Siloxane-modified polyurethane composition

By blending silicone compounds and isocyanate compounds with specific structures into polyurethane compositions, the problems of insufficient heat resistance and strength of silicone-modified polyurethane resins are solved, and high tensile strength and excellent heat resistance are achieved. Synthesis of silicone modified polyurethane compositions.

CN118765295APending Publication Date: 2024-10-11SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023650.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2023-02-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing silicone-modified polyurethane resins have deficiencies in heat resistance and strength, and when reacting under solvent-free conditions, by-products are easily generated, resulting in reduced strength.

Method used

By blending silicone compounds with specific structures into the polyurethane composition, including hydroxyl-containing organosilicon compounds and isocyanate compounds, and optimizing the structure of the silicone-modified polyurethane composition through hydrosilylation reaction, its tensile strength is improved. and heat resistance.

Benefits of technology

The synthesis of a silicone-modified polyurethane composition with high tensile strength and excellent heat resistance is achieved, avoiding the generation of by-products and improving the physical properties and heat resistance of the resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765295A_ABST
    Figure CN118765295A_ABST
Patent Text Reader

Abstract

Provided is a siloxane-modified polyurethane composition containing (A) a hydroxyl group-containing organosilicon compound represented by formula (1) (R13SiO1 / 2) k (R12SiO2 / 2) p (R1SiO3 / 2) q (SiO4 / 2) r (1) [R1 is a monovalent hydrocarbon group or the like, but at least one of all R1 groups is a group represented by formula (2). K > 0, p > = 0, q > = 0, r > = 0, and k + p + q > = 2. ] # imgabs0 # (R2 is a hydrogen atom or the like, and R3 is a hydrogen atom or a methyl group. S is an integer of 0-4, t is an integer of 2-4, and u is a number of 1-3. And the dashed line represents a bonding end. ); (B) an isocyanate compound having two or more isocyanate groups in one molecule; and (C) an organic compound having two or more functional groups capable of reacting with an isocyanate group in one molecule.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a siloxane-modified polyurethane composition, and more particularly to a siloxane-modified polyurethane composition having a novel structure and a cured product thereof. Background Art

[0002] Polyurethane resin has excellent tensile strength, bending resistance, abrasion resistance, and oil resistance, and can be made thermoplastic or thermosetting depending on the composition, so it can be processed into various shapes.

[0003] As raw materials of the polyurethane resin, polyol, isocyanate, chain extender, etc. are used. In order to impart flexibility and slip properties to the polyurethane resin, copolymerization of hydroxyl-containing siloxane as a polyol has been proposed (Patent Documents 1 to 8).

[0004] The hydroxyl-containing polysiloxanes described in these patent documents are industrially produced by a hydrosilylation reaction of hydrogen polysiloxane with a hydroxyl-containing olefin compound such as allyl glycol or a polyoxyalkylene monoallyl ether.

[0005] However, for example, since allyl glycol has low compatibility with hydrogen polysiloxane, when reacting in the absence of a solvent, it is necessary to use an excess amount of allyl glycol relative to the hydrosilyl group.

[0006] In order to eliminate this, when an alcohol solvent such as ethanol or 2-propanol is used in the hydrosilylation reaction, the reactivity increases, and a byproduct is easily generated by a dehydrogenation reaction between the hydroxyl groups in the solvent and the hydrosilyl groups of the hydrogen polysiloxane. This byproduct causes the strength of the siloxane-modified polyurethane resin to decrease.

[0007] In addition, the above-mentioned patent document also reports a hydroxyl group-containing polysiloxane having a structure equivalent to that obtained by adding hydrogen polysiloxane to allyl alcohol, although it has not yet been produced industrially.

[0008] In addition, polysiloxanes having phenolic hydroxyl groups and hydroxyalkylene phenyl groups are also proposed in Patent Document 9, but phenolic hydroxyl groups are not suitable for polyurethane resin synthesis due to their low reactivity with isocyanate groups. In addition, polysiloxanes having hydroxyalkylene phenyl groups are difficult to produce industrially.

[0009] On the other hand, polyurethane resin has a problem of low heat resistance, and siloxane-modified polyurethane resin has a problem of reduced strength as described above.

[0010] From the above perspectives, a siloxane-modified polyurethane resin having excellent heat resistance and strength has been desired.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 10-101766

[0014] Patent Document 2: Japanese Patent Application Publication No. 2017-52821

[0015] Patent Document 3: Japanese Patent Application Publication No. 2004-250683

[0016] Patent Document 4: Japanese Patent Application Publication No. 2004-332126

[0017] Patent Document 5: Japanese Patent Application Publication No. 2011-174037

[0018] Patent Document 6: Japanese Patent Application Publication No. 2014-77120

[0019] Patent Document 7: Japanese Patent Application Publication No. 2014-193945

[0020] Patent Document 8: International Publication No. 2016 / 158967

[0021] Patent Document 9: Japanese Patent Application No. 2007-508425 Summary of the invention

[0022] Problems to be solved by the invention

[0023] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a siloxane-modified polyurethane composition which is easy to synthesize and can form a cured product having high resin physical property values ​​such as tensile strength and excellent heat resistance.

[0024] Means for solving problems

[0025] The present inventors have conducted intensive studies to solve the above problems and, as a result, have found that the above problems can be solved by blending a siloxane compound having a specific structure into a polyurethane composition, thereby completing the present invention.

[0026] That is, the present invention provides:

[0027] 1. A siloxane-modified polyurethane composition comprising:

[0028] (A) a hydroxyl-containing organosilicon compound represented by the following general formula (1):

[0029] (R 1 3SiO 1 / 2 ) k (R 1 2SiO 2 / 2 ) p (R 1 SiO 3 / 2 ) q (SiO4 / 2 ) r (1) [In formula (1), R 1 are independently selected from a monovalent hydrocarbon group having 1 to 10 carbon atoms and a group represented by the following formula (2), but all R 1 At least one of the groups is a group represented by the following formula (2). k, p, q and r are numbers such that k>0, p≥0, q≥0, r≥0, and k+p+q≥2. The bonding order of each siloxane unit shown in the parentheses is arbitrary.

[0030] [Chemistry 1]

[0031]

[0032] (In formula (2), R 2 are independently a hydrogen atom or a group selected from a monovalent hydrocarbon group having 1 to 5 carbon atoms and an alkoxy group having 1 to 5 carbon atoms, R 3 is a hydrogen atom or a methyl group. s is an integer of 0 to 4, t is an integer of 2 to 4, and u is a number of 1 to 3. The dotted line represents the bonding end. )]

[0033] (B) an isocyanate compound having two or more isocyanate groups in one molecule, and

[0034] (C) an organic compound having two or more functional groups reactive with an isocyanate group in one molecule;

[0035] 2. The siloxane-modified polyurethane composition according to 1, wherein the group represented by formula (2) is any one of the following formulas (3) to (5),

[0036] [Chemistry 2]

[0037]

[0038] (Where t and u are the same as above, and the dotted line represents the bonding end.)

[0039] 3. The siloxane-modified polyurethane composition according to 1 or 2, wherein in the formula (1) of the component (A), k is a number of 2 to 5, p is a number of 2 to 100, q is a number of 0 to 3, r is 0, and all R 1 2 to 5 of the groups are groups represented by formula (2);

[0040] 4. The siloxane-modified polyurethane composition according to any one of 1 to 3, wherein the component (A) is an addition reaction product of an organohydrogenpolysiloxane represented by the following general formula (6) and a compound containing a hydroxyl group and an aliphatic unsaturated group represented by the following general formula (7),

[0041] (R 4 3SiO 1 / 2 ) k (R 4 2SiO 2 / 2 ) p (R 4 SiO 3 / 2 ) q (SiO 4 / 2 ) r (6)

[0043] (In formula (6), R 4 are independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, but all R 4 At least one of the groups is a hydrogen atom. k, p, q and r are the same as above. In addition, the bonding order of each siloxane unit shown in the brackets is arbitrary.)

