system, the comparison results of Examples 10, 1 to 3, and 11 show that the curability and wear resistance of Examples 2 to 3 and 11 at room temperature in an open system are far superior to those of Examples 10 and 1.

[0228] Therefore, from the viewpoint of improving the curability and / or abrasion resistance at room temperature and in an open system, the content of adipic acid is preferably 0.09 parts by mass or more based on 100 parts by mass of the urethane prepolymer.

Claims

1. A room temperature curable polyurethane composition comprising: A urethane prepolymer formed from a polyether polyol and toluene diisocyanate and having an isocyanate group, A curing agent comprising trimethylene bis(4-aminobenzoate) and / or 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester, and adipic acid as a catalyst, The molar ratio of the isocyanate group of the urethane prepolymer to the amino group of the curing agent is 0.90 to 2.00, The content of trimethylene bis(4-aminobenzoate) and / or 3,5-diamino-4-chlorobenzoic acid-2-methylpropyl ester is 95 to 100 mol % of the total amount of the curing agent.

2. The polyurethane composition according to claim 1, wherein The entire amount of the curing agent is trimethylene bis(4-aminobenzoate).

3. The polyurethane composition according to claim 1, wherein The total amount of the curing agent is 2-methylpropyl 3,5-diamino-4-chlorobenzoate.

4. The polyurethane composition according to any one of claims 1 to 3, wherein The molar ratio is 1.00 to 1.

25.

5. The polyurethane composition according to any one of claims 1 to 4, wherein The molar ratio is 1.02 to 1.

08.

6. The polyurethane composition according to any one of claims 1 to 5, wherein The content of the adipic acid is 0.03 to 0.20 parts by mass based on 100 parts by mass of the urethane prepolymer.

7. The polyurethane composition according to any one of claims 1 to 6, wherein The content of the adipic acid is 0.09 to 0.13 parts by mass based on 100 parts by mass of the urethane prepolymer.

8. The polyurethane composition according to any one of claims 1 to 7, which is used for a hose for a ship. 9 . A marine hose, formed using the polyurethane composition according to claim 1 . 10 . The ship hose according to claim 9 , which has an outermost layer formed using the polyurethane composition.