[0044] [Chemistry 3]

[0045]

[0046] (In formula (7), R 2 , R 3 , s, t and u are the same as above. )

[0047] 5. The siloxane-modified polyurethane composition according to 4, wherein the compound containing a hydroxyl group and an aliphatic unsaturated group represented by formula (7) is any one of the compounds represented by the following formulas (8) to (10),

[0048] [Chemistry 4]

[0049]

[0050] (Where t and u are the same as above.)

[0051] 6. The siloxane-modified polyurethane composition according to 4 or 5, wherein in the formula (6), k is a number of 2 to 5, p is a number of 2 to 100, q is a number of 0 to 3, r is 0, and all R 4 2 to 5 of the groups are hydrogen atoms;

[0052] 7. The siloxane-modified polyurethane composition according to any one of 1 to 6, wherein the component (B) is represented by the following formula (11):

[0053] OCN-Q-NCO(11)

[0054] (In the above formula, Q is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms.)

[0055] 8. The siloxane-modified polyurethane composition according to 7, wherein in the formula (11), Q is a linear or branched alkylene group or an alkylene group having an alicyclic structure;

[0056] 9. The siloxane-modified polyurethane composition according to any one of 1 to 8, wherein the functional group of the component (C) that is reactive with an isocyanate group is a group selected from a hydroxyl group, an amino group, a carboxyl group and a mercapto group;

[0057] 10. A heat-cured product of the siloxane-modified polyurethane composition according to any one of 1 to 9;

[0058] 11. The heat-cured product of the siloxane-modified polyurethane composition according to 10, which has thermoplasticity.

[0059] Effects of the Invention

[0060] The siloxane-modified polyurethane composition of the present invention can be easily synthesized, and can form a cured product having higher resin physical property values ​​such as tensile strength and excellent heat resistance than conventional polyurethane compositions. DETAILED DESCRIPTION

[0061] The present invention is described in detail below.

[0062] The siloxane-modified polyurethane composition of the present invention contains the following components (A) to (C).

[0063] (A) a hydroxyl-containing organosilicon compound represented by the following formula (1),

[0064] (B) an isocyanate compound having two or more isocyanate groups in one molecule,

[0065] (C) An organic compound having two or more functional groups reactive with an isocyanate group in one molecule.

[0066] [(A)Component]

[0067] The component (A) is a hydroxyl group-containing organosilicon compound represented by the following formula (1).

[0068] (R 1 3SiO 1 / 2 ) k (R 1 2SiO 2 / 2 ) p (R 1 SiO 3 / 2 ) q (SiO 4 / 2 ) r (1)

[0070] In the above formula (1), R 1 are independently selected from a monovalent hydrocarbon group having 1 to 10 carbon atoms and a group represented by the following formula (2). 1 At least one of the groups is an organic group represented by the following formula (2), and preferably all R 1 Two to five of the groups are organic groups represented by the following formula (2).

[0071] [Chemistry 5]

[0072]

[0073] (In formula (2), the dotted line represents the bonding end.)

[0074] As R 1 The monovalent hydrocarbon group having 1 to 10 carbon atoms may be straight-chain, branched or cyclic, and includes alkyl groups having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and more preferably 1 to 3 carbon atoms; cycloalkyl groups having 5 to 10 carbon atoms, preferably 5 to 8 carbon atoms; aryl groups having 6 to 10 carbon atoms, preferably 6 to 8 carbon atoms, and aralkyl groups having 7 to 10 carbon atoms.

[0075] As R 1 Specific examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl and tolyl; aralkyl groups such as benzyl and phenethyl; and the like.

[0076] Among these, R 1 Preferred are methyl, ethyl and phenyl.

[0077] In formula (2), R 2 They are independently a hydrogen atom or a group selected from a monovalent hydrocarbon group having 1 to 5 carbon atoms and an alkoxy group having 1 to 5 carbon atoms.

[0078] As R 2 A monovalent hydrocarbon group having 1 to 5 carbon atoms, which may be linear or branched, and specific examples thereof include 1 Among the groups exemplified in , the same groups are linear or branched hydrocarbon groups having 1 to 5 carbon atoms, and among them, methyl group, isopropyl group and tert-butyl group are preferred.

[0079] As R 2 The alkoxy group having 1 to 5 carbon atoms is preferably an alkoxy group having 1 to 3 carbon atoms, and specific examples thereof include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, and n-pentoxy. Among them, methoxy and ethoxy are preferred.

[0080] R 3 A hydrogen atom or a methyl group.

[0081] In formula (2), s is an integer of 0-4, preferably an integer of 0-2.

[0082] t is an integer of 2 to 4, and preferably 2 or 3.

[0083] u is a number from 1 to 3, and the repeating unit in the bracket with u may be a single repeating unit chemically or a combination of different repeating units, and the average value thereof may be a number from 1 to 3. When u is 0, the hydroxyl group is phenolic, and for example, the reactivity to the isocyanate group is reduced, so u is 1 or more. In the case of a combination of different repeating units, the case where u is 0 is not included. In addition, if u exceeds 3, the heat resistance is reduced, so the case where u is 4 or more is not included, and u is a number from 1 to 3. The repeating unit in the bracket with u is particularly preferably a chemically single repeating unit.

[0084] Examples of the group represented by formula (2) include groups represented by the following formulae, but the group is not limited to these.

[0085] [Chemistry 6]

[0086]

[0087] (In the formula, t and u are the same as above. The dotted line represents a bonding end.) Among these, the following formulas (3) to (5) are preferred.

[0088] [Chemistry 7]

[0089]

[0090] (Where t and u are the same as above. The dotted lines represent the bond ends.)

[0091] Specific examples of the groups represented by the above formulae (3) to (5) include groups represented by the following formulae, but are not limited thereto. Among these, groups represented by formulae (3a), (4a) to (4e), and (5a) are preferred.

[0092] [Chemistry 8]

[0093]

[0094] (Where the dotted lines represent the bond ends.)

[0095] In the formula (1), k, p, q, and r are numbers satisfying k>0, p≥0, q≥0, and r≥0. However, it is a number satisfying k+p+q≥2.

[0096] k is preferably a number of 2-5, more preferably a number of 2-4.

[0097] p is preferably a number of 2-100, more preferably a number of 5-80.

[0098] q is preferably a number of 0 to 3, more preferably a number of 0 to 2, and even more preferably 1 or 2.

[0099] r is preferably a number of 0 to 3, more preferably 0 or 1, and even more preferably 0.

[0100] k+p+q is preferably a number of k+p+q≥5, and more preferably a number of k+p+q≥8.

[0101] The bonding order of the siloxane units shown in the parentheses is not particularly limited, and the siloxane units may be randomly bonded or may form a block structure.

[0102] As the hydroxyl-containing organosilicon compound used in the present invention, it is preferred that in the above formula (1), k is a number of 2 to 5, p is a number of 2 to 100, q is a number of 0 to 3, r is 0, and all R 1 The compound wherein 2 to 5 of the groups are groups represented by the above formula (2), more preferably k is a number of 2 to 4, p is a number of 5 to 80, q is a number of 0 to 2, r is 0, and all R 4 A compound in which two or three of the groups are groups represented by the above formula (2).

[0103] The group represented by the above formula (2) may be present at either the end of the molecular chain (one end or both ends), in the middle of the molecular chain, or in both ends. It is preferably present at least at the end of the molecular chain (one end or both ends), and more preferably at both ends of the molecular chain.

[0104] As the hydroxyl group-containing organosilicon compound used in the present invention, a compound represented by the following formula is particularly preferred.

[0105] [Chemistry 9]

[0106]

[0107] (In the formula, n is a number n ≥ 0, and k, p and q are the same as above.)

[0108] The weight average molecular weight of the hydroxyl-containing organosilicon compound used in the present invention is preferably 400 to 15000, more preferably 600 to 10000, further preferably 600 to 8000, particularly preferably 600 to 5000. The weight average molecular weight is a polystyrene conversion value measured by gel permeation chromatography (GPC) under the following conditions.

[0109] [Measurement conditions]

[0110] Developing solvent: tetrahydrofuran (THF)

[0111] Flow rate: 0.6mL / min

[0112] Detector: Differential Refractive Index Detector (RI)

[0113] Column: TSK Guardcolumn SuperH-H

[0114] TSKgel SuperHM-N(6.0mmI.D.×15cm×1)

[0115] TSKgel SuperH2500(6.0mmI.D.×15cm×1)

[0116] (All manufactured by Tosoh Corporation)

[0117] Column temperature: 40°C

[0118] Sample injection volume: 50 μL (THF solution with a concentration of 0.3 mass %)

[0119] The kinematic viscosity of the hydroxyl-containing organosilicon compound used in the present invention is preferably 40 to 10,000 mm 2 / s, more preferably 50 to 5000 mm 2 / s. It should be noted that the method for measuring the kinematic viscosity is as described later.

[0120] The hydroxyl-containing organosilicon compound used in the present invention can be obtained, for example, by hydrosilylation of an organohydrogenpolysiloxane represented by the following general formula (6) and a compound represented by the following general formula (7) having a hydroxyl group and an aliphatic unsaturated group (allyl group or methallyl group).

[0121] As the organohydrogenpolysiloxane, an organohydrogenpolysiloxane represented by the following formula (6) was used.

[0122] (R 4 3SiO 1 / 2 ) k (R 4 2SiO 2 / 2 ) p (R 4 SiO 3 / 2 ) q (SiO 4 / 2 ) r (6)

[0124] In formula (6), R 4 are independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms. 4At least one of the groups is a hydrogen atom, preferably all R 4 2 to 5 atoms in the group are hydrogen atoms.

[0125] As R 4 The monovalent hydrocarbon group may be 1 The groups are the same as those exemplified in , and among them, a methyl group, an ethyl group, and a phenyl group are preferred.

[0126] k, p, q and r are the same as above.

[0127] The bonding order of the siloxane units shown in the parentheses is not particularly limited, and the siloxane units may be randomly bonded or may form a block structure.

[0128] As the organohydrogenpolysiloxane, in the above formula (6), k is a number of 2 to 5, p is a number of 2 to 100, q is a number of 0 to 3, r is 0, and all R 4 The organohydrogenpolysiloxane is preferably an organohydrogenpolysiloxane in which 2 to 5 of the groups are hydrogen atoms, k is 2 to 4, p is 5 to 80, q is 0 to 2, r is 0, and all R 4 An organohydrogenpolysiloxane in which 2 or 3 of the groups are hydrogen atoms.

[0129] The hydrogen atom may be present at either the molecular chain terminal (one or both terminals), in the middle of the molecular chain, or both terminals. It is preferably present at least at the molecular chain terminal (one or both terminals), and more preferably at both terminals.

[0130] Specific examples of the organohydrogenpolysiloxane represented by the formula (6) include 1,1,3,3-tetramethyldisiloxane, dimethylpolysiloxane terminated with dimethylhydrogensiloxy groups at both ends of the molecular chain, methylhydrogenpolysiloxane terminated with dimethylhydrogensiloxy groups at both ends of the molecular chain, methylhydrogensiloxane-dimethylsiloxane copolymer terminated with dimethylhydrogensiloxy groups at both ends of the molecular chain, methylhydrogensiloxane-dimethylsiloxane copolymer terminated with dimethylhydrogensiloxy groups at both ends of the molecular chain, methylhydrogensiloxane-diphenylsiloxane copolymer terminated with dimethylhydrogensiloxy groups at both ends of the molecular chain, and (CH3)3SiO 1 / 2 Unit and (CH3)2HSiO 1 / 2 Unit and (CH3)2SiO Unit and CH3SiO 3 / 2 The copolymer consists of (CH3)2HSiO 1 / 2 Unit and (CH3)2SiO Unit and CH3SiO 3 / 2 The copolymer consists of (CH3)2HSiO 1 / 2 Unit and (C6H5)2SiO unit and (CH3)2SiO unit and CH3SiO 3 / 2The copolymer consists of (CH3)(C6H5)HSiO 1 / 2 Unit and (CH3)2SiO Unit and CH3SiO 3 / 2 The copolymer consists of (CH3)2HSiO 1 / 2 Unit and (CH3)2SiO unit and C6H5SiO 3 / 2 These may be used alone or in combination of two or more.

[0131] Among these, dimethylpolysiloxane terminated with dimethylhydrogensiloxy groups at both ends of the molecular chain and (CH3)2HSiO 1 / 2 Unit and (CH3)2SiO Unit and CH3SiO 3 / 2 Copolymer composed of units.

[0132] On the other hand, as the compound having a hydroxyl group and an aliphatic unsaturated group, a compound represented by the following formula (7) was used.

[0133] [Chemistry 10]

[0134]

[0135] (In formula (7), R 2 , R 3 , s, t and u are the same as above. )

[0136] Examples of the group represented by formula (7) include groups represented by the following formulae, but are not limited thereto. These may be used alone or in combination of two or more.

[0137] [Chemistry 11]

[0138]

[0139] (Where t and u are the same as above.)

[0140] Among these, compounds represented by the following formulae (8) to (10) are preferred.

[0141] [Chemistry 12]

[0142]

[0143] (Where t and u are the same as above.)

[0144] Specific examples of the groups represented by the above formulae (8) to (10) include groups represented by the following formulae, but are not limited thereto. Among these, groups represented by formulae (8a), (9a) to (9e), and (10a) are preferred.

[0145] [Chemistry 13]

[0146]

[0147] The compound represented by the formula (7) and having a hydroxyl group and an aliphatic unsaturated group can be obtained, for example, by the following method.

[0148] When a phenol compound having an allyl group in the molecule which is easily available as a commercial product such as o-allylphenol and eugenol (2-methoxy-4-allylphenol) is used as the initial raw material, it can be obtained by a known method by allowing a specified amount of ethylene oxide, propylene oxide, butylene oxide, tetrahydrofuran, etc. or a mixture thereof to react with a phenolic hydroxyl group.

[0149] In addition, for example, when a phenol compound such as phenol, 2,6-dimethylphenol, 2,4-di-tert-butylphenol, 2,6-di-tert-butylphenol is used as the initial raw material, first, an allyl halide compound such as allyl bromide, allyl chloride, methallyl chloride, etc. is reacted with these phenol compounds under alkaline conditions using a known method to obtain allyl (or methallyl) phenyl ether.

[0150] Next, thermal rearrangement of the allyl group is performed to obtain allylated (or methallylated) phenol, which can be obtained by addition reaction with a predetermined amount of ethylene oxide, propylene oxide, butylene oxide, tetrahydrofuran or a mixture thereof in the same manner as above.

[0151] Since the thermal rearrangement reaction of the allyl group occurs at the ortho or para position, it is more preferable to use a compound having only one of the ortho and para positions vacant, such as 2,6-dimethylphenol, 2,4-di-tert-butylphenol, and 2,6-di-tert-butylphenol, in order to obtain a high-purity product.

[0152] In the reaction of the organohydrogenpolysiloxane with the compound having a hydroxyl group and an aliphatic unsaturated group, the amount of the compound having a hydroxyl group and an aliphatic unsaturated group supplied to the reaction is preferably such that the number of moles of the aliphatic unsaturated group (allyl group or methallyl group) possessed by the compound having a hydroxyl group and an aliphatic unsaturated group is in excess relative to the number of moles of the hydrosilyl group possessed by the organohydrogenpolysiloxane.

[0153] For example, the amount ratio may be preferably 1 to 5 moles, more preferably 1 to 2 moles, and further preferably 1 to 1.5 moles relative to 1 mole of the hydrosilyl group. If it is less than 1 mole, the amount of the aliphatic unsaturated group is insufficient, and dehydrogenation may occur easily. On the other hand, if it exceeds 5 moles, a large amount of unreacted products of the compound having a hydroxyl group and an aliphatic unsaturated group remain in the reaction system, which may be uneconomical.

[0154] The hydrosilylation reaction of the organohydrogenpolysiloxane of formula (6) and the compound having a hydroxyl group and an aliphatic unsaturated group of formula (7) is preferably carried out in the presence of a catalyst. The catalyst is not particularly limited, and conventionally known addition reaction catalysts can be used.

[0155] Specific examples of the catalyst include simple substances of platinum group metals such as platinum (including platinum black), palladium, rhodium, and ruthenium, and metal catalysts containing these platinum group metals, gold, nickel, cobalt, etc. Among these, platinum group metal catalysts containing platinum, palladium, or rhodium are particularly preferred.

[0156] Specific examples of catalysts having platinum, palladium or rhodium include PtCl4, H2PtCl6·6H2O, Pt-ether complexes, Pt-olefin complexes, PdCl2(PPh3)2, PdCl2(PhCN)2, RhCl2(PPh3)3 (in the above formula, Ph is a phenyl group), complexes of platinum chloride, chloroplatinic acid or chloroplatinate and vinyl-containing siloxane, etc. These catalysts may be used alone or as a mixture of two or more.

[0157] Among these, a metal catalyst containing platinum is more preferred, and a Karstedt catalyst (a complex of 1,1,3,3-tetramethyl-1,3-divinyldisiloxane and a sodium hydrogen carbonate neutralized product of chloroplatinic acid) is particularly preferred.

[0158] These catalysts can be used after being diluted with a solvent such as alcohols, aromatics, hydrocarbons, or ketones as necessary.

[0159] There is no particular limitation on the amount of the catalyst, as long as it is a catalytic amount. The so-called catalytic amount is an amount sufficient to cause the above-mentioned addition reaction to proceed, for example, relative to 100 parts by mass of hydrogen polysiloxane, the amount of the main metal atom of the above-mentioned metal catalyst is preferably 0.02 parts by mass or less, more preferably 0.00001 to 0.02 parts by mass, further preferably 0.0001 to 0.01 parts by mass, and particularly preferably 0.0003 to 0.005 parts by mass.

[0160] The catalyst may be added in full at the beginning of the reaction, or may be added in divided portions during the reaction.

[0161] Even low catalyst amount can fully react. But if the amount of catalyst is too little, sometimes the speed of reaction is too slow, so preferably above the above-mentioned lower limit. In addition, even if the amount of catalyst is too much, the speed of reaction is not particularly improved, and sometimes becomes uneconomical.

[0162] If the obtained hydroxyl-containing siloxane contains a large amount of residual metal catalyst, this may cause coloration. Therefore, it is preferred that the amount of residual metal catalyst is small. In the production method of the present invention, the amount of metal catalyst contained in the obtained hydroxyl-containing siloxane can be preferably 0.02 parts by mass or less, more preferably 0.01 parts by mass or less, and further preferably 0.005 parts by mass or less, based on the amount of the main metal atom converted relative to 100 parts by mass of the siloxane.

[0163] Furthermore, after the addition reaction is completed, the remaining metal catalyst can be adsorbed and removed using activated carbon or the like.

[0164] The hydrosilylation reaction of the organohydrogenpolysiloxane and the compound having a hydroxyl group and an aliphatic unsaturated group in the present invention is different from the known synthesis method of polysiloxane containing a hydroxyalkyl group, and one of its characteristics is that it can be carried out without using a solvent. A solvent may be used as needed within the scope of not impairing the purpose of the present invention.

[0165] Specific examples of the solvent include toluene, xylene, benzene, hexane, cyclohexane, methylcyclohexane, ethylcyclohexane, chloroform, dichloromethane, carbon tetrachloride, tetrahydrofuran (THF), diethyl ether, acetone, methyl ethyl ketone, dimethylformamide (DMF), acetonitrile and the like.

[0166] When a solvent is used, it may or may not be distilled off after completion of the addition reaction.

[0167] The reaction temperature of the hydrosilylation is preferably 20 to 200° C., more preferably 40 to 180° C., and even more preferably 60 to 150° C. The reaction time is preferably within 20 hours, more preferably within 12 hours, and even more preferably within 8 hours.

[0168] [(B) ingredient]

[0169] The component (B) is an isocyanate compound having two or more isocyanate groups in one molecule. The component (B) is not particularly limited as long as it has two or more isocyanate groups in one molecule, and examples thereof include compounds represented by the following formula (11).

[0170] OCN-Q-NCO (11) (In the above formula, Q is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms.)

[0171] Examples of the divalent hydrocarbon group of Q include a linear or branched alkylene group preferably having 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms, and further preferably 1 to 8 carbon atoms; a cycloalkylene group preferably having 3 to 10 carbon atoms, and more preferably 3 to 6 carbon atoms; an alkylene group having an alicyclic structure preferably having 4 to 15 carbon atoms, and more preferably 4 to 13 carbon atoms; an arylene group preferably having 6 to 15 carbon atoms, and more preferably 6 to 10 carbon atoms; an aralkylene group preferably having 7 to 15 carbon atoms, and more preferably 7 to 13 carbon atoms, and further examples include groups formed by combining these groups.

[0172] Among these, Q is preferably a linear or branched alkylene group, an alkylene group having an alicyclic structure, or an aralkylene group, and more preferably a linear or branched alkylene group, or an alkylene group having an alicyclic structure.

[0173] Specific examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, a dodecamethylene group, a tetradecamethylene group, and the like.

[0174] Specific examples of the cycloalkylene group include cyclopentylene and cyclohexylene.

[0175] As the alkylene group having an alicyclic structure, an alkylene group having a saturated alicyclic structure is preferred, and specific examples thereof include a methylenecyclohexyl group and a methylenebicyclohexyl group.

[0176] Specific examples of the arylene group include a phenylene group and a naphthylene group.

[0177] Specific examples of the aralkylene group include a methylenephenylene group and a methylenebisphenylene group.

[0178] In addition, part of the hydrogen atoms of these groups may be substituted by other substituents. Examples of other substituents include alkyl groups having 1 to 3 carbon atoms such as methyl and ethyl groups; alkoxy groups having 1 to 3 carbon atoms such as methoxy and ethoxy groups; halogen atoms such as chlorine and bromine; and carboxyl groups.

[0179] Specific examples of the isocyanate compound represented by the formula (11) include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, diisocyanate compounds such as esters, 1,5-tetrahydronaphthalene diisocyanate, tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethylene diisocyanate, trimethylhexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, hydrogenated xylylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate.

[0180] Moreover, as (B)component, it is also possible to use isocyanate compounds such as polymeric MDI, reaction products of the above-mentioned diisocyanate compounds and trimethylolpropane, and trimers of the above-mentioned isocyanate compounds.

[0181] The component (B) may be used alone or in combination of two or more.

[0182] Among these, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate are preferred.

[0183] [(C) ingredient]

[0184] (C) component is an organic compound having two or more functional groups capable of reacting with an isocyanate group in one molecule. Examples of the functional group capable of reacting with an isocyanate group include a hydroxyl group, an amino group, a carboxyl group, a thiol group, and the like. As the (C) component, there is no particular limitation as long as it has two or more such functional groups in one molecule, and compounds having a hydroxyl group or an amino group are preferred.

[0185] Specific examples of the component (C) include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 1,4-pentanediol, 1,3-pentanediol, 1,2-pentanediol, 2,5-pentanediol, 2,4-pentanediol, 2,3-pentanediol, 1,6-hexanediol, 1,5-hexanediol, Polyols (diols) such as glycol, 1,4-hexanediol, 1,3-hexanediol, 1,2-hexanediol, 2,6-hexanediol, 2,5-hexanediol, 2,4-hexanediol, 2,3-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol (1,4-dihydroxymethylcyclohexane), 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, and methylpentanediol.

[0186] Furthermore, examples include trifunctional alcohols such as glycerol and trimethylolpropane; tetrafunctional alcohols such as pentaerythritol and α-methylglucoside; hexafunctional alcohols such as sorbitol and sucrose; alkanolamines such as monoethanolamine, diethanolamine and triethanolamine; ethylenediamine, diaminotoluene, diphenylmethanediamine, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2,6-diethylaniline), diamines such as bis(2-ethyl-6-methylaniline), diethylmethylphenylenediamine, 4,6-diethyl-2-methyl-1,3-phenylenediamine, 2-methyl-4,6-bis(methylthio)-1,3-phenylenediamine, 4-methyl-2,6-bis(methylthio)-1,3-phenylenediamine, bis(4-amino-2,3-dichlorophenyl)methane (TCDAM), trimethylenebis(4-aminobenzoate), and isophoronediamine.

[0187] These may be used alone or in combination of two or more.

[0188] Among these, polyols (diols) and diamines are preferred, and 1,4-butanediol, 1,4-cyclohexanedimethanol (1,4-dihydroxymethylcyclohexane) and isophoronediamine are particularly preferred.

[0189] The amount of components (A) to (C) is preferably such that {the total number of isocyanate groups contained in component (B)} / {the total number of hydroxyl groups and amino groups contained in components (A) and (C)}=0.7 to 1.4, more preferably 0.8 to 1.2, further preferably 0.9 to 1.1, and particularly preferably 0.95 to 1.05.

[0190] [Other ingredients]

[0191] The composition of the present invention may contain other components in addition to the components (A) to (C) within a range that does not impair the effects of the present invention. Examples of other components include polyols, catalysts, antioxidants, ultraviolet absorbers, light stabilizers, solvents, and the like.

[0192] Examples of the polyol include polyether polyols, polyester polyols, polycarbonate polyols, etc. other than component (C). Specifically, examples include polyethylene glycol, polypropylene glycol, polyethylene glycol-polytetramethylene glycol, polytetramethylene ether glycol, polytetramethylene glycol, polyhexamethylene glycol, etc. obtained by polymerizing or copolymerizing alkylene oxides or cyclic ethers.

[0193] Examples of the catalyst include triethylamine, N,N-dimethylcyclohexylamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylhexamethylenediamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentamethyldipropylenetriamine, triethylenediamine, N-methyl-N'-(2-dimethylaminoethyl)piperazine, N-ethylmorpholine, 1,2-dimethylimidazole, dimethylethanolamine, dimethylaminoethoxyethanol, N,N,N'-trimethylamino Amine compounds such as ethylethanolamine, N-methyl-N'-(2-hydroxyethyl)piperazine, and bis(2-dimethylaminoethyl)ether; tetraisopropoxytitanium, tetra-n-butoxytitanium, tetra-tert-butoxytitanium, and diisopropoxybisacetylacetonate titanium complex; organic titanium compounds such as tetra-2-ethylhexyloxytitanium and diisopropoxybis(ethyl acetoacetate)titanium; organic zirconium compounds such as tetrabutoxyzirconium, tetrapropoxyzirconium, tetra(2,4-pentanedione)zirconium, and dibutoxybis(ethyl acetoacetate)zirconium; organic tin compounds such as dibutyltin diacetate and dibutyltin dilaurate, etc.

[0194] Examples of the antioxidant include hindered phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants.

[0195] Examples of the ultraviolet absorber include benzotriazole ultraviolet absorbers, triazine ultraviolet absorbers, benzophenone ultraviolet absorbers, and benzoate ultraviolet absorbers.

[0196] Examples of the light stabilizer include hindered amine light stabilizers and the like.

[0197] Examples of the solvent include toluene, xylene, benzene, hexane, cyclohexane, methylcyclohexane, ethylcyclohexane, chloroform, dichloromethane, carbon tetrachloride, tetrahydrofuran (THF), ether, acetone, methyl ethyl ketone, dimethylformamide (DMF), acetonitrile, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, N-methyl-2-pyrrolidone (NMP), 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide (DMAc), ethyl acetate, butyl acetate, and water.

[0198] In addition, organopolysiloxane containing amino groups at both ends of the molecular chain, such as dimethylpolysiloxane having amino groups at both ends of the molecular chain, etc., can also be used.

[0199] The siloxane-modified polyurethane composition of the present invention can be obtained by mixing the above-mentioned components according to a conventional method. Other components can be added to the components (A) to (C) at any timing.

[0200] The method (synthesis method) for producing a resin from the siloxane-modified polyurethane composition of the present invention is not particularly limited, and methods conventionally used for producing polyurethane resins can be used, for example, a prepolymer method, a one-shot method, and the like.

[0201] In the prepolymer method, component (A) and component (B) are first reacted. The reaction temperature is preferably 10 to 250° C., more preferably 20 to 150° C., and even more preferably 50 to 120° C. The reaction time is preferably 10 minutes to 10 hours, and more preferably 30 minutes to 5 hours.

[0202] Then, the component (C) is reacted at the same reaction temperature and reaction time as above.

[0203] The one-step method is a method of reacting component (A), component (B), and component (C) simultaneously. The reaction temperature is preferably 10 to 250° C., more preferably 20 to 150° C., and further preferably 50 to 120° C. The reaction time is preferably 10 minutes to 10 hours, and more preferably 30 minutes to 5 hours.

[0204] The siloxane-modified polyurethane composition of the present invention forms a thermoplastic resin or elastomer by curing (thermosetting) according to its composition, but can also be made into a thermosetting composition by using a polyfunctional isocyanate compound or polyol having three or more functions. As the composition of the present invention, it is preferred that a thermoplastic resin or elastomer is formed by curing.

[0205] Examples of the molding method include a method of cutting into pellets using a twin-screw extruder and then processing into a molded product using various commonly used molding machines, namely, an extrusion molding machine, an injection molding machine, a calender molding machine, a press molding machine, and the like.

[0206] In addition, the composition of the present invention can be preferably used as a primer or top coating agent for various plastics such as polyester, nylon, polyvinyl chloride, ABS, OPP, and CPP in a liquid state in which the composition is dissolved in an organic solvent or in a two-component or three-component liquid state in which the prepolymer and the chain extension component are separated. Furthermore, it can be used as a coating material, a surface coating material, a sealant, an OA roller, a shoe, a ski boot, an adhesive, a wood adhesive, a thermoplastic elastomer, a thermosetting elastomer, and the like for various fibers such as elastic fibers, various fiber woven fabrics, nonwoven fabrics, paper, natural leather, artificial leather, synthetic leather, and wood.

[0207] Example

[0208] The present invention will be described in more detail below with reference to Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited to the following Examples.

[0209] In the following examples, property evaluation was performed by the following methods.

[0210] The kinematic viscosity was measured at 25° C. using a Canon-Fenske viscometer according to the method described in JIS Z8803:2011.

[0211] The hydroxyl value is measured in accordance with JIS K 0070:1992.

[0212] The tensile strength was measured at a speed of 100 mm / min using a No. 6 dumbbell punched out from a 1 mm thick cured product sheet as a test piece according to the method described in JIS K 7312:1996.

[0213] Heat resistance was evaluated by measuring the tensile strength after heating at 120° C. for 3 days. No antioxidant or heat resistance enhancer was added. The reduction rate can be calculated by the following formula.

[0214] Reduction rate (%) = 100 - (tensile strength after heating / initial tensile strength × 100)

[0215] The modulus (storage modulus) was measured using a dynamic viscoelasticity measuring device Rheogel-E4000HP (manufactured by UBM Corporation). The measuring conditions were: elongation test of the test piece 0.8 to 1.5 mm, initial elongation 20 mm, strain 10 Hz at 5 μm, and a heating rate of 3°C / min from -50°C to 150°C.

[0216] [Synthesis example 1]

[0217] After nitrogen substitution in the beaker, 186.9 g of an unsaturated alcohol compound represented by the following formula (12) and 0.10 g of a Karstedt catalyst (platinum concentration 0.5 mass%) were placed and heated to 70° C. 363.0 g of a methylhydrogenpolysiloxane represented by the following formula (13) was added dropwise over 35 minutes. After the addition was completed, the mixture was stirred at 110° C. for 2 hours.

[0218] Next, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 2.5 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 497.0 g of a hydroxyl-containing organopolysiloxane represented by the following formula (14).

[0219] The appearance is colorless and transparent, and the kinematic viscosity is 125mm 2 / s, and the hydroxyl value is 112mgKOH / g.

[0220] [Chemistry 14]

[0221]

[0222] [Synthesis example 2]

[0223] After the beaker was purged with nitrogen, 446.9 g of an unsaturated alcohol compound represented by the following formula (15) and 0.23 g of a Karstedt catalyst (platinum concentration 0.5 mass%) were placed and heated to 60° C. 742.8 g of methyl hydrogen polysiloxane represented by the above formula (13) was added dropwise over 22 minutes. After the addition was completed, the mixture was stirred at 110° C. for 2 hours.

[0224] Next, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 5.9 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 1074.2 g of a hydroxyl-containing organopolysiloxane represented by the following formula (16).

[0225] The appearance is colorless and transparent, and the kinematic viscosity is 372mm 2 / s, and the hydroxyl value is 105mgKOH / g.

[0226] [Chemistry 15]

[0227]

[0228] [Synthesis example 3]

[0229] After nitrogen substitution in the beaker, 231.1 g of an unsaturated alcohol compound which is a mixture of a compound represented by the following formula (17) and a compound represented by the following formula (18) (the content ratio of the compound represented by the following formula (17) to the compound represented by the following formula (18) is formula (17) / formula (18) = 86 / 14 mol%) and 0.11 g of a Karstedt catalyst (platinum concentration 0.5 mass%) were added, and the mixture was heated to 70°C. 363.0 g of methyl hydrogen polysiloxane represented by the above formula (13) was added dropwise over 44 minutes. After the addition was completed, the mixture was stirred at 110°C for 2 hours.

[0230] Next, the unreacted product was heated and distilled off under reduced pressure (220°C / 400Pa). 3.0 g of activated carbon was added, and after stirring at room temperature for 2 hours, the mixture was filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 536.0 g of a hydroxyl-containing organopolysiloxane represented by the following formula (19). In the product, the ratio of primary hydroxyl group to secondary hydroxyl group was the same as the ratio of the compound of formula (17) to the compound of formula (18).

[0231] The appearance is colorless and transparent, and the kinematic viscosity is 283mm 2 / s, and the hydroxyl value is 92.2mgKOH / g.

[0232] [Chemistry 16]

[0233]

[0234] [Synthesis example 4]

[0235] After nitrogen substitution in the beaker, 160.0 g of an unsaturated alcohol compound represented by the following formula (20) and 0.07 g of a Karstedt catalyst (platinum concentration 0.5 mass%) were placed, and the mixture was heated to 70° C. 219.0 g of a methylhydrogenpolysiloxane represented by the above formula (13) was added dropwise over 38 minutes. After the addition was completed, the mixture was stirred at 110° C. for 2 hours.

[0236] Next, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 2.0 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 340.6 g of a hydroxyl-containing organopolysiloxane represented by the following formula (21).

[0237] The appearance is colorless and transparent, and the kinematic viscosity is 408mm 2 / s, and the hydroxyl value is 98.7mgKOH / g.

[0238] [Chemistry 17]

[0239]

[0240] [Synthesis example 5]

[0241] After the beaker was purged with nitrogen, 203.0 g of an unsaturated alcohol compound represented by the following formula (22) and 0.11 g of a Karstedt catalyst (platinum concentration 0.5 mass%) were placed and heated to 70° C. 325.2 g of methyl hydrogen polysiloxane represented by the above formula (13) was added dropwise over 20 minutes. After the addition was completed, the mixture was stirred at 110° C. for 2 hours.

[0242] Next, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 2.5 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 467.1 g of a hydroxyl-containing organopolysiloxane represented by the following formula (23).

[0243] The appearance is colorless and transparent, and the kinematic viscosity is 290mm 2 / s, and the hydroxyl value is 109mgKOH / g.

[0244] [Chemistry 18]

[0245]

[0246] [Comparative Synthesis Example 6]

[0247] After nitrogen substitution in the beaker, 64.7 g of allyl glycol and 0.15 g of Karstedt catalyst (platinum concentration 0.5 mass%) were added and heated to 70° C. 150.0 g of methyl hydrogen polysiloxane represented by the above formula (13) was added dropwise over 30 minutes. After completion of the addition, the mixture was stirred at 110° C. for 2 hours.

[0248] Next, the unreacted product was removed by heating under reduced pressure (120°C / 400 Pa). 1.0 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 171.9 g of a hydroxyl-containing organopolysiloxane represented by the following formula (24).

[0249] The appearance is colorless and transparent, and the kinematic viscosity is 35.0mm 2 / s, and the hydroxyl value is 115mgKOH / g.

[0250] [Chemistry 19]

[0251]

[0252] [Example 1]

[0253] After nitrogen substitution in the beaker, 71.1 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 1 and 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 36.5 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 12.8 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0254] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 1.

[0255] [Example 2]

[0256] After nitrogen substitution in the beaker, 72.7 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 2 and 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 35.0 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 12.2 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0257] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 1.

[0258] [Example 3]

[0259] After nitrogen substitution in the beaker, 76.7 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 3 and 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 32.4 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 11.3 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0260] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 1.

[0261] [Example 4]

[0262] After nitrogen substitution in the beaker, 75.0 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 4 and 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 33.9 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 11.9 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0263] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 1.

[0264] [Example 5]

[0265] After nitrogen substitution in the beaker, 71.8 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 5 and 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 36.0 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 12.6 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0266] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 1.

[0267] [Comparative Example 1]

[0268] After nitrogen substitution in the beaker, 70.3 g of the hydroxyl-containing organopolysiloxane of Comparative Synthesis Example 6 and 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 37.0 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 13.0 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0269] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 1.

[0270] [Table 1]

[0271]

[0272] The blending amount was such that the ratio of hydroxyl-containing organopolysiloxane: hexamethylene diisocyanate: 1,4-butanediol was 1.0: 3.06: 2.0 in terms of molar ratio. The addition amount of zirconium tetraacetylacetonate was 25 ppm.

[0273] As shown in Table 1, the cured products of the siloxane-modified polyurethane compositions of Examples 1 to 5 (siloxane-modified polyurethane resins) have higher initial tensile strength and lower reduction rates after heating at 120° C., and have improved heat resistance, compared with the cured product of the known composition of Comparative Example 1.

[0274] [Synthesis Example 7]

[0275] After nitrogen substitution in the beaker, 103.5 g of the unsaturated alcohol compound represented by the above formula (15) and 0.22 g of Karstedt catalyst (platinum concentration 0.5 mass%) were placed and heated to 70° C. 1012.5 g of methyl hydrogen polysiloxane represented by the following formula (25) was added dropwise over 15 minutes. After the addition was completed, the mixture was further stirred at 110° C. for 2 hours.

[0276] Then, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 5.6 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 1004.0 g of a hydroxyl-containing organopolysiloxane represented by the following formula (26).

[0277] The appearance is colorless and transparent, and the kinematic viscosity is 244mm 2 / s, and the hydroxyl value is 23.0mgKOH / g.

[0278] [Chemistry 20]

[0279]

[0280] [Comparative Synthesis Example 8]

[0281] After nitrogen substitution in the beaker, 30.6 g of allyl glycol and 0.18 g of Karstedt catalyst (platinum concentration 0.5 mass%) were added and heated to 70° C. 427.8 g of methyl hydrogen polysiloxane represented by the above formula (25) was added dropwise over 30 minutes. After completion of the addition, the mixture was further stirred at 110° C. for 2 hours.

[0282] Next, the unreacted product was removed by heating under reduced pressure (120°C / 400 Pa). 2.3 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 395.4 g of a hydroxyl-containing organopolysiloxane represented by the following formula (27).

[0283] The appearance is colorless and transparent, and the kinematic viscosity is 70.0mm 2 / s, and the hydroxyl value is 24.0mgKOH / g.

[0284] [Chemistry 21]

[0285]

[0286] [Example 6]

[0287] After nitrogen substitution in the beaker, 102.4 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 7, 16.1 g of 4,4'-diphenylmethane diisocyanate, 0.006 g of zirconium tetraacetylacetonate (Zr(acac)4), and 30 mL of methyl ethyl ketone were added and stirred at 80°C for 2 hours. After cooling to below 35°C, 3.8 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0288] The obtained block was molded at 210°C for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. In addition, the storage modulus at -30°C and +120°C was measured using the same cured sheet. The results are recorded in Table 2.

[0289] [Comparative Example 2]

[0290] After nitrogen substitution in the beaker, 99.6 g of the hydroxyl-containing organopolysiloxane of Comparative Synthesis Example 8, 16.3 g of 4,4'-diphenylmethane diisocyanate, 0.006 g of zirconium tetraacetylacetonate (Zr(acac)4), and 30 mL of methyl ethyl ketone were added and stirred at 80°C for 2 hours. After cooling to below 35°C, 3.8 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0291] The obtained block was molded at 210°C for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. In addition, the storage modulus at -30°C and +120°C was measured using the same cured sheet. The results are recorded in Table 2.

[0292] [Table 2]

[0293]

[0294] The blending amount was such that the ratio of hydroxyl-containing organopolysiloxane:4,4′-diphenylmethane diisocyanate:1,4-butanediol was 1.0:3.06:2.0 in terms of molar ratio. The addition amount of zirconium tetraacetylacetonate was 50 ppm.

[0295] As shown in Table 2, the cured product of the siloxane-modified polyurethane composition of Example 6 (siloxane-modified polyurethane resin) has higher initial tensile strength and lower reduction rate after heating at 120°C, and has improved heat resistance, compared with the cured product of the known composition of Comparative Example 2. Furthermore, the temperature dependence of the storage modulus is low, and the storage modulus is stable from low temperature to high temperature.

[0296] [Synthesis Example 9]

[0297] After nitrogen substitution in the beaker, 131.0 g of the unsaturated alcohol compound represented by the above formula (15) and 0.12 g of Karstedt catalyst (platinum concentration 0.5 mass%) were placed and heated to 70° C. 484.2 g of methyl hydrogen polysiloxane represented by the following formula (28) was added dropwise over 15 minutes. After completion of the addition, the mixture was further stirred at 110° C. for 2 hours.

[0298] Then, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 3.0 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 542.1 g of a hydroxyl-containing organopolysiloxane represented by the following formula (29).

[0299] The appearance is colorless and transparent, and the kinematic viscosity is 216mm 2 / s, and the hydroxyl value is 55.7mgKOH / g.

[0300] [Chemistry 22]

[0301]

[0302] [Example 7]

[0303] After nitrogen substitution in the beaker, 60.4 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 9, 0.003 g of zirconium tetraacetylacetonate (Zr(acac)4), and 20 mL of tetrahydrofuran were added, and 24.1 g of 4,4'-dicyclohexylmethane diisocyanate was added thereto, followed by stirring at 80°C for 2 hours. The mixture was cooled to below 35°C, and a mixed solution of 47.4 g of the amino-containing organopolysiloxane represented by the following formula (30) and 40 mL of tetrahydrofuran was added dropwise over 35 minutes.

[0304] [Chemistry 23]

[0305]

[0306] Next, 2.7 g of 1,4-butanediol was added and stirred for 5 minutes. The contents were then transferred to a Teflon (registered trademark) bucket, the solvent was removed at 50° C. under reduced pressure, and then heated at 120° C. for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0307] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 3.

[0308] [Example 8]

[0309] After nitrogen substitution in the beaker, 17.66 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 2, 80.5 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 7, and 0.012 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, and 17.0 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 5.9 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0310] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 3.

[0311] [Example 9]

[0312] After nitrogen substitution in the beaker, 83.9 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 7, 6.5 g of polytetramethylene glycol (molecular weight 250), 0.006 g of zirconium tetraacetylacetonate (Zr(acac)4), and 40 mL of methyl ethyl ketone were added, 22.1 g of hexamethylene diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 7.7 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket, the solvent was removed at 50°C under reduced pressure, and then heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0313] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 3.

[0314] [Synthesis Example 10]

[0315] After the beaker was purged with nitrogen, 48.7 g of the unsaturated alcohol compound represented by the above formula (12) and 0.10 g of Karstedt catalyst (platinum concentration 0.5 mass%) were added and heated to 80° C. 372.0 g of methyl hydrogen polysiloxane represented by the following formula (31) was added dropwise over 5 minutes. After the addition was completed, the mixture was further stirred at 110° C. for 2 hours.

[0316] Next, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 2.0 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 353.8 g of a hydroxyl-containing organopolysiloxane represented by the following formula (32).

[0317] The appearance is colorless and transparent, and the kinematic viscosity is 173mm 2 / s, and the hydroxyl value is 38.0mgKOH / g.

[0318] [Chemistry 24]

[0319]

[0320] [Example 10]

[0321] After nitrogen substitution in the beaker, 88.6 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 10 and 0.012 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 24.1 g of 4,4'-dicyclohexylmethane diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 5.4 g of 1,4-butanediol was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0322] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 3.

[0323] [Table 3]

[0324]

[0325] [Synthesis Example 11]

[0326] After the beaker was purged with nitrogen, 182.3 g of the unsaturated alcohol compound represented by the above formula (15) and 0.30 g of Karstedt catalyst (platinum concentration 0.5 mass%) were added and heated to 80° C. 1296.0 g of methyl hydrogen polysiloxane represented by the following formula (33) was added dropwise over 10 minutes. After the addition was completed, the mixture was stirred at 110° C. for 2 hours.

[0327] Next, the unreacted product was removed by heating under reduced pressure (220°C / 400 Pa). 7.4 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 1404.0 g of a hydroxyl-containing organopolysiloxane represented by the following formula (34).

[0328] The appearance is colorless and transparent, and the kinematic viscosity is 231mm 2 / s, and the hydroxyl value is 33.0mgKOH / g.

[0329] [Chemistry 25]

[0330]

[0331] [Synthesis Example 12]

[0332] After nitrogen substitution in the beaker, 80.8 g of the unsaturated alcohol compound represented by the above formula (22) and 0.25 g of Karstedt catalyst (platinum concentration 0.5 mass%) were placed and heated to 80° C. 762.7 g of methyl hydrogen polysiloxane represented by the above formula (25) was added dropwise over 5 minutes. After the addition was completed, the mixture was further stirred at 110° C. for 2 hours.

[0333] Next, the unreacted product was removed by heating under reduced pressure (230°C / 400 Pa). 4.5 g of activated carbon was added, and the mixture was stirred at room temperature for 2 hours and then filtered using a filter plate (NA-500, manufactured by Advantec Co., Ltd.) to obtain 776.0 g of a hydroxyl-containing organopolysiloxane represented by the following formula (35).

[0334] The appearance is colorless and transparent, and the kinematic viscosity is 191mm 2 / s, and the hydroxyl value is 24.5mgKOH / g.

[0335] [Chemistry 26]

[0336]

[0337] [Example 11]

[0338] After nitrogen substitution in the beaker, 95.2 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 11 and 0.012 g of zirconium tetraacetylacetonate (Zr(acac)4) were added, 17.8 g of isophorone diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 7.3 g of 1,4-dihydroxymethylcyclohexane was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0339] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 4.

[0340] [Example 12]

[0341] After nitrogen substitution in the beaker, 100.8 g of the hydroxyl-containing organopolysiloxane of Synthesis Example 12, 0.012 g of zirconium tetraacetylacetonate (Zr(acac)4), and 30 mL of tetrahydrofuran were added, 14.0 g of isophorone diisocyanate was added thereto, and stirred at 80°C for 2 hours. After cooling to below 35°C, 6.7 g of isophorone diamine was added and stirred for 5 minutes. Then, the contents were transferred to a Teflon (registered trademark) bucket and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin.

[0342] The obtained block was press-molded at 210° C. for 8 minutes and a molding pressure of 10 MPa to obtain a 1 mm thick cured sheet, and the tensile strength was measured. The results are shown in Table 4.

[0343] [Table 4]

[0344]

Claims

1. A siloxane-modified polyurethane composition comprising: (A) a hydroxyl-containing organosilicon compound represented by the following general formula (1): (R 1 3SiO 1 / 2 ) k (R 1 2SiO 2 / 2 ) p (R 1 SiO 3 / 2 ) q (SiO 4 / 2 ) r (1) In formula (1), R 1 are independently selected from a monovalent hydrocarbon group having 1 to 10 carbon atoms and a group represented by the following formula (2), but all R 1 At least one of the groups is a group represented by the following formula (2), k, p, q and r are respectively a number of k>0, a number of p≥0, a number of q≥0, a number of r≥0, and a number of k+p+q≥2, and the bonding order of each siloxane unit shown in the parentheses is arbitrary, [Chemistry 1] In formula (2), R 2 are independently a hydrogen atom or a group selected from a monovalent hydrocarbon group having 1 to 5 carbon atoms and an alkoxy group having 1 to 5 carbon atoms, R 3 is a hydrogen atom or a methyl group, s is an integer of 0 to 4, t is an integer of 2 to 4, u is a number of 1 to 3, and the dotted line represents a bonding end. (B) an isocyanate compound having two or more isocyanate groups in one molecule, and (C) An organic compound having two or more functional groups reactive with an isocyanate group in one molecule.

2. The siloxane-modified polyurethane composition according to claim 1, wherein The group represented by formula (2) is any one of the following formulas (3) to (5), [Chemistry 2] Wherein, t and u are the same as above, and the dotted line represents the bonding end.

3. The siloxane-modified polyurethane composition according to claim 1 or 2, wherein In the formula (1) of the component (A), k is a number of 2 to 5, p is a number of 2 to 100, q is a number of 0 to 3, r is 0, and all R 1 2 to 5 of the groups are groups represented by formula (2).

4. The siloxane-modified polyurethane composition according to any one of claims 1 to 3, wherein The component (A) is an addition reaction product of an organohydrogenpolysiloxane represented by the following general formula (6) and a compound containing a hydroxyl group and an aliphatic unsaturated group represented by the following general formula (7), (R 4 3SiO 1 / 2 ) k (R 4 2SiO 2 / 2 ) p (R 4 SiO 3 / 2 ) q (SiO 4 / 2 ) r (6) In formula (6), R 4 are independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, but all R 4 At least one of the groups is a hydrogen atom, k, p, q and r are the same as above, and the bonding order of each siloxane unit shown in the brackets is arbitrary, [Chemistry 3] In formula (7), R 2 , R 3 , s, t and u are the same as above.

5. The siloxane-modified polyurethane composition according to claim 4, wherein The compound represented by formula (7) containing a hydroxyl group and an aliphatic unsaturated group is any one of the compounds represented by the following formulas (8) to (10), [Chemistry 4] Wherein, t and u are the same as above.

6. The siloxane-modified polyurethane composition according to claim 4 or 5, wherein In the above formula (6), k is a number from 2 to 5, p is a number from 2 to 100, q is a number from 0 to 3, r is 0, and all R 4 2 to 5 atoms in the group are hydrogen atoms.

7. The siloxane-modified polyurethane composition according to any one of claims 1 to 6, wherein The component (B) is represented by the following formula (11): OCN-Q-NCO(11) In the above formula, Q is a substituted or unsubstituted divalent hydrocarbon group having 1 to 20 carbon atoms.

8. The siloxane-modified polyurethane composition according to claim 7, wherein In the above formula (11), Q is a linear or branched alkylene group or an alkylene group having an alicyclic structure.

9. The siloxane-modified polyurethane composition according to any one of claims 1 to 8, wherein The functional group of the component (C) that is reactive with an isocyanate group is a group selected from the group consisting of a hydroxyl group, an amino group, a carboxyl group and a mercapto group. 10 . A heat-cured product of the siloxane-modified polyurethane composition according to claim 1 . 11 . The heat-cured product of the siloxane-modified polyurethane composition according to claim 10 , which has thermoplasticity.